Polyamide flame-retardant fiber and preparation process thereof
Through the combined use of modified hydrotalcite and reinforcing fillers, the problems of nylon fiber being flammable, poorly hygroscopic, airtight and prone to static electricity are solved, and its flame retardant, antistatic and breathable properties are significantly improved, forming a fiber with excellent comprehensive properties. Nylon flame retardant fiber.
Patent Information
- Application Number
- CN202410970412.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-19
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame-retardant fibers, and in particular to a nylon flame-retardant fiber and a preparation process thereof. Background Art
[0002] Nylon fiber has excellent physical properties and textile properties, excellent wear resistance, oil resistance, low temperature resistance, chemical resistance, high strength, impact resistance, easy to dye, so it is widely used to make various interior decoration fabrics, ribbons, bedding, sofas, tents and parachutes. However, due to its molecular structure characteristics, it is a flammable material, and it is easy to produce molten droplets when burning, which brings huge safety hazards to daily use. In addition, nylon fiber also has the disadvantages of poor hygroscopicity, airtightness, and easy static electricity.
[0003] In view of the shortcomings of nylon fiber, it can be modified to improve the performance of the fiber. For example, hydrotalcite with flame retardant properties can be added. However, to achieve the expected flame retardant effect, a large amount of hydrotalcite needs to be added. Therefore, the hydrotalcite needs to be processed, and a small amount of organic and inorganic flame retardants are combined to achieve a good flame retardant effect. Silica with a certain air permeability is added to improve the air permeability of the fiber, and the surface of silica is modified to improve the antistatic performance of the fiber. Therefore, through the above modifications, researchers can prepare a nylon fiber with excellent flame retardant properties, antistatic properties and air permeability. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a nylon flame retardant fiber and a preparation process thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions: A nylon flame-retardant fiber comprises the following raw materials in parts by weight: 100 parts of nylon 6 chips, 3-5 parts of modified hydrotalcite, 2-6 parts of reinforcing filler, 0.3-0.6 parts of antioxidant, and 0.2-0.5 parts of lubricant; The modified hydrotalcite is prepared by the following steps: Step A1, add methyl dichlorophosphate and acetonitrile into a flask and stir to mix evenly, raise the system temperature to 60-70°C, add sodium N,N-di(2-hydroxyethyl)-2-aminoethanesulfonate acetonitrile solution three times, each time with an interval of 10 minutes, then raise the temperature to 80-90°C again, reflux for 16-22 hours, and filter to obtain the N / P intercalant; Step A2, heat deionized water to boiling state, add Zn(NO3)2·6H2O, Al(NO3)3·9H2O and Mg(NO3)2·6H2O and stir for 30 minutes, then transfer the mixed solution to a beaker, maintain the system temperature at 70°C, adjust the system pH to 10.5-11.3, and continue stirring for 3-4 hours to obtain a hydrotalcite precursor, then add N / P intercalation agent to the hydrotalcite precursor and continue stirring for 3-5 hours. After the reaction is completed, centrifuge, wash and dry to obtain modified hydrotalcite; Further, in step A1, the dosage ratio of methyl dichlorophosphate, acetonitrile and sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate acetonitrile solution is 0.01-0.03 mol:100 mL:100 mL, and the sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate acetonitrile solution is prepared by mixing sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate and acetonitrile in a dosage ratio of 0.02-0.06 mol:100 mL; Furthermore, in step A2, the dosage ratio of deionized water, Zn(NO3)2·6H2O, Al(NO3)3·9H2O, Mg(NO3)2·6H2O and N / P intercalant is 100mL: 0.03-0.06mol: 0.03-0.04mol: 0.03-0.06mol: 0.03-0.06mol.
[0006] The reinforcing filler is prepared by the following steps: Step B1, add bis(2-(2-methoxyethoxy)ethyl)amine into a flask containing methanol, stir and mix evenly under nitrogen, then add 1-pentene dropwise while stirring, raise the temperature to 35°C after the addition is completed, react for 4-5 hours, and after the reaction is completed, rotary evaporate to obtain intermediate 1; Step B2, adding epichlorohydrin to methanol and mixing and stirring evenly, heating to 60-70° C. in an oil bath, slowly adding intermediate product 1 under stirring, continuing stirring for 4-6 hours, cooling to room temperature after the reaction is completed, distilling under reduced pressure, and washing to obtain intermediate product 2; Step B3, add the intermediate product 2 into a flask containing methanol and stir to mix evenly, raise the temperature to 45-55°C, slowly add γ-aminopropyltriethoxysilane, stir and react under nitrogen for 8-12h, after the reaction is completed, distill under reduced pressure, wash and dry to obtain a product containing ether bond function; Step B4, dispersing nano-silicon dioxide in a mixture of ethanol and deionized water, ultrasonically dispersing for 30 minutes, adding the functional product, and heating to 60-70° C. to react for 4-6 hours. After the reaction is completed, a reinforced filler is obtained; Further, in step B1, the ratio of bis(2-(2-methoxyethoxy)ethyl)amine, methanol and 1-pentene is 0.01-0.03 mol:100 mL:0.01-0.03 mol; Further, in step B2, the usage ratio of epichlorohydrin, methanol and intermediate product 1 is 0.1-0.2 mol: 200 mL: 0.1-0.2 mol; Further, in step B3, the usage ratio of the intermediate product 2, methanol and γ-aminopropyltriethoxysilane is 0.1-0.2 mol: 100 mL: 0.1-0.2 mol; Furthermore, in step B4, the usage ratio of nano-silica, ethanol, deionized water and the product containing ether bond functionality is 1 g: 80 mL: 20 mL: 0.5-1 g.
[0007] A preparation process of nylon flame retardant fiber comprises the following steps: Weigh the raw materials by weight, add nylon 6 chips, modified hydrotalcite, reinforcing filler, antioxidant and lubricant into a high-speed mixer in sequence, mix and stir at a speed of 600-800 rpm for 10-15 minutes, then extrude and granulate through a twin-screw extruder, and then melt-spin the granules through an FDY high-speed spinning machine to obtain nylon flame-retardant fiber; Furthermore, the melt spinning process temperature is 220-230°C in zone 1, 230-240°C in zone 2, 230-245°C in zone 3, and 235-245°C in zone 4; the spinning speed is 4000-7000 m / min, and the draft ratio is 3-5 times.
[0008] Beneficial effects of the present invention:
[0009] The nylon fiber prepared by the present invention not only improves the flame retardancy of the nylon fiber, but also improves the antistatic property and air permeability by adding modified hydrotalcite and reinforcing filler, wherein the zinc doped in the modified hydrotalcite plays an anti-melting droplet role during combustion, and at the same time, the interlayers of the hydrotalcite are intercalated and modified, thereby further improving the flame retardancy of the matrix; the reinforcing filler is based on silicon dioxide, and the surface of the silicon dioxide is modified by a silane coupling agent, thereby improving the flame retardancy, antistatic property and air permeability of the matrix.
[0010] In the modified hydrotalcite, the chlorine atoms in methyl dichlorophosphate are first reacted with the hydroxyl groups in sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate to obtain an N / P intercalant; then, Zn(NO3)2·6H2O, Al(NO3)3·9H2O and Mg(NO3)2·6H2O are used as zinc source, aluminum source and magnesium source respectively to prepare a hydrotalcite precursor, and then the negatively charged sulfonate ions in the N / P intercalant are used to perform intercalation modification through adsorption and exchange to obtain the modified hydrotalcite. The addition of modified hydrotalcite improves the flame retardant properties of the matrix. This is because when hydrotalcite is decomposed by heat, a large amount of water and carbon dioxide are released, which can dilute and block the combustible gas. At the same time, the magnesium-aluminum oxides produced by thermal decomposition and the carbonized products produced when the polymer is burned can form a protective layer on the surface of the matrix, further blocking the invasion of oxygen to achieve the effect of gas-phase-solid phase flame retardancy; zinc elements form zinc compounds when the matrix is burned, and the zinc compounds can react with the amino groups produced when the polymer molecules are decomposed by heat to promote the cross-linking of the decomposed matrix into carbon, so that the matrix condenses around the zinc compounds, avoiding the polymer transfer caused by combustion. It plays an anti-melting droplet role; the introduction of N / P intercalant further improves the flame retardant properties of hydrotalcite. This is because phosphate and N source are introduced into the intercalant. Phosphate decomposes into phosphorus-containing free radicals such as P·, PO· and PO2· when burned and acts as a free radical scavenger to capture active free radicals H· and OH· in the gas phase, achieve free radical quenching, dilute the concentration of combustibles in the gas phase, interrupt the free radical chain reaction of combustion, and can generate oxygen-containing phosphoric acid, which promotes the formation of a dense carbon layer in the matrix, thereby improving the flame retardant properties of the matrix. In addition, NH3, N2 and NO generated by the thermal decomposition of the N source x Inert gases such as argon and argon can dilute the concentration of flammable and combustion-supporting gases in the air and cover the surface of the substrate to isolate it from the air.
[0011] In the reinforcing filler, a tertiary amine structure is first introduced by reacting the secondary amine in bis(2-(2-methoxyethoxy)ethyl)amine with the double bond in 1-pentene to obtain an intermediate product 1 containing an ether bond; then, the chlorine atom in epichlorohydrin is reacted with the tertiary amine in the intermediate product 1 to generate an intermediate product 2 containing an epoxy group and a quaternary ammonium salt structure; then, the epoxy group in the intermediate product 2 is reacted with the amino group in the silane coupling agent to generate an ether bond functional product; finally, the silanol bond generated by the hydrolysis of the ether bond functional product is condensed with the hydroxyl group on the surface of silica to obtain a reinforcing filler. The addition of reinforcing fillers further improves the comprehensive performance of the fiber; among them, silica is added to the fiber as a base of reinforcing fillers, which can widen the intervals between the fibers, thereby improving the air permeability of the fiber products. At the same time, silica also has a certain flame retardancy when the matrix burns; the introduction of hydrophilic ether bonds can enhance the hygroscopicity of the matrix, easily attract water molecules in the air, thereby improving the ability of the matrix to adsorb water molecules in the surrounding environment, forming a layer of water film on the surface of the matrix, accelerating the dissipation rate of surface electrostatic charge, and improving the antistatic performance of the matrix. DETAILED DESCRIPTION
[0012] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0013] The modified hydrotalcite is prepared by the following steps: Step A1, 0.01 mol of methyl dichlorophosphate and 100 mL of acetonitrile were added into a flask and stirred to mix evenly, the system temperature was raised to 60° C., 100 mL of sodium N, N-bis(2-hydroxyethyl)-2-aminoethanesulfonate acetonitrile solution was added three times, each time with an interval of 10 minutes, and then the temperature was raised to 80° C. again, and after reflux for 16 hours, the mixture was filtered to obtain an N / P intercalant. The sodium N, N-bis(2-hydroxyethyl)-2-aminoethanesulfonate acetonitrile solution was prepared by mixing sodium N, N-bis(2-hydroxyethyl)-2-aminoethanesulfonate and acetonitrile in a dosage ratio of 0.02 mol:100 mL; Step A2, heat 100 mL of deionized water to boiling, add 0.03 mol Zn(NO3)2·6H2O, 0.03 mol Al(NO3)3·9H2O and 0.03 mol Mg(NO3)2·6H2O and stir for 30 min, then transfer the mixed solution to a beaker, maintain the system temperature at 70°C, adjust the system pH to 10.5, and continue stirring for 3 h to obtain a hydrotalcite precursor, then add 0.03 mol N / P intercalant to the hydrotalcite precursor and continue stirring for 3 h. After the reaction is completed, centrifuge, wash and dry to obtain modified hydrotalcite.
[0014] The reinforcing filler is prepared by the following steps: Step B1, add 0.01 mol of bis(2-(2-methoxyethoxy)ethyl)amine into a flask containing 100 mL of methanol, stir and mix evenly under nitrogen, then dropwise add 0.01 mol of 1-pentene while stirring, raise the temperature to 35°C after the addition is completed, react for 4 hours, and after the reaction is completed, rotary evaporate to obtain intermediate 1; Step B2, add 0.1 mol of epichlorohydrin to 200 mL of methanol and mix and stir evenly, heat to 60° C. under oil bath conditions, slowly add 0.1 mol of intermediate 1 under stirring conditions, continue stirring for 4 h, cool to room temperature after the reaction is completed, distill under reduced pressure, and wash to obtain intermediate 2; Step B3, add 0.1 mol of intermediate product 2 into a flask containing 100 mL of methanol, stir and mix evenly, raise the temperature to 45° C., slowly add 0.1 mol of γ-aminopropyltriethoxysilane, stir and react under nitrogen for 8 hours, and after the reaction is completed, distill under reduced pressure, wash and dry to obtain a product containing an ether bond function; Step B4, disperse 1g of nano-silica in a mixture of 80mL of ethanol and 20mL of deionized water, ultrasonically disperse for 30min, add 0.5g of a product containing an ether bond function, and heat to 60°C for reaction for 4h. After the reaction is completed, a reinforced filler is obtained. Example 2
[0015] The modified hydrotalcite is prepared by the following steps: Step A1, 0.02 mol of methyl dichlorophosphate and 100 mL of acetonitrile were added to a flask and stirred to mix evenly, the system temperature was raised to 65° C., 100 mL of sodium N, N-bis(2-hydroxyethyl)-2-aminoethanesulfonate acetonitrile solution was added three times, each time with an interval of 10 minutes, and then the temperature was raised to 85° C. again, and after reflux for 19 hours, the mixture was filtered to obtain an N / P intercalant. The sodium N, N-bis(2-hydroxyethyl)-2-aminoethanesulfonate acetonitrile solution was prepared by mixing and stirring sodium N, N-bis(2-hydroxyethyl)-2-aminoethanesulfonate and acetonitrile in a dosage ratio of 0.04 mol:100 mL; Step A2, heat 100 mL of deionized water to boiling, add 0.045 mol Zn(NO3)2·6H2O, 0.035 mol Al(NO3)3·9H2O and 0.045 mol Mg(NO3)2·6H2O and stir for 30 min, then transfer the mixed solution to a beaker, maintain the system temperature at 70°C, adjust the system pH to 11, and continue stirring for 3.5 h to obtain a hydrotalcite precursor, then add 0.045 mol N / P intercalant to the hydrotalcite precursor and continue stirring for 4 h. After the reaction is completed, centrifuge, wash and dry to obtain modified hydrotalcite.
[0016] The reinforcing filler is prepared by the following steps: Step B1, add 0.02 mol of bis(2-(2-methoxyethoxy)ethyl)amine into a flask containing 100 mL of methanol, stir and mix evenly under nitrogen, then dropwise add 0.02 mol of 1-pentene while stirring, raise the temperature to 35°C after the addition is completed, react for 4.5 hours, and after the reaction is completed, rotary evaporate to obtain intermediate 1; Step B2, add 0.15 mol of epichlorohydrin to 200 mL of methanol and mix and stir evenly, heat to 65° C. under oil bath conditions, slowly add 0.15 mol of intermediate product 1 under stirring conditions, continue stirring for 5 h, cool to room temperature after the reaction is completed, distill under reduced pressure, and wash to obtain intermediate product 2; Step B3, add 0.15 mol of intermediate product 2 into a flask containing 100 mL of methanol, stir and mix evenly, raise the temperature to 50° C., slowly add 0.15 mol of γ-aminopropyltriethoxysilane, stir and react under nitrogen for 10 h, and after the reaction is completed, distill under reduced pressure, wash and dry to obtain a product containing an ether bond function; Step B4, disperse 1g of nano-silica in a mixture of 80mL of ethanol and 20mL of deionized water, ultrasonically disperse for 30min, add 0.75g of a product containing an ether bond function, and heat to 65°C to react for 5h. After the reaction is completed, a reinforced filler is obtained. Example 3
[0017] The modified hydrotalcite is prepared by the following steps: Step A1, 0.03 mol of methyl dichlorophosphate and 100 mL of acetonitrile were added to a flask and stirred to mix evenly, the system temperature was raised to 70° C., 100 mL of sodium N, N-bis(2-hydroxyethyl)-2-aminoethanesulfonate acetonitrile solution was added three times, each time with an interval of 10 minutes, and then the temperature was raised to 90° C. again, and after reflux for 22 hours, the mixture was filtered to obtain an N / P intercalant. The sodium N, N-bis(2-hydroxyethyl)-2-aminoethanesulfonate acetonitrile solution was prepared by mixing sodium N, N-bis(2-hydroxyethyl)-2-aminoethanesulfonate and acetonitrile in a dosage ratio of 0.06 mol:100 mL; Step A2, heat 100 mL of deionized water to boiling, add 0.06 mol Zn(NO3)2·6H2O, 0.04 mol Al(NO3)3·9H2O and 0.06 mol Mg(NO3)2·6H2O and stir for 30 min, then transfer the mixed solution to a beaker, maintain the system temperature at 70°C, adjust the system pH to 11.3, and continue stirring for 4 h to obtain a hydrotalcite precursor, then add 0.06 mol N / P intercalant to the hydrotalcite precursor and continue stirring for 5 h. After the reaction is completed, centrifuge, wash and dry to obtain modified hydrotalcite.
[0018] The reinforcing filler is prepared by the following steps: Step B1, add 0.03 mol of bis(2-(2-methoxyethoxy)ethyl)amine into a flask containing 100 mL of methanol, stir and mix evenly under nitrogen, then dropwise add 0.03 mol of 1-pentene while stirring, raise the temperature to 35°C after the addition is completed, react for 5 hours, and after the reaction is completed, rotary evaporate to obtain intermediate 1; Step B2, add 0.2 mol of epichlorohydrin to 200 mL of methanol and mix and stir evenly, heat to 70° C. under oil bath conditions, slowly add 0.2 mol of intermediate product 1 under stirring conditions, continue stirring for 6 hours, cool to room temperature after the reaction is completed, distill under reduced pressure, and wash to obtain intermediate product 2; Step B3, add 0.2 mol of intermediate product 2 into a flask containing 100 mL of methanol, stir and mix evenly, raise the temperature to 55° C., slowly add 0.2 mol of γ-aminopropyltriethoxysilane, stir and react under nitrogen for 12 h, and after the reaction is completed, distill under reduced pressure, wash and dry to obtain a product containing an ether bond function; Step B4, disperse 1g of nano-silica in a mixture of 80mL of ethanol and 20mL of deionized water, and disperse by ultrasonic for 30min, then add 1g of the product containing ether bond function, and heat to 70°C for reaction for 6h. After the reaction is completed, the reinforced filler is obtained. Example 4
[0019] A preparation process of nylon flame retardant fiber comprises the following steps: 100 parts of nylon 6 slices, 3 parts of modified hydrotalcite prepared in Example 1, 2 parts of reinforcing filler prepared in Example 1, 0.3 parts of thiodipropionic acid diester, and 0.2 parts of alkyl diphenyl ether oil; The raw materials were weighed by weight, and nylon 6 slices, modified hydrotalcite prepared in Example 1, reinforcing filler prepared in Example 1, thiodipropionate diester and alkyl diphenyl ether oil were added into a high-speed mixer in sequence, mixed and stirred at a speed of 600 rpm for 10 minutes, and then extruded into granules through a twin-screw extruder, and then the granules were melt-spun through an FDY high-speed spinning machine to obtain nylon flame-retardant fiber. The melt spinning process temperature was 220°C in zone 1, 230°C in zone 2, 230°C in zone 3, and 235°C in zone 4; the spinning speed was 4000 m / min, and the draft ratio was 3 times. Example 5
[0020] A preparation process of nylon flame retardant fiber comprises the following steps: 100 parts of nylon 6 slices, 4 parts of modified hydrotalcite prepared in Example 2, 4 parts of reinforcing filler prepared in Example 2, 0.5 parts of thiodipropionic acid diester, and 0.3 parts of alkyl diphenyl ether oil; The raw materials were weighed by weight, and nylon 6 slices, modified hydrotalcite prepared in Example 2, reinforcing filler prepared in Example 2, thiodipropionic acid diester and alkyl diphenyl ether oil were added into a high-speed mixer in sequence, mixed and stirred at a speed of 700 rpm for 12 minutes, and then extruded into granules through a twin-screw extruder, and then the granules were melt-spun through an FDY high-speed spinning machine to obtain nylon flame-retardant fiber. The melt spinning process temperature was 225°C in zone 1, 235°C in zone 2, 240°C in zone 3, and 240°C in zone 4. The spinning speed was 5000 m / min, and the draft ratio was 4 times. Example 6
[0021] A preparation process of nylon flame retardant fiber comprises the following steps: 100 parts of nylon 6 slices, 5 parts of modified hydrotalcite prepared in Example 3, 6 parts of reinforcing filler prepared in Example 3, 0.6 parts of thiodipropionic acid diester, and 0.5 parts of alkyl diphenyl ether oil; The raw materials were weighed by weight, and nylon 6 chips, modified hydrotalcite prepared in Example 3, reinforcing filler prepared in Example 3, thiodipropionic acid diester and alkyl diphenyl ether oil were added into a high-speed mixer in sequence, mixed and stirred at a speed of 800 rpm for 15 minutes, and then extruded into granules through a twin-screw extruder, and then the granules were melt-spun through an FDY high-speed spinning machine to obtain nylon flame-retardant fiber. The melt spinning process temperature was 230°C in zone 1, 240°C in zone 2, 245°C in zone 3, and 245°C in zone 4. The spinning speed was 7000 m / min, and the draft ratio was 5 times.
[0022] Comparative Example 1 This comparative example is a nylon fiber, which is different from Example 6 in that an equal amount of hydrotalcite is used to replace the modified hydrotalcite prepared in Example 3, and the rest are the same.
[0023] Comparative Example 2 This comparative example is a nylon fiber, which differs from Example 6 in that an equal amount of silicon dioxide is used to replace the reinforcing filler prepared in Example 3, and the rest are the same.
[0024] The performance tests were performed on the nylon fibers prepared in Examples 4-6 and Comparative Examples 1-2: Flame retardant performance test: in accordance with GB / T5455-2014 Textile combustion performance - Determination of vertical damage length, smoldering and after-flaming time; Antistatic performance test: Under the conditions of temperature 25°C and relative humidity 60%, a high resistance meter MCP-HT450 was used to apply a voltage of 250V to measure the initial surface resistivity of each embodiment and comparative example; Air permeability: The test method is GBT5453-1997 air permeability test of textiles; The test results are shown in the following table: Limiting oxygen index (%) Afterburning time (s) Melt drop situation Surface resistivity (Ω) Air permeability (mm / s) Example 4 28.5 0 No droplets <![CDATA[9.6×10 7 ]]> 48.5 Example 5 29.7 0 No droplets <![CDATA[8.9×10 7 ]]> 54.8 Example 6 32.8 0 No droplets <![CDATA[7.6×10 7 ]]> 60.1 Comparative Example 1 23.5 5 There are molten droplets <![CDATA[2.5×10 8 ]]> 47.6 Comparative Example 2 27.6 2 No droplets <![CDATA[9.7×10 9 ]]> 36.4
[0025] It can be seen from the above table that the nylon fiber prepared by the present invention has excellent flame retardancy, antistatic properties and air permeability, and can be widely used in the manufacture of textiles such as clothing, bedding, curtains, etc.
[0026] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A nylon flame retardant fiber, It is characterized in that The method comprises the following raw materials in parts by weight: 100 parts of nylon 6 chips, 3-5 parts of modified hydrotalcite, 2-6 parts of reinforcing filler, 0.3-0.6 parts of antioxidant, and 0.2-0.5 parts of lubricant; The modified hydrotalcite is prepared by the following steps: Step A1, add methyl dichlorophosphate and acetonitrile into a flask and stir to mix evenly, raise the system temperature to 60-70°C, add sodium N,N-di(2-hydroxyethyl)-2-aminoethanesulfonate acetonitrile solution three times, each time with an interval of 10 minutes, then raise the temperature to 80-90°C again, reflux for 16-22 hours, and filter to obtain the N / P intercalant; Step A2: Heat deionized water to a boil and add Zn(NO 3 ) 2 6H 2 O、Al(NO 3 ) 3 9H 2 O and Mg(NO 3 ) 2 6H 2 O and stirred for 30 minutes, then the mixed solution was transferred to a beaker, and the system temperature was maintained at 70°C, the system pH was adjusted to 10.5-11.3, and stirring was continued for 3-4 hours to obtain a hydrotalcite precursor, and then N / P intercalation agent was added to the hydrotalcite precursor and stirring was continued for 3-5 hours. After the reaction was completed, centrifugation, washing and drying were performed to obtain the modified hydrotalcite.
2. The nylon flame retardant fiber according to claim 1, It is characterized in that In step A1, the amount ratio of methyl dichlorophosphate, acetonitrile and sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate acetonitrile solution is 0.01-0.03 mol:100 mL:100 mL, and the sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate acetonitrile solution is prepared by mixing sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate and acetonitrile in an amount ratio of 0.02-0.06 mol:100 mL.
3. The nylon flame retardant fiber according to claim 1, It is characterized in that In step A2, deionized water, Zn(NO 3 ) 2 6H 2 O、Al(NO 3 ) 3 9H 2 O、Mg(NO 3 ) 2 6H 2 The dosage ratio of O and N / P intercalants is 100mL: 0.03-0.06mol: 0.03-0.04mol: 0.03-0.06mol: 0.03-0.06mol.
4. The nylon flame retardant fiber according to claim 1, It is characterized in that The reinforcing filler is prepared by the following steps: Step B1, add bis(2-(2-methoxyethoxy)ethyl)amine into a flask containing methanol, stir and mix evenly under nitrogen, then add 1-pentene dropwise while stirring, raise the temperature to 35°C after the addition is completed, react for 4-5 hours, and after the reaction is completed, rotary evaporate to obtain intermediate 1; Step B2, adding epichlorohydrin to methanol and mixing and stirring evenly, heating to 60-70° C. in an oil bath, slowly adding intermediate product 1 under stirring, continuing stirring for 4-6 hours, cooling to room temperature after the reaction is completed, distilling under reduced pressure, and washing to obtain intermediate product 2; Step B3, add the intermediate product 2 into a flask containing methanol and stir to mix evenly, raise the temperature to 45-55°C, slowly add γ-aminopropyltriethoxysilane, stir and react under nitrogen for 8-12h, after the reaction is completed, distill under reduced pressure, wash and dry to obtain a product containing ether bond function; Step B4, disperse nano-silicon dioxide in a mixture of ethanol and deionized water, perform ultrasonic dispersion for 30 minutes, add the functional product, and heat to 60-70° C. to react for 4-6 hours. After the reaction is completed, the reinforced filler is obtained.
5. The nylon flame retardant fiber according to claim 4, It is characterized in that In step B1, the usage ratio of bis(2-(2-methoxyethoxy)ethyl)amine, methanol and 1-pentene is 0.01-0.03 mol:100 mL:0.01-0.03 mol.
6. The nylon flame retardant fiber according to claim 4, It is characterized in that In step B2, the usage ratio of epichlorohydrin, methanol and intermediate product 1 is 0.1-0.2 mol: 200 mL: 0.1-0.2 mol.
7. The nylon flame retardant fiber according to claim 4, It is characterized in that In step B3, the usage ratio of the intermediate product 2, methanol and γ-aminopropyltriethoxysilane is 0.1-0.2 mol:100 mL:0.1-0.2 mol.
8. The nylon flame retardant fiber according to claim 4, It is characterized in that In step B4, the usage ratio of nano-silicon dioxide, ethanol, deionized water and the product containing ether bond function is 1g:80mL:20mL:0.5-1g.
9. The process for preparing a nylon flame retardant fiber according to claim 1, It is characterized in that The following steps are involved: The raw materials are weighed by weight, and nylon 6 chips, modified hydrotalcite, reinforcing filler, antioxidant and lubricant are added into a high-speed mixer in sequence, mixed and stirred at a speed of 600-800 rpm for 10-15 minutes, and then extruded into granules through a twin-screw extruder, and then the granules are melt-spun through an FDY high-speed spinning machine to obtain nylon flame-retardant fiber.
10. A process for preparing a nylon flame retardant fiber according to claim 9, It is characterized in that The melt spinning process temperature is 220-230°C in zone 1, 230-240°C in zone 2, 230-245°C in zone 3, and 235-245°C in zone 4. The spinning speed is 4000-7000m / min, and the draft ratio is 3-5 times.
Citation Information
Patent Citations
Synthesis of compound containing phosphorus, nitrogen and sulphur and preparation method of intercalation modified hydrotalcite by virtue of compound
CN106893369A
Smokeless flame-retardant waterproof cable material
CN113896988A
Flame-retardant foamed styrene resin composition
US20150344658A1
Easily dispersible hydrotalcite-based composite material for polymer, and preparation method therefor
WO2024108383A1
Cited By
Flame-retardant antistatic nylon fiber with skin-core structure and preparation method of flame-retardant antistatic nylon fiber
CN121951739A