PET / PTT double-component hollow parallel elastic fiber and preparation method thereof

Through the preparation method of PET/PTT bicomponent hollow side-by-side elastic fibers, the specific structure on the spinneret is used to control the viscosity difference between the PET and PTT components to form fibers with high hollowness and good warmth retention properties, which solves the problems in the existing technology. The problems of insufficient fiber elasticity and poor thermal insulation performance.

CN118756358APending Publication Date: 2024-10-11SHANGHAI DEKAI IND CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410885906.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing hollow fibers are susceptible to extrusion deformation during the production process, resulting in reduced hollowness, low elasticity, and insufficient warmth retention properties. Multi-component hollow fibers have problems with insufficient resilience and poor wrinkle resistance.

Method used

Using PET/PTT two-component hollow side-by-side elastic fiber, by controlling the viscosity difference between the PET component and the PTT component, a hollow cavity is formed on the spinneret, and is prepared by cooling, oiling, stretching and winding , forming fibers with high hollowness and permanent crimp characteristics.

Benefits of technology

The PET/PTT bicomponent hollow side-by-side elastic fiber with high hollowness, high crimp shrinkage, lightweight fabric and good warmth retention properties has been realized, which solves the problems of insufficient fiber elasticity and poor warmth retention properties in the existing technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118756358A_ABST
    Figure CN118756358A_ABST
Patent Text Reader

Abstract

The invention provides a PET / PTT (polyethylene terephthalate / polytrimethylene terephthalate) two-component hollow parallel elastic fiber and a preparation method thereof. The preparation method comprises the following steps that (1) PET slices and PTT slices are subjected to melt extrusion, melt pipeline conveying and metering pump metering respectively, a PET spinning melt and a PTT spinning melt are obtained, and the viscosity difference between the PET spinning melt and the PTT spinning melt is smaller than or equal to 2200 poise; and (2) enabling the PET spinning melt and the PTT spinning melt to flow to a spinneret plate of a spinning assembly according to respective runners, converging on the spinneret plate, enabling a PET component and a PTT component sprayed by the spinneret plate to be connected with each other to form a melt trickle with a hollow cavity, and sequentially cooling, oiling, stretching, interlacing and winding to obtain the hollow parallel elastic fiber. A specific spinneret plate is adopted, the viscosity of the PET component and the viscosity of the PTT component are adjusted and controlled, and the hollow parallel elastic fiber which has the permanent three-dimensional crimp characteristic, is high in hollow degree and crimp shrinkage rate, is light in fabric weight and is good in heat retention property is prepared through the FDY technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyester spinning, in particular to a PET / PTT two-component hollow parallel elastic fiber and a preparation method thereof. Background Art

[0002] Polyester spinning materials have always been the key driving force for technological progress in the clothing and related industries. As a textile material with a special structure, hollow fibers are widely used in clothing, home textiles and special functional textiles because of their light weight, warmth retention and stable shape. Currently, most hollow fibers on the market are single-component structures and are produced through the POY-DTY process. Although this process is mature, the fibers are easily extruded and deformed during the production process, resulting in reduced hollowness, low elasticity, and insufficient warmth retention. There are also some multi-component hollow fibers, which are made by spinning a variety of polyester blends, and have problems such as insufficient resilience and poor wrinkle resistance. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the deficiencies in the prior art, the present invention provides a PET / PTT two-component hollow parallel elastic fiber and a preparation method thereof, which solves the problems raised in the above-mentioned background technology.

[0005] (II) Technical solution

[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0007] According to a first aspect of the present invention, a PET / PTT two-component hollow parallel elastic fiber is provided, comprising a PET component and a PTT component, wherein the PET component and the PTT component are connected to each other to form a hollow parallel elastic fiber having a hollow cavity, wherein the single fiber fineness of the hollow parallel elastic fiber is 1 to 3.5 dtex, the breaking strength is ≥2.8 cN / dtex, and the hollowness is ≥16%.

[0008] Preferably, the wall thickness of the hollow parallel elastic fibers is 0.1-0.5 mm, the inner diameter of the long axis of the hollow parallel elastic fibers is 0.5-0.8 mm, and the outer diameter of the long axis of the hollow fibers is 0.7-1.0 mm.

[0009] Preferably, the hollow parallel elastic fibers have an elongation at break of 30-40%, a wastewater shrinkage of 12-15%, an oil content of 0.8-1.2%, a curling shrinkage of 60-70%, and a yarn unevenness of ≤1.6%.

[0010] According to a second aspect of the present invention, there is provided a method for preparing a PET / PTT two-component hollow parallel elastic fiber, comprising the following steps:

[0011] (1) melt-extruding PET slices and PTT slices respectively, transporting them through a melt pipeline and metering them through a metering pump to obtain a PET spinning melt and a PTT spinning melt, wherein the viscosity difference between the PET spinning melt and the PTT spinning melt is ≤2200 poise;

[0012] (2) The PET spinning melt and the PTT spinning melt flow to the spinneret of the spinning assembly according to their respective flow channels, merge at the spinneret, and the PET component and the PTT component ejected from the spinneret are connected to each other to form a melt stream with a hollow cavity, and then sequentially cooled, oiled, stretched, shaped and wound to obtain the hollow parallel elastic fiber.

[0013] In order to enable the PET spinning melt and the PTT spinning melt to spray out the two-component hollow parallel elastic fibers through a specific spinneret, the viscosity difference between the PET spinning melt and the PTT spinning melt must be ≤2000 poise to prepare the fibers.

[0014] Further preferably, in step (1), the viscosity difference between the PET spinning melt and the PTT spinning melt is 1000 to 2000 poise.

[0015] Preferably, in step (2), the spinneret includes a spinneret body and a plurality of spinneret holes, the cross-section of the spinneret holes includes a first C-shaped hole, a second C-shaped hole, and an elliptical hole formed by connecting the first C-shaped hole and the second C-shaped hole end to end, and the area of ​​the first C-shaped hole is greater than the area of ​​the second C-shaped hole.

[0016] Preferably, the major axis of the large ellipse formed by the first C-shaped hole and the second C-shaped hole connected end to end is 0.7-1.0 mm, and the major axis of the inner small ellipse formed by the first C-shaped hole and the second C-shaped hole connected end to end is 0.5-0.8 mm, wherein the major axis of the large ellipse and the major axis of the inner small ellipse are located on the same horizontal line, and the minor axis of the large ellipse is parallel to the minor axis of the inner small ellipse and does not overlap.

[0017] Preferably, in step (2), the spinneret holes on the spinneret plate include four C-shaped microholes with the same structure, and the four C-shaped microholes are continuously arranged in a circular array;

[0018] The distance between two adjacent C-shaped microholes is 0.05-0.12 mm;

[0019] The inner diameter of the C-shaped micropore is 0.7-1.0 mm, and the outer diameter of the C-shaped micropore is 0.5-0.8 mm.

[0020] Preferably, in step (2), the spinning temperature of the PET spinning melt is 270-295°C, and the spinning temperature of the PTT spinning melt is 242-272°C.

[0021] Preferably, in step (2), the melt stream is sequentially cooled, oiled, stretched, shaped and wound to obtain the hollow parallel elastic fiber with the following process parameters:

[0022] Cooling temperature 20~24℃;

[0023] Network pressure 0.3~0.4MPa;

[0024] One roller speed 1600~2100m / min;

[0025] The temperature of the first roller is 65~80℃;

[0026] Second roller speed 3800~3900m / min;

[0027] Second roller temperature 130~155℃;

[0028] Winding speed 3750~3800m / min.

[0029] (III) Beneficial effects

[0030] The present invention provides a PET / PTT two-component hollow parallel elastic fiber and a preparation method thereof. The fiber has the following beneficial effects:

[0031] The present invention provides a method for preparing a PET / PTT two-component hollow parallel elastic fiber, which adopts a PET component and a PTT component, and controls the viscosity of the PET component and the PTT component by controlling the temperature, so that the PET spinning melt and the PTT spinning melt are respectively ejected from the corresponding channels of the spinneret, and then sequentially subjected to cooling, oiling, stretching, shaping and winding to obtain a hollow parallel elastic fiber, which has the characteristics of permanent three-dimensional curling, high hollowness, high curling shrinkage, and the advantages of lightweight fabric and good warmth retention. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic cross-sectional view of the first spinneret hole in the process of preparing a PET / PTT two-component hollow parallel elastic fiber of the present invention;

[0033] Figure 2 It is a cross-sectional schematic diagram of the second spinneret hole in the process of preparing a PET / PTT two-component hollow parallel elastic fiber of the present invention;

[0034] Figure 3 This is an electron microscope image of a cross section of a PET / PTT two-component hollow parallel elastic fiber prepared in Example 1 of the present invention;

[0035] Figure 1 Among them, 1. the first C-shaped hole; 2. the second C-shaped hole; 3. the elliptical hole. DETAILED DESCRIPTION

[0036] In order to better illustrate the content of the present invention, a detailed description is given below in conjunction with specific embodiments.

[0037] The present invention adopts a spinneret, which comprises a spinneret body and a plurality of spinneret holes, wherein the cross section of the spinneret holes is as follows: Figure 1 As shown, it includes a first C-shaped hole 1 , a second C-shaped hole 2 , and an inner elliptical hole 3 formed by connecting the first C-shaped hole 1 and the second C-shaped hole 2 end to end, wherein the area of ​​the first C-shaped hole 1 is greater than that of the second C-shaped hole 2 .

[0038] In a specific embodiment, the major axis of the large ellipse formed by the first C-shaped hole 1 and the second C-shaped hole 2 connected end to end is 0.7-1.0 mm, and the major axis of the inner small ellipse formed by the first C-shaped hole 1 and the second C-shaped hole 2 connected end to end is 0.5-0.8 mm, wherein the major axis of the large ellipse and the major axis of the inner small ellipse are located on the same horizontal line, and the minor axis of the large ellipse is parallel to the minor axis of the inner small ellipse and does not overlap.

[0039] In a specific embodiment, the first C-shaped hole 1 is a channel for ejecting the PET spinning melt, and the second C-shaped hole 2 is a channel for ejecting the PTT spinning melt.

[0040] Another spinneret used in the present invention comprises a spinneret body and a plurality of spinneret holes, wherein the cross section of the spinneret hole is as follows: Figure 2 As shown, the spinneret includes four C-shaped microholes with the same structure, and the four C-shaped microholes are continuously arranged in a circular array; the distance between two adjacent C-shaped microholes is 0.05-0.12 mm; the inner diameter of the C-shaped microhole is 0.7-1.0 mm, and the outer diameter of the C-shaped microhole is 0.5-0.8 mm.

[0041] Example 1

[0042] The major axis of the large ellipse of the spinneret hole in the spinneret plate of this embodiment is 1.0 mm, and the major axis of the small ellipse inside is 0.8 mm.

[0043] The above spinneret is used to prepare a PET / PTT two-component hollow parallel elastic fiber, PET slices and PTT slices are melt-extruded respectively, and the melt is transported by a melt pipeline and metered by a metering pump to obtain a PET spinning melt and a PTT spinning melt, and the viscosity difference between the PET spinning melt and the PTT spinning melt is controlled to be 2000 poise; then the PET spinning melt and the PTT spinning melt flow to the spinneret of the spinning assembly according to their respective flow channels, and the PET component and the PTT component ejected from the spinneret are connected to each other to form a melt stream with a hollow cavity, wherein the PET spinning melt is ejected through a first C-shaped hole, and the PTT spinning melt is ejected through a second C-shaped hole, and then cooled, oiled, stretched, shaped and wound in sequence to obtain a PET / PTT two-component hollow parallel elastic fiber, such as Figure 3 shown.

[0044] In this embodiment, the spinning temperature of the PET spinning melt is 270°C, the spinning temperature of the PTT spinning melt is 242°C, the cooling temperature is 23°C, the network pressure is 0.32MPa, the speed of one roller is 1620m / min, the temperature of one roller is 78°C, the speed of the second roller is 3900m / min, the temperature of the second roller is 140°C, and the winding speed is 3800m / min.

[0045] The PET / PTT two-component hollow parallel elastic fiber prepared in this embodiment was tested, and its hollowness was 23.9%, the single fiber fineness was 3.46 dtex, the breaking strength was 2.95 cN / dtex, the breaking elongation was 30%, the boiling water shrinkage was 13%, the oil content was 1.0%, the curling shrinkage was 65%, and the CV value of the unevenness of the yarn was 1.05%.

[0046] Example 2

[0047] The spinneret of this embodiment includes four C-shaped microholes with the same structure, which are continuously arranged in a circular array; the distance between two adjacent C-shaped microholes is 0.12mm; the inner diameter of the C-shaped microhole is 0.7, and the outer diameter of the C-shaped microhole is 0.5mm.

[0048] The above spinneret is used to prepare PET / PTT two-component hollow parallel elastic fibers, PET slices and PTT slices are melt-extruded respectively, and the melts are transported by pipelines and metered by metering pumps to obtain PET spinning melt and PTT spinning melt, and the viscosity difference between the PET spinning melt and the PTT spinning melt is controlled to be 2200 poise; then the PET spinning melt and the PTT spinning melt flow to the spinneret of the spinning assembly according to their respective flow channels, and merge at the spinneret, and the PET component and the PTT component ejected from the spinneret are connected to each other to form a melt stream with a hollow cavity, wherein the PET spinning melt is ejected through two adjacent C-shaped micropores, and the PTT spinning melt is ejected through another two adjacent C-shaped micropores, and then cooled, oiled, stretched, shaped and wound in sequence to obtain the PET / PTT two-component hollow parallel elastic fibers.

[0049] In this embodiment, the spinning temperature of the PET spinning melt is 295°C, the spinning temperature of the PTT spinning melt is 272°C, the cooling temperature is 23°C, the network pressure is 0.32MPa, the speed of one roller is 2100m / min, the temperature of one roller is 60°C, the speed of the second roller is 3800m / min, the temperature of the second roller is 135°C, and the winding speed is 3750m / min.

[0050] The PET / PTT two-component hollow parallel elastic fiber prepared in this embodiment was tested, and its hollowness was 18%, the single fiber fineness was 2.08 dtex, the breaking strength was 3.0 cN / dtex, the breaking elongation was 32%, the boiling water shrinkage was 13%, the oil content was 1.2%, the curling shrinkage was 62%, and the CV value of the yarn unevenness was 0.95%.

[0051] Example 3

[0052] The preparation method of this embodiment is the same as that of embodiment 1, except that the viscosity difference between the PET spinning melt and the PTT spinning melt is 1500 poise.

[0053] The PET / PTT two-component hollow parallel elastic fiber prepared in this embodiment was tested, and its hollowness was 24.1%, the single fiber fineness was 3.52 dtex, the breaking strength was 3.35 cN / dtex, the breaking elongation was 31%, the boiling water shrinkage was 13%, the oil content was 1.0%, the curling shrinkage was 68%, and the CV value of the unevenness of the yarn was 1.00%.

[0054] Example 4

[0055] The preparation method of this embodiment is the same as that of embodiment 1, except that the viscosity difference between the PET spinning melt and the PTT spinning melt is 1000 poise.

[0056] The PET / PTT two-component hollow parallel elastic fiber prepared in this embodiment was tested, and its hollowness was 24.3%, the single fiber fineness was 3.54 dtex, the breaking strength was 2.9 cN / dtex, the breaking elongation was 30%, the boiling water shrinkage was 13%, the oil content was 0.8%, the curling shrinkage was 60%, and the CV value of the unevenness of the yarn was 1.00%.

[0057] Example 5

[0058] The preparation method of this embodiment is the same as that of embodiment 1, except that the viscosity difference between the PET spinning melt and the PTT spinning melt is 800 poise.

[0059] The PET / PTT two-component hollow parallel elastic fiber prepared in this embodiment was tested, and its hollowness was 21.6%, the single fiber fineness was 2.95 dtex, the breaking strength was 2.9 cN / dtex, the breaking elongation was 30%, the boiling water shrinkage was 13%, the oil content was 0.8%, the curling shrinkage was 60%, and the CV value of the unevenness of the yarn was 1.00%.

[0060] Comparative Example 1

[0061] The preparation method of this comparative example is the same as that of Example 1, except that the viscosity difference between the PET spinning melt and the PTT spinning melt is 2300 poise.

[0062] In this comparative example, due to the large viscosity difference, the PET spinning melt bends toward the PTT spinning melt when the filaments are discharged from the spinneret, resulting in sticking of the sheet and failure to spin into finished products.

[0063] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A PET / PTT two-component hollow parallel elastic fiber, characterized in that: The hollow parallel elastic fiber comprises a PET component and a PTT component. The PET component and the PTT component are connected to each other to form a hollow parallel elastic fiber with a hollow cavity. The single fiber fineness of the hollow parallel elastic fiber is 1 to 3.5 dtex, the breaking strength is ≥2.8 cN / dtex, and the hollowness is ≥16%.

2. The PET / PTT two-component hollow parallel elastic fiber according to claim 1, characterized in that: The wall thickness of the hollow parallel elastic fiber is 0.1-0.5 mm, the inner diameter of the long axis of the hollow parallel elastic fiber is 0.5-0.8 mm, and the outer diameter of the long axis of the hollow fiber is 0.7-1.0 mm.

3. The PET / PTT two-component hollow parallel elastic fiber according to claim 1, characterized in that: The hollow parallel elastic fibers have a breaking elongation of 30-40%, a wastewater shrinkage of 12-15%, an oil content of 0.8-1.2%, a curling shrinkage of 60-70%, and a yarn unevenness of ≤1.6%.

4. A method for preparing the PET / PTT two-component hollow parallel elastic fiber according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) melt-extruding PET slices and PTT slices respectively, transporting them through a melt pipeline and metering them through a metering pump to obtain a PET spinning melt and a PTT spinning melt, wherein the viscosity difference between the PET spinning melt and the PTT spinning melt is ≤2200 poise; (2) The PET spinning melt and the PTT spinning melt flow to the spinneret of the spinning assembly according to their respective flow channels, merge at the spinneret, and the PET component and the PTT component ejected from the spinneret are connected to each other to form a melt stream with a hollow cavity, and then sequentially cooled, oiled, stretched, networked and wound to obtain the hollow parallel elastic fiber.

5. The method for preparing a PET / PTT two-component hollow parallel elastic fiber according to claim 4, characterized in that: In step (1), the viscosity difference between the PET spinning melt and the PTT spinning melt is 1000 to 2000 poise.

6. The method for preparing a PET / PTT two-component hollow parallel elastic fiber according to claim 4, characterized in that: In step (2), the cross-section of the spinneret on the spinneret plate includes a first C-shaped hole, a second C-shaped hole, and an inner elliptical hole formed by connecting the first C-shaped hole and the second C-shaped hole end to end, and the area of ​​the first C-shaped hole is larger than that of the second C-shaped hole.

7. The method for preparing a PET / PTT two-component hollow parallel elastic fiber according to claim 6, characterized in that: The major axis of the large ellipse formed by the first C-shaped hole and the second C-shaped hole connected end to end is 0.7-1.0 mm, and the major axis of the inner small ellipse formed by the first C-shaped hole and the second C-shaped hole connected end to end is 0.5-0.8 mm, wherein the major axis of the large ellipse and the major axis of the inner small ellipse are located on the same horizontal line, and the minor axis of the large ellipse is parallel to the minor axis of the inner small ellipse and does not overlap.

8. The method for preparing a PET / PTT two-component hollow parallel elastic fiber according to claim 4, characterized in that: In step (2), the spinneret holes on the spinneret plate include four C-shaped microholes with the same structure, and the four C-shaped microholes are continuously arranged in a circular array; The distance between two adjacent C-shaped microholes is 0.05-0.12 mm; The inner diameter of the C-shaped micropore is 0.7-1.0 mm, and the outer diameter of the C-shaped micropore is 0.5-0.8 mm.

9. The method for preparing a PET / PTT two-component hollow parallel elastic fiber according to claim 4, characterized in that: In step (2), the spinning temperature of the PET spinning melt is 270-295°C, and the spinning temperature of the PTT spinning melt is 242-272°C.

10. The method for preparing a PET / PTT two-component hollow parallel elastic fiber according to claim 4, characterized in that: In step (2), the melt stream is sequentially cooled, oiled, stretched, shaped and wound to obtain the hollow parallel elastic fiber with the following process parameters: Cooling temperature 20~24℃; Network pressure 0.3~0.4MPa; One roller speed 1600~2100m / min; The temperature of the first roller is 65~80℃; Second roller speed 3800~3900m / min; Second roller temperature 130~155℃; Winding speed 3750~3800m / min.

Citation Information

Patent Citations

  • High-hollowness polyester filament and preparation method thereof as well as polyester filament for filling and preparation method thereof

    CN115595688A

  • High-hollowness wear-resistant polyester fiber and preparation method thereof

    CN116905114A

  • Hollow elastic fiber, fabric, spinneret plate and spinning assembly

    CN209619518U

  • Production of conjugate fiber

    JP2000144518A

  • Rayon-like polyester composite yarn having excellent drapability and high elasticity and manufacturing method thereof