Preparation method of high-strength, high-thermal-conductivity and high-reflection multi-layer composite cold shield and cold shield

By using a multi-layer composite structure of high thermal conductivity pure copper material and high-strength nickel-cobalt alloy material in the cold screen, combined with double-pulse electroforming and surface polishing, it solves the problem that traditional cold screens cannot have high strength, high thermal conductivity and high reflection at the same time. solve the problem and achieve efficient cooling and stray light suppression effects.

CN118756262APending Publication Date: 2024-10-11KUNMING INST OF PHYSICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410745413.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

It is difficult for traditional cold screens to meet the performance requirements of high strength, high thermal conductivity and high reflection on the outer surface at the same time, resulting in prolonged cooling time and poor stray light suppression effect.

Method used

High thermal conductivity pure copper material is used as the middle layer of the multi-layer composite cold shield, combined with high-strength nickel-cobalt alloy material as the boundary layer. Through double-pulse electroforming and special surface polishing treatment, the composition proportion and layer of pure copper and nickel-cobalt are controlled. Thickness ratio, to prepare a multi-layer composite cold screen that meets the requirements of light weight, thin wall, high precision, high strength, high thermal conductivity and high reflection of the outer surface.

Benefits of technology

It achieves an excellent combination of high strength, high thermal conductivity and high reflective performance of the outer surface of the cold screen, shortens the cooling time and improves the stray light suppression effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756262A_ABST
    Figure CN118756262A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-strength, high-thermal-conductivity and high-reflection multi-layer composite cold shield and the cold shield. A high-thermal-conductivity pure copper material is used as a middle layer of the multi-layer composite cold shield, and a high-strength nickel-cobalt alloy material is used as a boundary layer of the multi-layer composite cold shield; the multi-layer composite material cold shield which is light in weight, thin in wall, high in precision, high in strength, high in thermal conductivity and high in outer surface reflection is prepared by regulating and controlling the proportion of pure copper to nickel and cobalt in cooperation with special surface polishing treatment. The cold shield prepared by the method simultaneously meets the performance requirements of high strength, high heat conductivity and high outer surface reflection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of refrigerated infrared focal plane detectors, and in particular to a preparation method of a high-strength, high-thermal-conductivity, and high-reflectivity multi-layer composite cold screen and a cold screen. Background Art

[0002] The Dewar used in the refrigerated infrared focal plane detector is a vacuum insulation device, which not only provides a suitable low-temperature working environment for the detector chip, but also provides optical, mechanical and electrical interfaces for the detector. It is one of the core components of the infrared focal plane detector assembly. The cold screen is one of the key components of the Dewar assembly. As an optical exit pupil, the cold screen mainly plays the role of limiting the field of view. It should have a good stray light suppression effect. In order to better suppress stray light, a complex extinction structure is usually designed, and the inner surface is blackened to absorb stray light. At the same time, the assembly must work at a low temperature, and the cold screen has a greater impact on the cooling of the assembly. In order to effectively shorten the refrigeration startup time, the thermal conductivity of the cold screen is required to be high. In addition, the outer surface of the cold screen faces the normal temperature Dewar window frame seat shell. In order to reduce radiation heat leakage, the reflectivity of the outer surface of the cold screen should be high. To this end, the manufacturing of the cold screen must meet the performance requirements of light weight, thin wall, high precision, high strength, high thermal conductivity, and high reflectivity of the outer surface, so as to achieve the best match with the detector performance to more effectively shorten the cooling time and shield stray radiation.

[0003] Because the same metal material cannot have both high strength and high thermal conductivity, over the years, in order to meet the basic requirements of light weight, thin wall, high precision and high strength of the cold screen, low thermal conductivity and high strength nickel-cobalt cold screens have been widely used. In recent years, although the electroformed pure copper cold screen has met the requirements of high thermal conductivity of the cold screen, the copper cold screen has low strength and poor reliability. Although the method of gold plating on the outer surface of the cold screen has achieved the performance requirements of high strength and high reflectivity of the outer surface, the cold screens prepared domestically have not been able to have the excellent performance of high strength, high thermal conductivity and high reflectivity of the outer surface at the same time. Summary of the invention

[0004] The purpose of the present invention is to overcome the above-mentioned shortcomings and provide a method for preparing a high-strength, high-thermal-conductivity and high-reflectivity multi-layer composite cold screen to solve the problem that the cold screen prepared by traditional technology cannot have high strength, high thermal conductivity and high reflectivity on the outer surface at the same time.

[0005] The overall concept of the present invention is: using high thermal conductivity pure copper material as the middle layer of the multi-layer composite cold screen, and high strength nickel-cobalt alloy material as the boundary layer of the multi-layer composite cold screen; using double pulse electroforming, by adjusting the proportion of pure copper and nickel-cobalt components and combining with special surface polishing treatment, a multi-layer composite material cold screen that meets the requirements of light weight, thin wall, high precision, high strength, high thermal conductivity, and high reflection on the outer surface is prepared; the cold screen prepared by this method simultaneously meets the performance requirements of high strength, high thermal conductivity, and high reflection on the outer surface.

[0006] The technical solution of the present invention is:

[0007] A method for preparing a high-strength, high-thermal-conductivity, high-reflectivity multi-layer composite cold shield comprises the following steps:

[0008] Step 1, processing the cold screen core mold made of aluminum alloy;

[0009] Step 2, core mold surface treatment;

[0010] Step 3, electroforming a multi-layer composite cold shield;

[0011] Step 4, post-processing of multi-layer cold shield.

[0012] Furthermore, the surface pretreatment of the aluminum core mold in step 2 includes the following steps in sequence:

[0013] Step 21, degreasing and cleaning the core mold: placing the core mold in a solvent-based oil cleaning agent for ultrasonic cleaning for 40 to 60 minutes;

[0014] Step 22, core mold sandblasting: sandblast the core mold in all directions;

[0015] Step 23, ultrasonic cleaning of the core mold: ultrasonically cleaning the sandblasted core mold in pure water at 30 to 50° C. for 10 to 30 minutes;

[0016] Step 24, drying the core mold: drying the core mold after ultrasonic cleaning;

[0017] Step 25, core mold activation: place the core mold completely in an activation solution at 80°C to 90°C for 10 to 30 seconds. The activation solution formula is: H3PO4: 300ml; HNO3: 20ml; H2O: 80ml;

[0018] Step 26, core mold water washing: completely immerse the activated core mold in pure water, and perform ultrasonic cleaning until the acid and dirt on the surface of the core mold are completely removed.

[0019] Furthermore, the step 3 of electroforming a multilayer composite material cold shield comprises the following steps in sequence:

[0020] Step 31, electroforming the cold shield base layer: immerse the surface treated core mold as a cathode in a nickel-cobalt solution for electroforming. The current density is 2 to 10 A / dm 2 ,t C =10ms,t AA =5ms, pulse duty cycle is 20% to 50%, time is 1 to 4h. The formula of nickel-cobalt solution is Ni(NH2SO3)2·4H2O:400 to 500g / L, Co(NH2SO3)2·4H2O:10g / L, NiCl2:20g / L,

[0021] H3BO3: 30~40g / L, C 12 H 25 SO4Na: 0.1g / L, casting temperature is 40-50℃, and casting pH is 3.5-4.5.

[0022] Step 32, surface treatment of the cold shield substrate: take out the cold shield, put it in 50℃ pure water for ultrasonic cleaning for 3min~5min, blow it dry quickly, put it in 40~50℃ polishing liquid for polishing for 30s~120s, take out the parts and rinse them in pure water for 30~90s. The formula of the polishing liquid is: 550ml of bright polishing liquid, 100ml of surfactant, and 350ml of water.

[0023] Step 33, electroforming the cold shield middle layer: immerse the cold shield as a cathode in a copper solution for electroforming. The current density is 3 to 10 A / dm 2 ,t C =10ms,t AA =2ms, pulse duty ratio is 50% to 80%, time is 1 to 4h. Copper solution formula: CuSO4·5H2O: 150g to 200g / L, H2SO4: 50 to 80ml / L, HCl: 1ml / L, brightening additive 3ml to 5ml / L, casting temperature is 20℃ to 30℃, casting pH is 1.

[0024] Step 34, surface treatment of the middle layer of the cold shield: take out the cold shield, put it into 50℃ pure water for ultrasonic cleaning for 3min~5min, and then blow it dry quickly; then put it into 40~50℃ polishing liquid for polishing for 30s~120s, take out the parts and rinse them in pure water for 30~90s.

[0025] Step 35, electroforming the outermost layer of the cold shield: immerse the cold shield in a nickel-cobalt solution for electroforming. The current density is 2 to 10 A / dm 2 ,t C =10ms,t AA =5ms, pulse duty cycle is 20%~50%, time is 1~4h.

[0026] Step 36, surface treatment of the outermost layer of the cold shield: take out the cold shield, put it into 40℃~50℃ pure water for ultrasonic cleaning for 2min~3min, and then use nitrogen to quickly blow dry.

[0027] Furthermore, the post-processing of the multi-layer cold shield in step 4 includes the following steps in sequence:

[0028] Step 41, cold screen trimming: remove excess parts.

[0029] Step 42, cold screen demoulding: completely immerse the cold screen in a demoulding solution at 80°C to 90°C until the core mold is completely removed. The formula of the demoulding solution is 500g NaOH (AR); 2500ml H2O.

[0030] Step 43, cold screen cleaning: place the cold screen in pure water for ultrasonic cleaning, changing the pure water 2-3 times in the middle until the demoulding dirt on the inner and outer surfaces of the cold screen is removed.

[0031] Step 44, cold screen light emission: completely immerse the cold screen in the light emission liquid and ultrasonicate for 10 to 30 seconds. The formula of the light emission solution is HNO3: 200 to 250 ml; H2SO4: 80 to 100 ml; H2O: 60 to 100 ml.

[0032] Step 45, cold screen cleaning: after the light is emitted, the cold screen is taken out and completely immersed in water for ultrasonic cleaning until the solution and dirt on the inner and outer surfaces of the cold screen are completely removed.

[0033] Step 46, blow-dry the cold screen: completely place the cold screen in ethanol, take it out after 10s to 30s, and blow-dry it quickly.

[0034] The present invention also provides a cold screen prepared by the method for preparing the high-strength, high-thermal-conductivity, high-reflectivity multi-layer composite cold screen.

[0035] The mechanism and beneficial effects of the present invention include:

[0036] (1) The present invention utilizes double pulse electroforming, uses high thermal conductivity pure copper material as the middle layer of the cold shield, and high strength nickel-cobalt alloy material as the boundary layer of the cold shield. By adjusting the composition ratio of pure copper and nickel-cobalt and combining with special surface polishing treatment, a multilayer composite cold shield with excellent performance is prepared;

[0037] (2) In order to ensure high reflectivity of the outer surface of the prepared cold shield, the present invention performs the most appropriate surface treatment on the surfaces of the different layers of materials;

[0038] (3) In order to ensure the strong bonding force and high thickness uniformity between the prepared cold shield multilayer materials, the present invention adopts a suitable bidirectional pulse process;

[0039] (4) In order to achieve the excellent performance of high strength, high thermal conductivity and high outer surface reflection of the multi-layer cold shield, the present invention adopts the most appropriate layer thickness ratio.

[0040] (5) The present invention solves the problem that traditional nickel-cobalt cold screens and copper cold screens cannot simultaneously meet the requirements of high strength, high thermal conductivity, and high outer surface reflection. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is a double pulse current waveform.

[0042] Figure 2 This is a schematic diagram of the forward section of the multi-layer composite cold shield.

[0043] Figure 3This is a schematic diagram of the forward section of a traditional single-layer cold shield. DETAILED DESCRIPTION

[0044] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and several embodiments.

[0045] like Figure 2 As shown, the cold shield prepared by the process of the present invention can have a complex and diverse shape, and the specific shape can be designed according to the corresponding core mold according to the needs.

[0046] Example 1 is a detailed description case, and Examples 2 to 4 are detailed descriptions of steps (8) to (13) during the electroforming of the cold screen.

[0047] Example 1

[0048] A method for preparing a high-strength, high-thermal-conductivity, and high-reflectivity multi-layer composite cold shield is prepared in the following steps:

[0049] (1) Processing aluminum core mold with qualified dimensions.

[0050] (2) Core mold degreasing and cleaning: Place it in a solvent-based oil cleaning agent and ultrasonically clean it for 60 minutes, then air dry it.

[0051] (3) Cold screen core mold sandblasting.

[0052] (4) Core mold cleaning: Ultrasonic cleaning in 45°C water for 30 minutes.

[0053] (5) Drying the core mold: Dry in a ventilated place.

[0054] (6) Activation of core mold: Place it completely in 90℃ activation solution for 30 seconds.

[0055] (7) Core mold water washing: Immerse in pure water and perform ultrasonic cleaning until the acid and dirt on the surface of the core mold are completely removed.

[0056] (8) Electroforming cold screen base layer: The core mold is clamped on the tooling and immersed in the nickel-cobalt electroforming liquid as a cathode for double pulse electroforming (such as Figure 1 As shown), forward current density 8A / dm 2 , reverse current density 5A / dm 2 , forward duty cycle 50%, reverse duty cycle 30%, tc = 10ms, tAA = 5ms, time is 2h. The electroforming solution formula is

[0057] Ni(NH2SO3)2·4H2O:400g / L, Co(NH2SO3)2·4H2O:10g / L, NiCl2:20g / L, H3BO3:35g / L,

[0058] C 12 H25 SO4Na: 0.1g / L, casting temperature is 40℃, and casting pH is 4.0.

[0059] (9) Surface treatment of the cold screen substrate: Take out the cold screen, put it in 50℃ pure water for ultrasonic cleaning for 3 minutes, use nitrogen to quickly blow dry, then put it in 50℃ polishing liquid for polishing for 60 seconds, take out the parts and rinse them in pure water for 90 seconds. The formula of the polishing liquid is: 550ml of bright polishing liquid, 100ml of surfactant, and 350ml of water.

[0060] (10) Electroforming cold shield middle layer: The core mold is clamped on the tooling and immersed in the copper electroforming liquid as a cathode for double pulse electroforming. The forward current density is 10A / dm 2 , reverse current density 5A / dm 2 , forward duty cycle 80%, reverse duty cycle 50%, tc = 10ms, tAA = 2ms, time is 1.5h. Electroforming solution formula: CuSO4·5H2O: 180g / L,

[0061] H2SO4: 70ml / L, HCl: 1ml / L, brightening additive 5ml / L, casting temperature is 28℃, and casting pH is 1.

[0062] (11) Surface treatment of the cold screen intermediate layer: Take out the cold screen, put it in 50℃ pure water for ultrasonic cleaning for 3 minutes, use nitrogen to blow it dry quickly, then put it in 50℃ polishing liquid for polishing for 30 seconds, take out the parts and rinse them in pure water for 90 seconds. The formula of the polishing liquid is: 550ml of bright polishing liquid, 100ml of surfactant, and 350ml of water.

[0063] (12) The outermost layer of the electroformed cold screen: The core mold is clamped on the fixture and immersed in the nickel-cobalt electroforming liquid as a cathode for double pulse electroforming with a forward current density of 8A / dm 2 , reverse current density 5A / dm 2 , forward duty cycle 50%, reverse duty cycle 30%, tc = 10ms, tAA = 5ms, time is 2h. The electroforming solution formula is Ni(NH2SO3)2·4H2O: 400g / L, Co(NH2SO3)2·4H2O: 10g / L, NiCl2: 20g / L, H3BO3: 35g / L, C 12 H 25 SO4Na: 0.1g / L, casting temperature is 40℃, and casting pH is 4.0.

[0064] (13) Surface treatment of the outermost layer of the cold shield: Take out the cold shield, put it into 50°C pure water for ultrasonic cleaning for 3 minutes, and quickly blow dry it with nitrogen.

[0065] (14) Cold screen size trimming: Trim the cold screen after electroforming to remove excess parts.

[0066] (15) Cold screen demoulding: Place the cold screen completely in the boiling demoulding solution until the core mold is completely removed. The formula of the demoulding solution is NaOH (AR) 500g; H2O: 2500ml.

[0067] (16) Cold screen cleaning: Place the cold screen in pure water for ultrasonic cleaning, changing the pure water 2-3 times in the middle until the demolding dirt on the inner and outer surfaces of the cold screen is removed.

[0068] (17) Cold screen light extraction: Immerse the cold screen completely in the light extraction solution and ultrasonicate for 20 seconds. The light extraction solution formula is HNO3: 250ml; H2SO4: 80ml; H2O: 90ml.

[0069] (18) Cold screen cleaning: Place the cold screen in pure water at room temperature for ultrasonic cleaning, changing the pure water 3-4 times in the process until the solution and dirt on the inner and outer surfaces of the cold screen are removed.

[0070] (19) Blow-drying the cold screen: Place the cold screen completely in ethanol for 20 seconds. After taking out the cold screen, blow it dry quickly under a nitrogen gun.

[0071] The above-mentioned part is a multilayer composite cold shield with a composition ratio of 1 (nickel cobalt): 2 (copper): 1 (nickel cobalt), a thermal conductivity of 184.2 W / (mk), a Vickers hardness of 320 HV, and an average reflectivity of the outer surface of 0.93.

[0072] Example 2

[0073] The core mold is clamped on the fixture and immersed in the nickel-cobalt solution as a cathode for double pulse electroforming. The electroforming parameters are J C =8A / dm 2 ,J AA =5A / dm 2 ,γ c =50%,γ AA =30%,t C =10ms,t AA =5ms. After electroforming for 1.5h, take it out, put it into 50℃ pure water, ultrasonically clean it for 3min, blow it dry quickly, then put it into 50℃ polishing liquid for 60s, take out the cold screen and rinse it in pure water for 90s.

[0074] The surface treated cold screen was re-clamped on the fixture and immersed in the copper solution as a cathode for double pulse electroforming. The electroforming parameters were J C =10A / dm 2 ,J AA =5A / dm 2 ,γ c =80%,γAA =50%,t C =10ms,t AA = 2ms. After electroforming for 2h, take it out, put it into 50℃ pure water for ultrasonic cleaning for 3min, blow it dry quickly, then put it into 50℃ polishing liquid for polishing for 30s, and rinse it with pure water for 90s.

[0075] The surface treated cold screen was re-clamped on the fixture and immersed in the nickel-cobalt solution as a cathode for double pulse electroforming. The electroforming parameters were J C =8A / dm 2 ,J AA =5A / dm 2 ,γ c =50%,γ AA =30%,t C =10ms,t AA =5ms, take it out after electroforming for 1.5h, and rinse it in pure water until there is no dirt on the surface.

[0076] The obtained part is a multilayer composite cold shield with a layer thickness ratio of 1 (nickel cobalt): 3 (copper): 1 (nickel cobalt), a thermal conductivity of 275.5 W / (mk), a Vickers hardness of 271 HV, and an average reflectivity of the outer surface of 0.94.

[0077] Example 3

[0078] The core mold is clamped on the fixture and immersed in the nickel-cobalt electroforming solution as a cathode for double pulse electroforming. The electroforming parameters are J C =8A / dm 2 ,J AA =5A / dm 2 ,γ c =50%,γ AA =30%,t C =10ms,t AA =5ms, electroforming 7.5h, the obtained part is a single-layer cold shield composed of nickel-cobalt alloy material, with a thermal conductivity of 84.1W / (mk), a Vickers hardness of 290HV, and an average reflectivity of the outer surface of 0.75.

[0079] Example 4

[0080] The core mold is clamped on the fixture and immersed in the copper electroforming liquid as a cathode for pulse electroforming. The electroforming parameters are J C =10A / dm 2 ,J AA =5A / dm 2 ,γ c =80%,γ AA =50%,t C =10ms,t AA=2ms, electroforming for 3.5 hours, the obtained part is a single-layer cold shield composed of pure copper material, with a thermal conductivity of 275.8W / (mk), a Vickers hardness of 140HV, and a final average reflectivity of the outer surface of 0.81.

[0081] It can be seen from the above examples that a single-layer nickel-cobalt cold screen has high strength, low thermal conductivity and poor reflectivity; a single-layer copper cold screen has high thermal conductivity but low strength. The present invention adjusts the proportion of pure copper and nickel-cobalt components, combines special surface polishing treatment and uses double-pulse electroforming to prepare a multi-layer (nickel-cobalt-copper-nickel-cobalt) composite cold screen with excellent properties of high strength, high thermal conductivity and high reflectivity on the outer surface.

Claims

1. A method for preparing a high-strength, high-thermal-conductivity, and high-reflectivity multi-layer composite cold shield. It is characterized in that The steps include: Step 1, processing the cold screen core mold made of aluminum alloy; Step 2, core mold surface treatment; Step 3, electroforming a multi-layer composite cold shield, comprising: Step 31, immersing the surface-treated core mold as a cathode in a nickel-cobalt solution to electroform a cold shield base layer; Step 32, surface treatment of the cold shield base layer; Step 33, immersing the cold shield as a cathode in a copper solution to electroform a cold shield intermediate layer; Step 34, surface treatment of the cold shield intermediate layer; Step 35, immersing the cold shield in a nickel-cobalt solution to electroform the outermost layer of the cold shield; Step 36, treating the outermost surface of the cold shield; Step 4, post-processing of multi-layer cold shield.

2. A method for preparing a high-strength, high-thermal-conductivity, high-reflectivity multi-layer composite cold shield according to claim 1, It is characterized in that In step 31: The formula of the nickel-cobalt solution is: Ni(NH 2 SO 3 ) 2 ·4H 2 O: 400~500g / L, Co(NH 2 SO 3 ) 2 ·4H 2 O:10g / L,NiCl 2 :20g / L,H 3 BO 3 :30~40g / L, C 12 H 25 SO 4 Na: 0.1 g / L; The temperature of the nickel-cobalt solution is 40-50°C, and the pH value of the nickel-cobalt solution is 3.5-4.

5.

3. A method for preparing a high-strength, high-thermal-conductivity, high-reflectivity multi-layer composite cold shield according to claim 1, It is characterized in that In step 33: The formula of the copper solution is: CuSO 4 ·5H 2 O:150g~200g / L, H 2 SO 4 :50~80ml / L, HCl:1ml / L, brightening additive:3~5ml / L; The temperature of the copper solution is 20-30°C, and the pH value of the copper solution is 1.

4. A method for preparing a high-strength, high-thermal-conductivity, high-reflection multi-layer composite cold shield according to any one of claims 1 to 3, Features: The current density of electroforming in step 31 is 2 to 10 A / dm 2 ,t C =10ms,t AA =5ms, pulse duty cycle is 20%~50%, time is 1h~4h; The current density of electroforming in step 33 is 3 to 10 A / dm 2 ,t C =10ms,t AA =2ms, pulse duty cycle is 50% to 80%, time is 1 to 4h; The current density of electroforming in step 35 is 2 to 10 A / dm 2 ,t C =10ms,t AA =5ms, pulse duty cycle is 20%~50%, time is 1~4h.

5. A method for preparing a high-strength, high-thermal-conductivity, high-reflectivity multi-layer composite cold shield according to any one of claims 1 to 3, It is characterized in that In step 32, the surface treatment of the cold shield base layer includes: Take out the cold screen, put it into 50℃ pure water for ultrasonic cleaning for 3-5 minutes, blow it dry quickly, put it into 40-50℃ polishing liquid for polishing for 30-120 seconds, take out the parts and rinse them with pure water for 30-90 seconds; The polishing liquid formula is: 550ml of bright polishing liquid, 100ml of surfactant, and 350ml of water.

6. A method for preparing a high-strength, high-thermal-conductivity, high-reflectivity multi-layer composite cold shield according to any one of claims 1 to 3, Features: The surface treatment of the intermediate layer of the cold shield in step 34 includes: taking out the cold shield, ultrasonically cleaning it in 50°C pure water for 3-5 minutes, and then quickly drying it; then polishing it in 40-50°C polishing liquid for 30-120 seconds, taking out the parts and rinsing them in pure water for 30-90 seconds; The surface treatment of the outermost layer of the cold shield in step 36 includes: taking out the cold shield, putting it into 40-50° C. pure water for ultrasonic cleaning for 2-3 minutes, and then quickly blowing it dry with nitrogen.

7. A method for preparing a high-strength, high-thermal-conductivity, high-reflection multi-layer composite cold shield according to any one of claims 1 to 3, It is characterized in that Step 4 also includes: Step 41, cold screen trimming: removing excess parts; Step 42, cold screen demoulding: completely immerse the cold screen in a demoulding solution at 80-90° C. until the core mold is completely removed; Step 43, cold screen cleaning: placing the cold screen in pure water for ultrasonic cleaning, changing the pure water 2-3 times in the middle, until the demoulding dirt on the inner and outer surfaces of the cold screen is removed; Step 44, cold screen light emission: completely immerse the cold screen in the light emission liquid and perform ultrasound for 10 to 30 seconds; Step 45, cold screen cleaning: after the light is emitted, the cold screen is taken out and completely immersed in water for ultrasonic cleaning until the solution and dirt on the inner and outer surfaces of the cold screen are completely removed; Step 46, blow-dry the cold screen: completely place the cold screen in ethanol, take it out after 10 to 30 seconds, and blow-dry it quickly.

8. A method for preparing a high-strength, high-thermal-conductivity, high-reflectivity multi-layer composite cold shield according to claim 7, Features: The formula of the demoulding solution in step 42 is: NaOH: 500g, H 2 O: 2500ml; The formula of the light emitting solution in step 44 is: HNO 3 :200~250ml,H 2 SO 4 :80~100ml,H 2 O: 60~100ml.

9. A method for preparing a high-strength, high-thermal-conductivity, high-reflection multi-layer composite cold shield according to any one of claims 1 to 3, It is characterized in that The step 2 of pre-treating the core mold surface comprises: Step 21, degreasing and cleaning the core mold: placing the core mold in a solvent-based oil cleaning agent for ultrasonic cleaning for 40 to 60 minutes; Step 22, core mold sandblasting: sandblast the core mold in all directions; Step 23, ultrasonic cleaning of the core mold: ultrasonically cleaning the sandblasted core mold in pure water at 30 to 50° C. for 10 to 30 minutes; Step 24, drying the core mold: drying the core mold after ultrasonic cleaning; Step 25, core mold activation: place the core mold completely in the activation solution at 80-90°C for 10-30s. The activation solution formula is: H 3 PO 4 : 300ml, HNO 3 :20ml,H 2 O: 80ml; Step 26, core mold water washing: completely immerse the activated core mold in pure water, and perform ultrasonic cleaning until the acid and dirt on the surface of the core mold are completely removed.

10. A cold shield prepared by the method for preparing a high-strength, high-thermal-conductivity, high-reflectivity multi-layer composite cold shield according to any one of claims 1 to 9.