Neutron-gamma ray integrated shielding magnesium-based composite material and preparation method and application thereof
By adding tungsten particles and boron carbide particles to the magnesium alloy matrix, a high-density neutron-gamma ray integrated shielding magnesium-based composite material is prepared, which solves the problem of light weight and high efficiency that traditional materials cannot meet in the radiation environment of new nuclear reactors. Shielding problem, achieving lightweight materials, efficient shielding and structure-function integration.
Patent Information
- Application Number
- CN202410888707.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-11
AI Technical Summary
When faced with radiation environments such as new small reactors, mobile reactors, and fusion reactors, traditional neutron and gamma-ray shielding materials are difficult to meet the requirements of lightweight, integrated mechanical-radiation protection performance, radiation resistance, and high temperature resistance, and the shielding assembly The element content is difficult to adjust and the design flexibility is poor.
Neutron-gamma ray integrated shielding magnesium-based composite materials using a magnesium alloy matrix and tungsten particles and boron carbide particles as reinforcements are prepared through mechanical mixing, vacuum degassing and hot isostatic pressing molding processes to produce high-density, elastic materials. It is a material with high modulus and high bending strength, and the content of shielding components can be adjusted to adapt to different radiation environments.
It achieves integrated shielding of neutrons and gamma rays, has lightweight, high efficiency, structure-function integration, good machinability and environmental friendliness, and is suitable for shielding applications of new nuclear reactors.
Smart Images

Figure CN118756019A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of particle-reinforced magnesium-based composite materials and nuclear radiation protection, and specifically relates to a neutron-gamma ray integrated shielding magnesium-based composite material and a preparation method and application thereof. Background Art
[0002] With the depletion of traditional fossil energy reserves and the continuous growth of energy supply demand for economic development, society is facing increasingly prominent energy security issues. Therefore, the development of nuclear energy has received more and more attention. In recent years, my country has built more than 20 new commercial nuclear power plants, and has also actively developed fourth-generation nuclear power plants and fusion nuclear power plants. However, while releasing nuclear energy, nuclear reactions also produce highly penetrating neutrons and gamma rays, causing serious radiation damage to workers and equipment around the reactor. Therefore, radiation protection materials must be arranged between the radiation source and the protected object to weaken the intensity and dose of radiation particles through the scattering and absorption of radiation particles by the material.
[0003] At present, the commonly used neutron and gamma-ray shielding materials in the nuclear power field include: heavy metals and their alloys, barite concrete, metal hydrides, polyethylene and lead-boron polyethylene, etc. These materials generally have certain defects in mechanical properties, shielding efficiency, chemical stability, high temperature resistance, service life and environmental friendliness. This makes it difficult for traditional shielding materials to meet the new requirements of lightweight, integrated mechanical-radiation protection performance, radiation resistance and high temperature resistance when facing radiation environments with compact structures, high radiation intensity and high operating temperatures such as new small reactors, mobile reactors and future fusion reactors. In addition, the content of effective shielding components in traditional shielding materials is not easy to adjust, and the shielding design flexibility is poor when facing neutron and gamma-ray coupled radiation sources with new energy spectrum forms. Summary of the invention
[0004] In view of the above problems, the present invention provides a neutron-gamma ray integrated shielding magnesium-based composite material and a preparation method and application thereof, which specifically include the following contents:
[0005] A neutron-gamma ray integrated shielding magnesium-based composite material comprises a magnesium alloy matrix and a reinforcement distributed in the magnesium alloy matrix, wherein the reinforcement comprises tungsten particles accounting for 20-65% of the total weight percentage of the magnesium-based composite material and 20-45% of boron carbide particles, the tungsten particles and the boron carbide particles accounting for less than 100% of the total weight percentage of the magnesium-based composite material, the average particle size of the tungsten particles is ≤20μm, and the average particle size of the boron carbide particles is ≤50μm.
[0006] Preferably, the average particle size of the tungsten particles is 1-20 μm; and / or the average particle size of the boron carbide particles is 1-50 μm.
[0007] Preferably, the tungsten purity of the tungsten particles is ≥ 99 wt %; and / or the total boron-carbon content of the boron carbide particles is ≥ 98 wt %.
[0008] Preferably, the tungsten particles are tungsten particles with low agglomeration tendency that have been pre-dispersed by anhydrous ethanol, pre-dispersed by air jet milling, or pre-dispersed by both.
[0009] Preferably, the boron carbide particles are boron carbide particles with low stress concentration tendency that have been pre-grinded by jet milling to remove sharp edges and corners of the particles.
[0010] Preferably, the magnesium alloy is a rare earth magnesium alloy.
[0011] Preferably, the rare earth magnesium alloy is a gadolinium-containing rare earth magnesium alloy, wherein the mass content of gadolinium in the gadolinium-containing rare earth magnesium alloy is 5-12wt%.
[0012] Preferably, the rare earth magnesium alloy is one or more of magnesium alloys with commercial grades VE, VW, VK and / or non-commercial grades of magnesium-gadolinium (Mg-Gd), magnesium-gadolinium-yttrium (Mg-Gd-Y), magnesium-gadolinium-zinc (Mg-Gd-Zn), magnesium-gadolinium-zirconium (Mg-Gd-Zr), and magnesium-gadolinium-calcium (Mg-Gd-Ca) alloys.
[0013] Preferably, the magnesium-based composite material has a density of ≥99%, an elastic modulus of ≥90 GPa, a flexural strength of ≥200 MPa, and a 3 ≤Density≤5.5g / cm 3 .
[0014] A method for preparing the neutron-gamma ray integrated shielding magnesium-based composite material comprises the following steps:
[0015] (1) Mixing and dispersing: mechanically mixing tungsten particles, boron carbide particles and rare earth magnesium alloy particles to obtain a mixed powder;
[0016] (2) Vacuum degassing: The mixed powder is placed in a metal package, degassed and then sealed;
[0017] (3) Hot isostatic pressing: hot isostatic pressing is performed, and then the metal sheath is removed by machining to obtain the neutron-gamma ray integrated shielding magnesium-based composite material.
[0018] Preferably, between step (1) and step (2), cold isostatic pressing is further included: the mixed powder is placed in a polymer sheath, sealed, and then cold isostatically pressed in a liquid medium. Cold isostatic pressing is an optional step, and can be skipped when the size of the neutron-gamma ray integrated shielding magnesium-based composite material to be prepared is small, and the powder mixed in step (1) is directly placed in a metal sheath and the operation of step (2) is performed.
[0019] Preferably, the cold isostatic pressing pressure is 100-200 MPa and the holding time is 5-10 min.
[0020] Preferably, the average particle size of the rare earth magnesium alloy particles in step (1) is ≤60 μm; and / or, the mechanical mixing method is: using a mixer under the protection of one or more atmospheres of argon, nitrogen, and carbon dioxide, the tungsten particles, boron carbide particles, and rare earth magnesium alloy particles are mixed uniformly, the diameter of the grinding balls in the mixer is Φ5-Φ20 mm, and / or the weight ratio of the grinding balls to the powder to be mixed is (0.25-2):1, and / or the mixing time is 12-36 hours. More preferably, the tungsten particles and boron carbide particles are pretreated before mixing, including pre-dispersing the tungsten particles with anhydrous ethanol, pre-dispersing them with a jet mill, or pre-dispersing them with a combination of the two to obtain tungsten particles with a low tendency to agglomerate; pre-grinding the boron carbide particles with a jet mill to remove the sharp edges of the particles to obtain boron carbide particles with a low tendency to stress concentration, and then mixing the tungsten particles, boron carbide particles, and rare earth magnesium alloy particles. This can prevent agglomeration and further improve the uniformity of mixing.
[0021] Preferably, the sealing method in step (2) is: at a temperature of 400-500°C and a vacuum degree of 10 -2 -10 -5 Pa under the condition of welding seal.
[0022] Preferably, the sintering temperature of the hot isostatic pressing in step (3) is 400-550°C, the pressure is 100-200 MPa, the heat preservation and pressure holding time is 1-4 hours, and the cooling method is furnace cooling.
[0023] A method for preparing the neutron-gamma ray integrated shielding magnesium-based composite material comprises the following steps:
[0024] (1) Mixing and dispersing: mechanically mixing tungsten particles, boron carbide particles and rare earth magnesium alloy particles to obtain a mixed powder; the average particle size of the rare earth magnesium alloy particles in step (1) is ≤60μm; and / or the mechanical mixing method is: using a mixer under the protection of one or more atmospheres of argon, nitrogen and carbon dioxide to uniformly mix the tungsten particles, boron carbide particles and rare earth magnesium alloy particles, the diameter of the grinding balls in the mixer is Φ5-Φ20mm, and / or the weight ratio of the grinding balls to the powder to be mixed is (0.25-2):1, and / or the mixing time is 12-36h. More preferably, the tungsten particles and boron carbide particles are pre-treated before mixing, including pre-dispersing the tungsten particles with anhydrous ethanol, pre-dispersing them with a jet mill or pre-dispersing them with a combination of the two to obtain tungsten particles with a low tendency to agglomerate; pre-grinding the boron carbide particles with a jet mill to remove sharp edges and corners of the particles to obtain boron carbide particles with a low tendency to stress concentration, and then the tungsten particles, boron carbide particles and rare earth magnesium alloy particles are uniformly mixed. This prevents agglomeration and further improves the uniformity of the mix;
[0025] (2) Vacuum hot pressing: The mixed powder is subjected to vacuum hot pressing, and the sintering temperature is controlled to be 400-550°C, the pressing force is 10-50t, and the vacuum degree is 10 -2 -10 -5 Pa, the heat preservation and pressure preservation time is 2-8h, and then the furnace is cooled to obtain the neutron-gamma ray integrated shielding magnesium-based composite material.
[0026] An application of the neutron-gamma ray integrated shielding magnesium-based composite material in radiation protection.
[0027] Beneficial effects of the present invention:
[0028] (1) The neutron-gamma ray integrated shielding magnesium-based composite material disclosed in the present invention adds tungsten and boron elements to the magnesium alloy matrix in the form of particle reinforcements. By optimizing the particle size matching of the powder particles, the density and uniformity of the material are ensured while improving the material strength, and the shielding effect of the material is greatly improved, thereby achieving integrated shielding of neutrons and gamma rays. In addition, the magnesium alloy and the magnesium alloy containing gadolinium used in the present invention, as a key element for improving the strength and plasticity of magnesium alloys, also has a very high thermal neutron absorption cross section, which can improve the shielding performance while taking into account the overall mechanical properties of the composite material, thereby achieving the structural-functional integration of the magnesium-based composite shielding material.
[0029] (2) In the prior art, metal-based composite materials generally use aluminum alloy as the matrix of the composite material. The density of aluminum alloy is relatively large, and the radiation shielding effect of the matrix is relatively limited. The present invention uses magnesium alloy as the matrix. The density of magnesium alloy is only about two-thirds of that of aluminum alloy. The neutron-gamma ray integrated shielding magnesium-based composite material disclosed in the present invention has the advantages of being lighter and more efficient than traditional aluminum-based composite shielding materials. In the composite material described in the present invention, the boron content is greater than that of the existing aluminum-based boron carbide neutron absorbing material and boron-containing stainless steel material (boron content ≤ 2.25wt%).
[0030] (3) The neutron-gamma ray integrated shielding magnesium-based composite material disclosed in the present invention has the advantages of flexible shielding design and light weight, and the content and density of shielding components can be adjusted within a certain range according to the shielding requirements; at the same time, the material also has the advantages of structural-functional integration, better machinability than ceramic shielding materials such as boron carbide, and better environmental friendliness than heavy metal shielding materials such as lead. It is particularly suitable for neutron and gamma ray shielding application scenarios of nuclear radiation devices such as new nuclear reactors that require miniaturized, lightweight, and structural-functional integrated shielding components.
[0031] (4) The present invention discloses two methods for preparing neutron-gamma ray integrated shielding magnesium-based composite materials. By limiting the raw material particle size, pretreatment method, mixing method, etc., the occurrence of particle agglomeration is avoided, and a better mixing effect can be achieved to make the internal components of the material more evenly distributed. In addition, according to the characteristics of the material components, the present invention also designs the pressing process parameters, so that the neutron-gamma ray integrated shielding magnesium-based composite materials prepared by the method disclosed in the present invention have the advantages of lightweight, excellent mechanical properties, and high shielding performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly show the relevant technical details of the embodiments of the present invention, the drawings required in the embodiments are briefly introduced. It should be understood that the following drawings are only used to show some specific embodiments of the present invention, and therefore should not be regarded as limiting the content and scope of the invention. For general R&D and technical personnel in this field and profession, other relevant drawings can still be easily obtained according to the drawings of this specification without creative work.
[0033] Figure 1 This is an example SEM photo of gadolinium-containing rare earth magnesium alloy particles;
[0034] Figure 2 This is a sample SEM photo of tungsten particles;
[0035] Figure 3 This is an example SEM photo of boron carbide particles;
[0036] Figure 4This is an example SEM photo of the microstructure morphology of the neutron-gamma ray integrated shielding magnesium-based composite material. DETAILED DESCRIPTION
[0037] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The embodiments shown below do not limit the invention content described in the claims. In addition, the entire contents of the structures represented by the following embodiments are not limited to those necessary as solutions to the invention described in the claims.
[0038] A neutron-gamma ray integrated shielding magnesium-based composite material comprises a magnesium alloy matrix and a reinforcement distributed in the magnesium alloy matrix, wherein the reinforcement comprises tungsten particles accounting for 20-65% of the total weight percentage of the magnesium-based composite material and 20-45% of boron carbide particles, the tungsten particles and the boron carbide particles accounting for less than 100% of the total weight percentage of the magnesium-based composite material, the average particle size of the tungsten particles is ≤20μm, and the average particle size of the boron carbide particles is ≤50μm. Among them, the content of tungsten particles can be 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, etc., and the average particle size can be 1μm, 2μm, 4μm, 6μm, 8μm, 10μm, 12μm, 15μm, 18μm, etc.; the content of boron carbide particles can be 22%, 25%, 28%, 30%, 35%, 38%, 40%, 42%, etc., and the average particle size can be 1μm, 2μm, 4μm, 6μm, 8μm, 10μm, 12μm, 15μm, 20μm, 25μm, 30μm, 35μm, 40μm, 45μm, etc.;
[0039] In some embodiments of the present invention, the average particle size of the tungsten particles is 1-20 μm; and / or the average particle size of the boron carbide particles is 1-50 μm.
[0040] In some embodiments of the present invention, the tungsten purity of the tungsten particles is ≥ 99 wt %; and / or the total boron-carbon content of the boron carbide particles is ≥ 98 wt %.
[0041] In some embodiments of the present invention, the tungsten particles are tungsten particles with low agglomeration tendency that have been pre-dispersed by anhydrous ethanol, pre-dispersed by air jet milling, or pre-dispersed by both.
[0042] In some embodiments of the present invention, the boron carbide particles are boron carbide particles with low stress concentration tendency that have been pre-ground by a jet mill to remove sharp edges and corners of the particles.
[0043] In some embodiments of the present invention, the magnesium alloy is a rare earth magnesium alloy.
[0044] In some embodiments of the present invention, the rare earth magnesium alloy is a gadolinium-containing rare earth magnesium alloy, wherein the mass content of the gadolinium element in the gadolinium-containing rare earth magnesium alloy is 5-12wt%, specifically 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, etc.
[0045] In some embodiments of the present invention, the rare earth magnesium alloy is one or more of magnesium alloys with commercial grades VE, VW, VK and / or non-commercial grades of magnesium-gadolinium (Mg-Gd), magnesium-gadolinium-yttrium (Mg-Gd-Y), magnesium-gadolinium-zinc (Mg-Gd-Zn), magnesium-gadolinium-zirconium (Mg-Gd-Zr), and magnesium-gadolinium-calcium (Mg-Gd-Ca) alloys.
[0046] In some embodiments of the present invention, the magnesium-based composite material has a density of ≥99%, an elastic modulus of ≥90 GPa, a flexural strength of ≥200 MPa, and a 3 ≤Density≤5.5g / cm 3 .
[0047] In some embodiments of the present invention, the method for preparing the neutron-gamma ray integrated shielding magnesium-based composite material comprises the following steps:
[0048] (1) Mixing and dispersing: mechanically mixing tungsten particles, boron carbide particles and rare earth magnesium alloy particles to obtain a mixed powder;
[0049] (2) Vacuum degassing: The mixed powder is placed in a metal package, degassed and then sealed;
[0050] (3) Hot isostatic pressing: hot isostatic pressing is performed, and then the metal sheath is removed by machining to obtain the neutron-gamma ray integrated shielding magnesium-based composite material.
[0051] In some embodiments of the present invention, between step (1) and step (2), cold isostatic pressing is further included: the mixed powder is placed in a polymer sheath, sealed, and then cold isostatic pressing is performed in a liquid medium. Cold isostatic pressing is an optional step, and can be skipped when the size of the neutron-gamma ray integrated shielding magnesium-based composite material to be prepared is small, and the powder mixed in step (1) is directly placed in a metal sheath and the operation of step (2) is performed.
[0052] In some embodiments of the present invention, the cold isostatic pressing pressure is 100-200 MPa, and the holding time is 5-10 min. Specifically, the cold isostatic pressing pressure can be 100 MPa, 110 MPa, 120 MPa, 130 MPa, 150 MPa, 180 MPa, 190 MPa, 200 MPa, etc.; the holding time can be 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, etc.
[0053] In some embodiments of the present invention, the average particle size of the rare earth magnesium alloy particles in step (1) is ≤60 μm, and can be specifically 1 μm, 2 μm, 5 μm, 8 μm, 10 μm, 15 μm, 20 μm, 30 μm, 40 μm, 50 μm, 55 μm, etc.; and / or, the mechanical mixing method is: using a mixer to uniformly mix the tungsten particles, boron carbide particles and rare earth magnesium alloy particles under the protection of one or more atmospheres of argon, nitrogen and carbon dioxide; the diameter of the grinding balls in the mixer is Φ5-Φ20 mm , specifically 5mm, 6mm, 8mm, 10mm, 12mm, 15mm, 20mm, etc.; and / or the weight ratio of grinding balls to powder to be mixed is (0.25-2):1, specifically 0.25:1, 0.3:1, 0.5:1, 0.8:1, 1:1, 1.2:1, 1.5:1, 2:1, etc.; and / or the mixing time is 12-36h, specifically 12h, 15h, 18h, 20h, 22h, 25h, 28h, 30h, 32h, 34h, 36h, etc. More preferably, the tungsten particles and the boron carbide particles are pretreated before mixing, including pre-dispersing the tungsten particles with anhydrous ethanol, pre-dispersing them with a jet mill, or pre-dispersing them with a combination of the two, to obtain tungsten particles with a low tendency to agglomerate; pre-grinding the boron carbide particles with a jet mill to remove sharp edges and corners of the particles, to obtain boron carbide particles with a low tendency to stress concentration, and then the tungsten particles, boron carbide particles, and rare earth magnesium alloy particles are uniformly mixed. This can prevent agglomeration and further improve the uniformity of mixing.
[0054] In some embodiments of the present invention, the sealing method in step (2) is: at a temperature of 400-500°C and a vacuum degree of 10 -2 -10 -5 The specific temperature can be 410℃, 420℃, 440℃, 460℃, 480℃, 490℃, etc., and the vacuum degree can be 10 -3 Pa, 5×10 -4 Pa, 10 -4 Pa, 5×10 -5 Pa, 10 -5 Pa et al.
[0055] In some embodiments of the present invention, the sintering temperature of the hot isostatic pressing in step (3) is 400-550°C, the pressure is 100-200MPa, the heat preservation and pressure holding time is 1-4h, and the cooling method is furnace cooling. Specifically, the sintering temperature can be 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, etc.; the pressure can be 100MPa, 110MPa, 120MPa, 140MPa, 160MPa, 180MPa, 200MPa, etc.; the time can be 1h, 1.1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, 2.5h, 2.8h, 3h, 2.5h, 3.8h, 4h, etc.
[0056] In some embodiments of the present invention, the method for preparing the neutron-gamma ray integrated shielding magnesium-based composite material comprises the following steps:
[0057] (1) Mixing and dispersing: mechanically mixing tungsten particles, boron carbide particles and rare earth magnesium alloy particles to obtain a mixed powder; the average particle size of the rare earth magnesium alloy particles in step (1) is ≤60μm, and can be 1μm, 2μm, 5μm, 8μm, 10μm, 15μm, 20μm, 30μm, 40μm, 50μm, 55μm, etc.; and / or, the mechanical mixing method is: using a mixer to uniformly mix the tungsten particles, boron carbide particles and rare earth magnesium alloy particles under the protection of one or more atmospheres of argon, nitrogen and carbon dioxide; the mixing The diameter of the grinding balls in the machine is Φ5-Φ20mm, specifically 5mm, 6mm, 8mm, 10mm, 12mm, 15mm, 20mm, etc.; and / or the weight ratio of the grinding balls to the powder to be mixed is (0.25-2):1, specifically 0.25:1, 0.3:1, 0.5:1, 0.8:1, 1:1, 1.2:1, 1.5:1, 2:1, etc.; and / or the mixing time is 12-36h, specifically 12h, 15h, 18h, 20h, 22h, 25h, 28h, 30h, 32h, 34h, 36h, etc. More preferably, the tungsten particles and the boron carbide particles are pre-treated before mixing, including pre-dispersing the tungsten particles with anhydrous ethanol, pre-dispersing them with a jet mill, or pre-dispersing them with a combination of the two, to obtain tungsten particles with a low tendency to agglomerate; pre-grinding the boron carbide particles with a jet mill to remove sharp edges and corners of the particles, to obtain boron carbide particles with a low tendency to stress concentration, and then the tungsten particles, boron carbide particles, and rare earth magnesium alloy particles are mixed evenly. This can prevent agglomeration and further improve the uniformity of mixing;
[0058] (2) Vacuum hot pressing: The mixed powder is subjected to vacuum hot pressing, and the sintering temperature is controlled to be 400-550°C, the pressing force is 10-50t, and the vacuum degree is 10 -2 -10 -5Pa, heat preservation and pressure holding time is 2-8h, and then cooled with the furnace to obtain the neutron-gamma ray integrated shielding magnesium-based composite material. Specifically, the sintering temperature can be 400℃, 410℃, 420℃, 440℃, 460℃, 480℃, 500℃, 520℃, 540℃, etc.; the pressing force can be 10t, 12t, 15t, 20t, 25t, 30t, 35t, 40t, 45t, 50t, etc.; the vacuum degree can be 10 -3 Pa, 5×10 -4 Pa, 10 -4 Pa, 5×10 -5 Pa, 10 -5 Pa, etc.; the insulation and pressure holding time can be 2h, 3h, 4h, 5h, 6h, 7h, 8h, etc.
[0059] An application of the neutron-gamma ray integrated shielding magnesium-based composite material in radiation protection.
[0060] Example 1
[0061] In this embodiment, the neutron-γ-ray integrated shielding magnesium-based composite material is prepared by mixing 20wt% tungsten particles, 20wt% boron carbide particles and 60wt% VE82M rare earth magnesium alloy particles, and the average particle sizes are 5μm, 10μm and 50μm respectively (see attached Figure 1-3 The preparation method is as follows:
[0062] (1) Using a double cone mixer under argon protection, the powders of tungsten particles, boron carbide particles and rare earth magnesium alloy particles were mixed for 12 hours;
[0063] (2) The uniformly mixed powder is placed in a pre-made nitrile rubber bag, sealed and cold isostatically pressed at 100 MPa for 5 min;
[0064] (3) The cold pressed powder blank is placed in a pre-made aluminum package and kept at 400°C for 15 hours with a vacuum degree of less than 1×10 -3 Sealing under the condition of Pa;
[0065] (4) The temperature was raised to 420°C at a rate of 10°C / min, and the hot isostatic pressing conditions were 150MPa and 3h of heat preservation and pressure maintenance. The magnesium-based composite shielding material was formed by cooling to room temperature with the furnace; the surface aluminum skin was removed to obtain a blank of the magnesium-based composite shielding material (its microstructure is shown in the attached figure). Figure 4 As shown in the figure, the white particles are tungsten particles, the gray matrix is a magnesium alloy matrix, and the black particles are boron carbide particles).
[0066] Example 2
[0067] The process steps of this implementation case are basically the same as those of Implementation Case 1, except that: the powder raw materials are mixed in a ratio of 65wt% tungsten particles, 20wt% boron carbide particles and 15wt% VW83M rare earth magnesium alloy particles, with average particle sizes of 20μm, 40μm and 20μm, respectively; at the same time, the hot isostatic pressing jacket is changed to a steel jacket, and the hot isostatic pressing conditions are changed to 500℃, a pressure of 150MPa, and insulation and pressure maintenance for 4h.
[0068] Example 3
[0069] The process steps of this embodiment are basically the same as those of Embodiment 1, except that: the powder raw materials are formulated in a ratio of 20wt% tungsten particles, 45wt% boron carbide particles and 35wt% self-produced magnesium-gadolinium-zirconium (containing about 10wt% gadolinium and about 1wt% zirconium) rare earth magnesium alloy particles, with average particle sizes of 10μm, 50μm and 20μm, respectively; at the same time, the hot isostatic pressing jacket is changed to a steel jacket, and the hot isostatic pressing conditions are changed to 500°C, a pressure of 150MPa, and insulation and pressure maintenance for 4h.
[0070] Example 4
[0071] The process steps of this implementation case are basically the same as those of Implementation Case 1, except that the average particle sizes of the three powders are adjusted to 5 μm, 10 μm, and 20 μm; at the same time, the hot isostatic pressing jacket is changed to a steel jacket, and the hot isostatic pressing conditions are changed to 500°C, a pressure of 120 MPa, and insulation and pressure maintenance for 3 hours.
[0072] Example 5
[0073] The raw materials of this embodiment are the same as those of Embodiment 1, except that step (2) of cold isostatic pressing in Embodiment 1 is omitted, and the mixed powder is directly used for hot isostatic pressing.
[0074] Example 6
[0075] The raw materials of this embodiment are the same as those of embodiment 1, except that a one-step vacuum hot pressing process is used to replace step (2) cold isostatic pressing, step (3) vacuum degassing, and step (4) hot isostatic pressing in embodiment 1, and the mixed powder is directly used for vacuum hot pressing. The mixed powder is loaded into the mold cavity of the vacuum hot press, and the sintering temperature is set to 530°C, the pressing force is set to 30t, and the vacuum degree is set to ≤1×10 -3 Pa, the heat preservation and pressure holding time is 6 hours, and then the furnace is cooled, and the mold cavity is opened to obtain the initial blank of the magnesium-based composite shielding material.
[0076] The material properties of the above embodiment are shown in Table 1:
[0077] Table 1 Material properties of the above examples
[0078]
[0079]
[0080] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A neutron-gamma ray integrated shielding magnesium-based composite material, characterized in that: The invention comprises a magnesium alloy matrix and a reinforcement distributed in the magnesium alloy matrix, wherein the reinforcement comprises 20-65% of tungsten particles and 20-45% of boron carbide particles in a total weight percentage of the magnesium-based composite material, the tungsten particles and the boron carbide particles account for less than 100% of the total weight percentage of the magnesium-based composite material, the average particle size of the tungsten particles is ≤20 μm, and the average particle size of the boron carbide particles is ≤50 μm.
2. The neutron-gamma ray integrated shielding magnesium-based composite material according to claim 1, characterized in that: The average particle size of the tungsten particles is 1-20 μm; and / or the average particle size of the boron carbide particles is 1-50 μm.
3. The neutron-gamma ray integrated shielding magnesium-based composite material according to claim 1, characterized in that: The tungsten purity of the tungsten particles is ≥ 99 wt %; and / or the total boron-carbon content of the boron carbide particles is ≥ 98 wt %.
4. The neutron-gamma ray integrated shielding magnesium-based composite material according to claim 1, characterized in that: The tungsten particles are tungsten particles with low agglomeration tendency that have been pre-dispersed by anhydrous ethanol, pre-dispersed by air jet milling, or pre-dispersed by both.
5. The neutron-gamma ray integrated shielding magnesium-based composite material according to claim 1, characterized in that: The boron carbide particles are pre-ground by a jet mill to remove sharp edges and corners of the particles and have a low stress concentration tendency.
6. The neutron-gamma ray integrated shielding magnesium-based composite material according to claim 1, characterized in that: The magnesium alloy is a rare earth magnesium alloy.
7. The neutron-gamma ray integrated shielding magnesium-based composite material according to claim 6, characterized in that: The rare earth magnesium alloy is a gadolinium-containing rare earth magnesium alloy, wherein the mass content of gadolinium in the gadolinium-containing rare earth magnesium alloy is 5-12wt%.
8. The neutron-gamma ray integrated shielding magnesium-based composite material according to claim 7, characterized in that: The rare earth magnesium alloy is one or more of magnesium alloys with commercial grades VE, VW, VK and / or non-commercial grades of magnesium-gadolinium alloy, magnesium-gadolinium-yttrium alloy, magnesium-gadolinium-zinc alloy, magnesium-gadolinium-zirconium alloy, and magnesium-gadolinium-calcium alloy.
9. The neutron-gamma ray integrated shielding magnesium-based composite material according to any one of claims 1 to 8, characterized in that: The magnesium-based composite material has a density of ≥99%, an elastic modulus of ≥90 GPa, a flexural strength of ≥200 MPa, and a 3 ≤Density≤5.5g / cm 3 .
10. A method for preparing the neutron-gamma ray integrated shielding magnesium-based composite material according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Mixing and dispersing: mechanically mixing tungsten particles, boron carbide particles and rare earth magnesium alloy particles to obtain a mixed powder; (2) Vacuum degassing: The mixed powder is placed in a metal package, degassed and then sealed; (3) Hot isostatic pressing: hot isostatic pressing is performed, and then the metal sheath is removed by machining to obtain the neutron-gamma ray integrated shielding magnesium-based composite material.
11. The method for preparing a neutron-gamma ray integrated shielding magnesium-based composite material according to claim 10, characterized in that: Between step (1) and step (2), the method further comprises cold isostatic pressing: the mixed powder is placed in a polymer package, sealed, and then cold isostatically pressed in a liquid medium.
12. The method for preparing a neutron-gamma ray integrated shielding magnesium-based composite material according to claim 11, characterized in that: The cold isostatic pressing pressure is 100-200 MPa, and the holding time is 5-10 min.
13. The method for preparing a neutron-gamma ray integrated shielding magnesium-based composite material according to claim 10, characterized in that: The average particle size of the rare earth magnesium alloy particles in step (1) is ≤60 μm; and / or the mechanical mixing method is: using a mixer to uniformly mix the tungsten particles, boron carbide particles and rare earth magnesium alloy particles under the protection of one or more atmospheres of argon, nitrogen and carbon dioxide, the diameter of the grinding balls in the mixer is Φ5-Φ20 mm, and / or the weight ratio of the grinding balls to the powder to be mixed is (0.25-2):1, and / or the mixing time is 12-36 h.
14. The method for preparing a neutron-gamma ray integrated shielding magnesium-based composite material according to claim 10, characterized in that: The sealing method in step (2) is: at a temperature of 400-500°C and a vacuum degree of 10 -2 -10 -5 Pa under the condition of welding seal.
15. The method for preparing the neutron-gamma ray integrated shielding magnesium-based composite material according to any one of claims 10 to 14, characterized in that: The sintering temperature of the hot isostatic pressing in step (3) is 400-550°C, the pressure is 100-200MPa, the heat preservation and pressure holding time is 1-4h, and the cooling method is furnace cooling.
16. A method for preparing the neutron-gamma ray integrated shielding magnesium-based composite material according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Mixing and dispersing: mechanically mixing tungsten particles, boron carbide particles and rare earth magnesium alloy particles to obtain a mixed powder; (2) Vacuum hot pressing: The mixed powder is subjected to vacuum hot pressing, and the sintering temperature is controlled to be 400-550°C, the pressing force is 10-50t, and the vacuum degree is 10 -2 -10 -5 Pa, the heat preservation and pressure preservation time is 2-8h, and then the furnace is cooled to obtain the neutron-gamma ray integrated shielding magnesium-based composite material.
17. The method for preparing a neutron-gamma ray integrated shielding magnesium-based composite material according to claim 16, characterized in that: The average particle size of the rare earth magnesium alloy particles in step (1) is ≤60 μm; and / or the mechanical mixing method is: using a mixer to uniformly mix the tungsten particles, boron carbide particles and rare earth magnesium alloy particles under the protection of one or more atmospheres of argon, nitrogen and carbon dioxide, the diameter of the grinding balls in the mixer is Φ5-Φ20 mm, and / or the weight ratio of the grinding balls to the powder to be mixed is (0.25-2):1, and / or the mixing time is 12-36 h.
18. Use of the neutron-gamma ray integrated shielding magnesium-based composite material according to any one of claims 1 to 9 in radiation protection.
Citation Information
Cited By
Lightweight neutron shielding material and manufacturing method thereof
CN121105179A