Application of MOFs modified nitrogen-phosphorus-silicon flame retardant to cotton fabric

By using MOFs modified nitrogen-phosphorus silicon flame retardant in textiles, combined with hydroxyl and carboxyl functional groups and silicone, the problem of easy shedding and poor water resistance of textile flame retardants is solved, and efficient flame retardant performance and water resistance are achieved, significantly Improves the flame retardant properties and heat resistance of cotton fabrics.

CN118756497APending Publication Date: 2024-10-11YANTAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410756223.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-08-07
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing textile flame retardant technology has problems such as easy shedding of flame retardants, carbonization of materials due to strong acidity, poor water resistance, and reduced flame retardant properties. It is especially difficult to maintain long-term flame retardant effects in cotton fabric applications.

Method used

Using MOFs modified nitrogen-phosphorus silicon flame retardant, hydroxyl and carboxyl functional groups are introduced during the synthesis process, combined with silicone and reinforcing materials to form a flame retardant with good water resistance, and the flame retardant properties of cotton fabrics are improved through specific processing. .

Benefits of technology

Significantly improves the flame retardant properties and water resistance of cotton fabrics, extends the durability of flame retardants, reduces smoke release and burning time, and enhances the material's heat resistance and smoke suppression properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004889534200000141
    Figure BDA0004889534200000141
  • Figure BDA0004889534200000142
    Figure BDA0004889534200000142
  • Figure BDA0004889534200000151
    Figure BDA0004889534200000151
Patent Text Reader

Abstract

The invention relates to preparation of a MOFs modified nitrogen-phosphorus-silicon flame retardant and application in cotton fabrics, tris (2-ethoxyl) isocyanurate, maleic anhydride, tetrakis hydroxymethyl phosphonium sulfate and the like are used for synthesizing the nitrogen-phosphorus-silicon flame retardant, the nitrogen-phosphorus-silicon flame retardant is combined with MOFs substances and is used for an after-finishing process of the cotton fabrics, and after the flame retardant is added, the oxygen index of the obtained cotton is greatly improved, and the flame retardant has a good flame retardant effect on the cotton fabrics. Compared with a traditional cotton fabric flame retardant CP in the market, the flame retardant has the advantage that the washing resistance and flame retardance are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention is a divisional application of 2023109846823. Technical Field

[0002] The invention relates to the preparation of MOFs modified nitrogen-phosphorus-silicon flame retardant, and in particular relates to the preparation of MOFs modified nitrogen-phosphorus-silicon flame retardant and its application in cotton fabrics. Background Art

[0003] Textiles include industrial textiles, medical and sanitary textiles, geotechnical and architectural textiles, safety and protection textiles, filtration and separation textiles, non-woven fabrics, rope and net products, papermaking textiles, military textiles, etc. They are widely used in clothing, home furnishing, medical and health, electronic information intelligence, construction, energy and other fields, and occupy a large market in the world. my country has the most complete textile industry system in the world, and the textile industry is also an important part of my country's national economy. In 2021, with the effective prevention and control of the new coronavirus vaccine and the epidemic, the global economy has recovered. my country's textile industry has worked hard to overcome the difficulties of repeated epidemics, rising raw material prices, and poor international transportation capacity, and the economic operation situation has improved. According to an article published by the China National Textile and Apparel Council, in 2021, the added value of my country's textile industry above designated size increased by 4.4% year-on-year, and the average growth rate from 2020 to 2021 was 0.8%, of which the textile industry increased by 1.0% in two years and the chemical fiber industry increased by 4.7% in two years. The retail sales of clothing, shoes and hats, and needle textiles above the limit amounted to 1,384.2 billion yuan, a year-on-year increase of 12.7%. However, as the economy returns to normal development, the safety hazards caused by textiles still exist. In March 2022, a fire broke out at Sichuan Jinglun Textile Co., Ltd., injuring 4 people and causing 1 missing. From the video of the fire, black smoke billowed at the scene. In November 2021, a factory building in Wuzhou Sihai Textile Finishing Industrial Park, Anchang Street, Shaoxing, caught fire, and the fire was serious. In September of the same year, a textile factory in Wannian County, Shangrao, Jiangxi Province caught fire, and the fire area was about 15,000 square meters. In January 2019, three warehouses where textile products were stacked at Wujin Chengnan Textile Factory in Changzhou caught fire, with thick smoke billowing and the roofs almost completely burned. In January 2017, the temperature of the machine in the workshop of a cotton factory in Rudong, Jiangsu was too high, igniting cotton yarn, causing the cotton strips stored in the entire workshop to catch fire. The fire was swift and the flames rose to seal the door. After two consecutive rounds of firefighters rescued, it was extinguished. Textile factory fires have emerged one after another for several years, posing a great threat to the safety of people and property.

[0004] Currently, there are two methods for flame retardant treatment of fabrics. One is to introduce monomers with flame retardant effect or use flame retardant treated fibers during the material synthesis process, so that the synthesized fabric also has flame retardant effect.

[0005] Shariatinia Z et al. used ultrasonic radiation to synthesize 5 new nano-phosphoramide compounds, which were tie-dyed on cotton fibers to make flame-retardant fabrics. Tests show that phosphoramide promotes the dehydration of substances into carbon, so that the mass loss of cotton fibers at 800°C is only 43.52%, giving them good flame retardant and antibacterial properties. In addition, the study found that when the fibers are flame-retarded, the flame-retardant components with unsaturated CC bonds can form CO covalent bonds with -OH on the fibers, thereby grafting onto cotton fabrics to obtain excellent and stable flame retardant properties, and the fabric can still maintain its original fiber structure after burning. However, flame-retardant components that do not contain unsaturated bonds cannot polymerize or graft with fibers, but can only be dispersed between fibers and produce electrostatic interactions with the functional groups of the fibers. Therefore, the flame retardant effect is limited, and the fibers of the treated fabrics break during the burning process.

[0006] The method of preparing flame-retardant fibers first and then spinning them into fabrics has a simple production process, a high utilization rate of flame retardants, and low toxicity. The flame retardant component is combined with the fiber, so that the component is not easily lost and has good water resistance. However, when the fiber is flame-retarded, the flame retardant needs to be screened, which limits the application of this method.

[0007] Another method is to use a flame retardant to treat the fabric after it is prepared so that it has certain flame retardant properties. Wang SH et al. synthesized an environmentally friendly nitrogen-phosphorus flame retardant 6-chloro-1,3,5-triazine-p-aminobenzenesulfonic acid-2-methylphosphonic acid dimethyl ester (CTSGP) and used it for flame retardant treatment of cotton fabrics. Tests found that when the weight of the cotton fabric increased by 21.4% after treatment, the LOI value increased to 29.0% (the LOI value of the untreated cotton fabric was 18.0%), and the residual carbon length was 6.2 cm. The nitrogen gas and organic phosphorus carbon layer produced during combustion help improve the flame retardant properties of cotton fabrics;

[0008] In the early stage, our team used pentaerythritol as carbon source and phosphoric acid as acid source to prepare pentaerythritol phosphate, added phosphorus pentachloride (PCl5) and ethanolamine, synthesized nitrogen-phosphorus flame retardant, and used nitrogen-phosphorus flame retardant for flame retardant treatment of cotton fabrics. Two different methods for preparing flame retardant finishing liquid were designed. By testing the flame retardant properties of treated cotton, the best finishing liquid formula was determined as follows: dissolve the flame retardant in distilled water and adjust the pH to 6.0-6.5 with a 10% mass concentration of NaOH solution. When the amount of flame retardant added was 100g / L, when the cotton burned, the fire source was removed and the sample was extinguished quickly, there was no smoke, no afterburning time, the smoldering time was short, the damaged length was 6.8cm, and the LOI was 32.0%, which was 77.8% higher than that of untreated cotton. After 50 washings, the LOI value was still higher than that of untreated cotton. Compared with the commercially available CP flame retardant of the same concentration, its LOI value increased by 14.0%, from all damage to only 6.8cm damage.

[0009] This method is low-cost and simple to operate, but there are also three situations: first, the flame retardant is applied to the structural gap of the material; second, the flame retardant can be combined with the substrate by chemical bonds; third, the acidity of the flame retardant system is too high, which can easily carbonize cotton fabrics, especially when the cotton fabrics are treated for washability, which is especially manifested as a decrease in the mechanical properties of cotton fabrics. For the former, during the subsequent washing and other processes of the treated material, the flame retardant components fall off from the inside of the material due to external factors, resulting in a decrease in the flame retardant properties of the material compared to when it was just treated. The middle one is a reactive treatment, which connects the material to be treated with the flame retardant component by chemical bonds, so the component is not easy to lose and the flame retardant effect is relatively stable, for the latter. At present, synthetic flame retardants are used to flame retardant fabrics, which is the most commonly used flame retardant method.

[0010] In view of the above-mentioned defects, the present invention relates to a nitrogen-phosphorus-silicon synergistic flame retardant, which does not use or produce a large amount of medium-strong acids such as phosphoric acid or hydrochloric acid during the synthesis process, does not produce toxic formaldehyde, will not carbonize cotton fabrics, improves its flame retardant oxygen index, and reduces the flaming combustion time and the flameless combustion time.

[0011] Metal organic framework materials (MOFs for short) are a type of porous materials with a network skeleton structure formed by metal ions and organic ligands connected by coordination bonds. They have a large specific surface area and good thermal stability, which has attracted the attention of researchers. In recent years, with the efforts of many researchers, many new MOFs have been prepared and great progress has been made. MOFs are currently widely used in hydrogen storage, separation, catalysis, flame retardancy and adsorption.

[0012] As an organic-inorganic hybrid material, MOFs' organic ligands can improve the compatibility between flame retardants and substrates, and can make polymers have better mechanical properties. Organic ligands can provide flame retardant elements or flame retardant groups to improve flame retardant efficiency. Compared with organic flame retardants, MOFs also have a large number of unsaturated metal sites, which can be used as active sites for catalyzing carbonization during combustion and promote carbonization reactions during combustion. As a porous material, MOFs has the characteristics of large specific surface area, many internal pores, and strong adsorption capacity. It can adsorb smoke cores, smoke particles, and toxic and harmful gases produced by materials during combustion, and can greatly improve the smoke suppression performance of polymers. However, MOFs are currently used in epoxy resins, butylene terephthalate / polypropylene composites, polylactic acid, thermoplastic polyurethane, polystyrene, etc., but not in textiles.

[0013] Aiming at the advantages of MOFs, the present invention utilizes its advantages of catalytic carbonization and strong adsorption capacity to improve the flame retardant properties of cotton fabrics. Summary of the invention

[0014] The present invention relies on the Shandong Province Small and Medium Enterprises Promotion Project "Research and Industrialization of Low Smoke, Melt-Drop Resistant Nitrogen-Phosphorus-Silicon Environmentally Friendly Flame Retardants 2022TSGC2552", and aims at the preparation of MOFs-modified nitrogen-phosphorus-silicon flame retardants and their application in cotton fabrics. The flame retardant does not use or produce a large amount of medium-strong acids such as phosphoric acid or hydrochloric acid during the synthesis process, nor does it produce toxic formaldehyde, and will not carbonize cotton fabrics at room temperature. The obtained cotton fabric has improved carbonization properties when heated and reduced smoke release, thereby increasing its flame retardant oxygen index and reducing the flaming combustion time and the flameless combustion time.

[0015] The preparation of MOFs modified nitrogen-phosphorus-silicon flame retardant and its application in cotton fabrics are characterized in that the preparation includes the preparation of MOFs modified nitrogen-phosphorus-silicon flame retardant and the use of MOFs modified nitrogen-phosphorus-silicon flame retardant for flame retardant treatment of cotton fabrics, wherein the preparation of MOFs modified nitrogen-phosphorus-silicon flame retardant includes the following process:

[0016] (1) Add 16-20 g of distilled water to 26 g of tris(2-hydroxyethyl)isocyanurate and 9.8-11.2 g of maleic anhydride, stir and react at 55-75° C. for 1-3 h, then add 0.3-0.4 g of initiator, stir and react at 75-85° C. for 2-3 h to obtain a polymer of isocyanurate and maleic anhydride;

[0017] (2) Add 3.5-4.2 g of tetrakis(hydroxymethyl)phosphonium sulfate and 1-2 g of tris(hydroxymethyl)aminomethane to the system of step (1), adjust the pH to 7-8, stir and react at 60-90° C. for 1-2 h, add 3.2-4.1 g of organosilicon, stir and react at 50-70° C. for 1-2 h, then add 1.2-2.5 g of reinforcing material A, stir and react at 90° C. for 1-2 h, then add 1.6-2.4 g of sodium dialdehyde carboxymethyl cellulose, stir and react at 60-70° C. for 30-40 min, to obtain the nitrogen-phosphorus-silicon flame retardant;

[0018] (3) Weigh 21 g of aminoacetic acid and 35 g of 1,4-dioxane, stir and mix, adjust the pH to 8 with 30% by mass sodium hydroxide, remove water by distillation under reduced pressure, add 16.6-29.8 g of cyanuric chloride to the system three times, each time with an interval of 15 minutes, heat the reaction system to 110° C. to reflux the reaction system, and react at this temperature for 3-5 hours, cool naturally to room temperature, acidify the solution to pH=3 with 15% by mass dilute hydrochloric acid, maintain stirring for 30-60 minutes, centrifuge the mixed solution, wash with 60 mL of water, 30 mL of 95% alcohol and 40 mL of anhydrous methanol, respectively, and vacuum dry to obtain cyanuric chloride flame retardant;

[0019] (4) 15 g of the product obtained in step (3) was dissolved in 75.00 mL of a mixed solution consisting of N,N-dimethylacetamide and methanol in a volume ratio of 4:1, 7.5-11.6 g of chromium chloride and 10 drops of ammonia were added thereto, the mixed solution was stirred for about 10 min until there were no solid particles in the system, the mixed system was transferred to a polytetrafluoroethylene-lined reactor, reacted at 120° C. for 24-36 h, and the MOFs product was obtained by programmed cooling.

[0020] (5) Add 2.1 g of the MOFs product obtained in step (4) to step (2), and react at 70-80° C. for 1-2 h to obtain a MOFs-modified nitrogen-phosphorus-silicon flame retardant.

[0021] The initiator is any one of ammonium persulfate and potassium persulfate;

[0022] The organosilicon is any one of γ-aminopropyltriethoxysilane and double-terminal alcohol hydroxy silicone oil IOTA 2110 (Anhui IOTA Silicone Oil Co., Ltd.);

[0023] The reinforcing material A is prepared by dropping 15-18 g of phosphorus oxychloride into 11 g of phenol, controlling the reaction temperature at 30-40 ° C, protecting with nitrogen, adding for 20-50 min, stirring for 1-2 h, adjusting the pH to 7, adding 16-22 g of α, ω-dihydroxy polydimethylsiloxane to the system, stirring at 50-70 ° C for 30-40 min, and then adding 3.1-4.6 g of aluminum sulfate and 1.6-2.4 g of zirconium sulfate.

[0024] and 6.3-7.3 g of sodium ethylenediamine di-o-phenylacetate, react at 40-50° C. with stirring for 30-40 min, control the pH to neutral during the reaction, and after the reaction is completed, filter under reduced pressure and dry the product to obtain a light yellow product, which is the reinforcing material A;

[0025] The dialdehyde sodium carboxymethyl cellulose is prepared by accurately weighing 1.6 g of sodium carboxymethyl cellulose and placing it in a beaker containing 30 mL of deionized water, stirring and dissolving to obtain an aqueous solution of sodium carboxymethyl cellulose, adding 20 mL of a 0.2 g / L NaIO4 solution, adjusting the pH of the system to 4, reacting under stirring conditions at 50 to 60° C. in the dark for 1 to 2 hours, pouring the product after the reaction into 15 to 30 mL of anhydrous ethanol to filter the precipitate, collecting the filter cake, washing the filter cake alternately with deionized water and anhydrous ethanol, and drying the washed filter cake at 60 to 70° C. for 2 to 5 hours to obtain the dialdehyde sodium carboxymethyl cellulose;

[0026] The application process of cotton fabric is as follows: (a) Flame retardant pretreatment process of cotton fabric: cut the cotton fabric into several square cotton fabrics of 25 cm × 25 cm for use, pour the pretreatment liquid into a plastic beaker, place the cut fabric flatly under the liquid surface, soak for 1 to 3 hours, take out and wash, and dry at 60 to 90°C;

[0027] The preparation method of the pretreatment liquid is as follows: 90-95g of water, 0.5-1g of alkali, and 0.4-0.7g of Fit C surface treatment agent are added and stirred evenly to obtain the pretreatment liquid;

[0028] (b) Process of flame retardant treatment of cotton fabric: transfer the flame retardant finishing liquid to a conical flask, immerse the cotton fabric of step (a), place it in a water bath constant temperature oscillator and oscillate for 20 to 40 minutes at a temperature of 60 to 90° C. and a rotation speed of 30 to 60 rpm. After the oscillation is completed, take out the fabric, squeeze out the water, and the squeezing rate is 70%. Dry it in an electric constant temperature blast drying oven at 60 to 90° C., repeat the above operation 2 to 5 times, and bake the cotton fabric after the third drying at 103 to 110° C. for 4 to 7 minutes and take it out.

[0029] The preparation method of the flame retardant finishing liquid is as follows: 8-10g of the MOFs-modified nitrogen-phosphorus-silicon flame retardant of claim 1, 89-93g of distilled water, 2-4g of aziridine-modified isocyanate crosslinking agent, 0.5-1.6g of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine and 0.2-1.0g of benzylamine are placed in a beaker, and after the reagents are completely dissolved, the pH value is adjusted to 7.5 with alkali to obtain a flame retardant finishing liquid.

[0030] The alkali in the flame retardant pretreatment process can be any solution such as NaOH, KOH, etc.

[0031] The positive effects of the present invention are:

[0032] (1) The principle of the present invention is to solve the problem that tris(2-hydroxyethyl)isocyanurate has a small molecular weight, is extremely soluble in water, has poor thermal stability when used alone as a carbon-forming agent, and is easy to migrate and precipitate from the material. Tris(2-hydroxyethyl)isocyanurate and maleic anhydride are used to carry out a ring-opening reaction of hydroxyl groups and anhydride, and the double bond of maleic anhydride is introduced into tris(2-hydroxyethyl)isocyanurate. Considering that the molecular weight of the obtained product is small, an initiator of about 3% by weight of maleic anhydride is used for moderate polymerization to increase the molecular weight of the product, and a large number of functional groups such as hydroxyl groups and carboxyl groups are introduced into the polymer system.

[0033] (2) There are a large number of hydroxyl and carboxyl groups in the copolymer of isocyanurate and maleic anhydride. Tetrakis(hydroxymethyl)phosphonium sulfate with good flame retardancy is introduced into the system. The tetrakis(hydroxymethyl)phosphonium sulfate is introduced into the polymer system by the reaction between carboxyl and hydroxyl groups. At the same time, the amino group in tris(hydroxymethyl)aminomethane is reacted with the carboxyl or amino group in the system to introduce tris(hydroxymethyl)aminomethane with good charring property. The obtained product is then reacted with the amino or hydroxyl group in the organosilicon to introduce silicon element into the system. Then, reinforcing material is introduced into the obtained product. This not only improves the strength of the flame retardant, but more importantly, improves the strength of the cotton fabric after washing. This is different from the traditional flame retardant (which is easy to form a strong acid system and will cause the strength of the cotton fabric to decrease). At the same time, it improves the defect that the cotton fabric is often washed with water and the flame retardancy is greatly reduced. Therefore, the present invention uses a reinforcing cotton washing material containing ketones to modify the cotton fabric to prevent the flame retardant from being washed away, thereby improving the water resistance of the flame retardant and the durability of the flame retardant cotton fiber.

[0034] (3) The reinforcing material utilizes the rigidity of the benzene ring combined with the flexibility of silicone to assist aluminum sulfate in complexing the hydroxyl groups in the system. At the same time, with the help of the large number of carboxyl anions and hydroxyl groups in the sodium ethylenediamine di-o-phenylacetate system, aluminum sulfate, which is easily complexed, can be used to combine. The aluminum sulfate can then combine with the hydroxyl groups in the cotton fabric, so that the system can introduce compounds that combine rigidity and flexibility, and these groups can be better combined with the cotton fabric.

[0035] (4) The present invention utilizes that sodium carboxymethyl cellulose can be oxidized by sodium periodate, and the 1,4-glucoside on the sodium carboxymethyl cellulose undergoes a ring-opening reaction, the bond between C2 and C3 is broken, and the hydroxyl groups at both ends of the open ring are oxidized to aldehyde groups. The aldehyde groups are used to seal the hydroxyl groups in the flame retardant. At the same time, the oxidation product of sodium carboxymethyl cellulose, dialdehyde carboxymethyl cellulose, can maintain the fiber shape, can be complexed with aluminum in the flame retardant, and can also combine with the hydroxyl groups in the cotton fiber and the flame retardant, forming a network distribution structure, thereby enhancing the strength of the cotton fiber and improving the water washability of the cotton fiber.

[0036] (5) Before flame retardant treatment, the material needs to be pretreated to improve the disadvantage of low liquid carrying rate and remove impurities and additives on the surface of cotton fabric for subsequent flame retardant treatment. N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine is added during the finishing process to improve the strength of cotton fabric. At the same time, dialdehyde carboxymethyl cellulose combines with the hydroxyl group of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine in a weak alkaline environment. At the same time, N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine combines with the hydroxyl group of cotton fiber to improve the water resistance of cotton fabric. The benzylamine in it not only enhances the weak alkalinity of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine, but also enhances the rigidity of the cotton fiber system, resulting in that the strength of the fiber will not decrease significantly (the flame retardancy will also decrease less). Aziridine-modified isocyanate is used as a cross-linking agent to combine the flame retardant component with cotton fabric, so that the flame retardant can exert a flame retardant effect.

[0037] (6) Aminoacetic acid is used for neutralization to seal the carboxyl group, so that the amino group reacts with the C-Cl in cyanuric chloride to form a flame retardant with a large molecular weight. At the same time, chromium trichloride is used for complexation with the carboxyl group to facilitate the dispersion of the flame retardant component around the chromium trichloride. The resulting MOFs compound has relatively strong heat resistance and can absorb smoke, resulting in a significant reduction in the smoke of cotton fabrics. It also catalyzes the carbonization of cotton fabrics, greatly enhancing the carbonization of the combustion surface of cotton fabrics, and improving the flame retardancy of cotton fabrics. The imino, carboxyl and chromium in the MOFs compound system are combined with the hydroxyl groups in the cotton fabric. The MOFs-modified nitrogen-phosphorus-silicon flame retardant is dispersed on the cotton fabric and also has a strong bond, so the decrease in water resistance of the flame retardant is not particularly large.

[0038] (7) Fit C surface treatment agent comes from Qihe Lihou Chemical Co., Ltd., double-terminal alcohol hydroxy silicone oil IOTA2110 comes from Anhui Aiyota Silicone Oil Co., Ltd., aziridine modified isocyanate crosslinking agent comes from Shanghai Zelong Chemical Co., Ltd. XC-205 type, α, ω-dihydroxy polydimethylsiloxane was prepared with reference to Yang Caiping's academic paper and can also be purchased. For chemicals whose companies are not specified, as long as the main components are suitable, they can be used. DETAILED DESCRIPTION

[0039] The present invention is further described below with reference to examples.

[0040] Example 1

[0041] Preparation of MOFs modified nitrogen-phosphorus-silicon flame retardant and its application in cotton fabrics. The preparation of MOFs modified nitrogen-phosphorus-silicon flame retardant is as follows:

[0042] (1) Add 16 g of distilled water to 26 g of tris(2-hydroxyethyl)isocyanurate and 9.8 g of maleic anhydride, stir and react at 55° C. for 1 h, then add 0.3 g of ammonium persulfate (dissolved in 5 g of water), stir and react at 75° C. for 2 h, to obtain a polymer of isocyanurate and maleic anhydride;

[0043] (2) Add 3.5 g of tetrakis(hydroxymethyl)phosphine sulfate and 1 g of tris(hydroxymethyl)aminomethane to the system of step (1), adjust the pH to 7-8 with sodium hydroxide, stir and react at 60° C. for 1 h, add 3.2 g of γ-aminopropyltriethoxysilane, stir and react at 50° C. for 1 h, then add 1.2 g of reinforcing material A, stir and react at 90° C. for 1 h, then add 1.6 g of sodium dialdehyde carboxymethyl cellulose, stir and react at 60° C. for 30 min, and obtain the nitrogen-phosphorus-silicon flame retardant; (3) Weigh 21 g of aminoacetic acid and 35 g of 1,4-dioxane, stir and mix, adjust the pH to 8 with a 30% by mass sodium hydroxide aqueous solution, and distill under reduced pressure. Remove water, add 16.6 g of cyanuric chloride into the system three times (if the system cannot be stirred, add solvent 1,4-dioxane), each time with an interval of 15 minutes, heat the reaction system to 110°C to make the reaction system reach reflux state (maintain the system pH to 8), and react at this temperature for 3 hours, cool naturally to room temperature, acidify the solution to pH = 3 with 15% mass fraction of dilute hydrochloric acid, stir vigorously throughout the whole process, the solution becomes turbid when the dilute hydrochloric acid is added, maintain stirring for 30 minutes, centrifuge the mixed solution, wash with 60 mL of water, 30 mL of 95% alcohol and 40 mL of anhydrous methanol, respectively, and vacuum dry to obtain cyanuric chloride flame retardant;

[0044] (4) 15 g of the product obtained in step (3) was dissolved in 75.00 mL of a mixed solution consisting of N,N-dimethylacetamide and methanol in a volume ratio of 4:1, 7.5 g of chromium chloride and 10 drops of ammonia water were added thereto, the mixed solution was stirred for about 10 min until there were no solid particles in the system, the mixed system was transferred to a polytetrafluoroethylene liner (reactor), reacted at 120° C. for 24 h, and programmed cooling to obtain the MOFs product.

[0045] (5) Add 2.1 g of the MOFs product obtained in step (4) to step (2), and react at 70° C. for 1 h to obtain a MOFs-modified nitrogen-phosphorus-silicon flame retardant.

[0046] The reinforcing material A is prepared by dropping 15 g of phosphorus oxychloride into 11 g of phenol, controlling the reaction temperature at 30°C, protecting with nitrogen, adding for 20 min, stirring for 1 h, adjusting the pH to 7, adding 16 g of α,ω-dihydroxypolydimethylsiloxane to the system, stirring and reacting at 50°C for 30 min, adding 3.1 g of aluminum sulfate, 1.6 g of zirconium sulfate and 6.3 g of sodium ethylenediamine di-o-phenylacetate, stirring and reacting at 40°C for 30 min, controlling the pH to neutral during the reaction, completing the reaction, vacuum filtering, and drying the product to obtain a light yellow product, which is the reinforcing material A;

[0047] The sodium dialdehyde carboxymethyl cellulose is prepared by accurately weighing 1.6 g of sodium carboxymethyl cellulose and placing it in a beaker containing 30 mL of deionized water, stirring and dissolving to obtain an aqueous solution of sodium carboxymethyl cellulose, adding 20 mL of a 0.2 g / L NaIO4 solution, adjusting the pH of the system to 4, reacting under stirring conditions at 50° C. in the dark for 1 h, pouring the product after the reaction into 15 mL of anhydrous ethanol to filter the precipitate, collecting the filter cake, washing the filter cake alternately with deionized water and anhydrous ethanol, and drying the washed filter cake at 60° C. for 2 h to obtain sodium dialdehyde carboxymethyl cellulose;

[0048] The MOFs modified nitrogen-phosphorus-silicon flame retardant is applied to cotton fabrics as follows: (a) Flame retardant pretreatment process of cotton fabrics: Cut the cotton fabrics into several square cotton fabrics of 25 cm × 25 cm for later use, pour the pretreatment liquid into a plastic beaker, place the cut fabrics flat under the liquid surface, soak for 1 hour, take out and wash, and dry at 60°C;

[0049] The preparation method of the pretreatment liquid is as follows: 90 g of water, 0.5 g of NaOH (a 30% by mass aqueous solution), and 0.4 g of Fit C surface treatment agent (Qihe Lihou Chemical Co., Ltd., the same below) are added and stirred to obtain a pretreatment liquid;

[0050] (b) Process of flame retardant treatment of cotton fabric: transfer the flame retardant finishing liquid to a conical flask, immerse the cotton fabric in step (a), and oscillate in a water bath constant temperature oscillator for 20 minutes at a temperature of 60° C. and a rotation speed of 30 rpm. After the oscillation is completed, take out the fabric, squeeze out the water, and the squeezing rate is 70%, and dry it in an electric constant temperature blast drying oven at 60° C.;

[0051] The preparation method of the flame retardant finishing liquid is as follows: 8 g of the MOFs-modified nitrogen-phosphorus-silicon flame retardant of claim 1, 89 g of distilled water, 4 g of aziridine-modified isocyanate crosslinking agent, 0.5 g of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine and 0.2 g of benzylamine are placed in a beaker, and after the reagents are completely dissolved, the pH value is adjusted to 7.5 with NaOH to obtain a flame retardant finishing liquid;

[0052] (c) Repeat the process twice, placing the cotton in the flame retardant finishing liquid, and controlling the liquid penetration rate to 70% (the shaking time, shaking temperature, rotation speed, and drying temperature are the same as those in step b). The cotton fabric after the third drying is baked at 103° C. for 4 min, and then taken out to obtain a flame retardant cotton fabric.

[0053] Example 2

[0054] Preparation of MOFs modified nitrogen-phosphorus-silicon flame retardant and its application in cotton fabrics. The preparation of MOFs modified nitrogen-phosphorus-silicon flame retardant includes the following processes:

[0055] (1) Add 20 g of distilled water to 26 g of tris(2-hydroxyethyl)isocyanurate and 11.2 g of maleic anhydride, stir and react at 75° C. for 3 h, then add 0.4 g of potassium persulfate (dissolved in 5 g of water), stir and react at 85° C. for 3 h to obtain a polymer of isocyanurate and maleic anhydride;

[0056] (2) Add 4.2 g of tetrakis(hydroxymethyl)phosphine sulfate and 2 g of tris(hydroxymethyl)aminomethane to the system of step (1), adjust the pH to 7-8 with sodium hydroxide, stir and react at 90° C. for 2 h, add 4.1 g of double-end alcohol hydroxy silicone oil IOTA2110 (Anhui Iota Silicone Oil Co., Ltd.), stir and react at 70° C. for 2 h, then add 2.5 g of reinforcing material A, stir and react at 90° C. for 2 h, then add 2.4 g of sodium dialdehyde carboxymethyl cellulose, stir and react at 70° C. for 40 min, and obtain the nitrogen-phosphorus-silicon flame retardant;

[0057] (3) Weigh 21 g of aminoacetic acid and 35 g of 1,4-dioxane, stir and mix, adjust the pH to 8 with a 30% sodium hydroxide aqueous solution, remove water by distillation under reduced pressure, add 29.8 g of cyanuric chloride to the system three times, each time with an interval of 15 minutes, heat the reaction system to 110° C. to reflux the reaction system (maintaining the pH of the system at 8), and react at this temperature for 5 hours, cool naturally to room temperature, acidify the solution to pH = 3 with 15% dilute hydrochloric acid, and stir vigorously throughout the process. When the dilute hydrochloric acid is added, the solution becomes turbid and releases a large number of bubbles. Stirring is maintained for 60 minutes, and the mixed solution is centrifuged, washed with 60 mL of water, 30 mL of 95% alcohol and 40 mL of anhydrous methanol, respectively, and dried in vacuo to obtain a cyanuric chloride flame retardant;

[0058] (4) 15 g of the product obtained in step (3) was dissolved in 75.00 mL of a mixed solution consisting of N,N-dimethylacetamide and methanol in a volume ratio of 4:1, 11.6 g of chromium chloride and 10 drops of ammonia water were added thereto, the mixed solution was stirred for about 10 min until there were no solid particles in the system, the mixed system was transferred to a polytetrafluoroethylene-lined reactor, reacted at 120° C. for 36 h, and programmed cooling to obtain the MOFs product.

[0059] (5) Add 2.1 g of the MOFs product obtained in step (4) to step (2), and react at 80° C. for 2 h to obtain a MOFs-modified nitrogen-phosphorus-silicon flame retardant.

[0060] The reinforcing material A is prepared by dropping 18 g of phosphorus oxychloride into 11 g of phenol, controlling the reaction temperature at 40°C, protecting with nitrogen, adding for 50 min, stirring for 2 h, adjusting the pH to 7, adding 22 g of α,ω-dihydroxypolydimethylsiloxane to the system, stirring and reacting at 70°C for 40 min, adding 4.6 g of aluminum sulfate, 2.4 g of zirconium sulfate and 7.3 g of sodium ethylenediamine di-o-phenylacetate, stirring and reacting at 50°C for 40 min, controlling the pH to neutral during the reaction, completing the reaction, vacuum filtering, and drying the product to obtain a light yellow product, which is the reinforcing material A;

[0061] The dialdehyde sodium carboxymethyl cellulose is prepared by accurately weighing 1.6 g of sodium carboxymethyl cellulose and placing it in a beaker containing 30 mL of deionized water, stirring and dissolving to obtain an aqueous solution of sodium carboxymethyl cellulose, adding 20 mL of a 0.2 g / L NaIO4 solution, adjusting the pH of the system to 4, reacting under stirring conditions at 60° C. in the dark for 2 h, pouring the product after the reaction into 30 mL of anhydrous ethanol to filter the precipitate, collecting the filter cake, washing the filter cake alternately with deionized water and anhydrous ethanol, and drying the washed filter cake at 70° C. for 5 h to obtain the dialdehyde sodium carboxymethyl cellulose;

[0062] The application process of cotton fabric is as follows: (a) Flame retardant pretreatment process of cotton fabric: cut the cotton fabric into several square cotton fabrics of 25 cm × 25 cm for use, pour the pretreatment liquid into a plastic beaker, place the cut fabric flat under the liquid surface, soak for 3 hours, take out and wash, and dry at 90°C;

[0063] The preparation method of the pretreatment liquid is as follows: 95g of water, 1g of KOH (30% aqueous solution by mass), and 0.7g of Fit C surface treatment agent are added and stirred to obtain the pretreatment liquid;

[0064] (b) Process of treating the cotton fabric with flame retardancy: the flame retardant finishing liquid is transferred to a conical flask, and the cotton fabric of step (a) is immersed in the flame retardant finishing liquid. The cotton fabric is placed in a water bath constant temperature oscillator and oscillated for 40 min at a temperature of 90° C. and a rotation speed of 60 rpm. After the oscillation is completed, the fabric is taken out and the water is squeezed out. The squeezing rate is 70%. The fabric is dried in an electric constant temperature blast drying oven at 90° C. The above operation is repeated 5 times (as emphasized in Example 1). The cotton fabric after the sixth drying is baked at 110° C. for 7 min and taken out to obtain a flame retardant cotton fabric.

[0065] The preparation method of the flame retardant finishing liquid is as follows: 10 g of the MOFs-modified nitrogen-phosphorus-silicon flame retardant of claim 1, 93 g of distilled water, 4 g of aziridine-modified isocyanate crosslinking agent, 1.6 g of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine and 1.0 g of benzylamine are placed in a beaker, and after the reagents are completely dissolved, the pH value is adjusted to 7.5 with KOH to obtain a flame retardant finishing liquid.

[0066] Example 3

[0067] Preparation of MOFS modified nitrogen-phosphorus-silicon flame retardant and its application in cotton fabrics. The preparation of MOFs modified nitrogen-phosphorus-silicon flame retardant includes the following processes:

[0068] (1) 26 g of tris(2-hydroxyethyl)isocyanurate, 10.5 g of maleic anhydride and 18 g of distilled water were stirred at 65° C. for 2 h, and then 0.35 g of ammonium persulfate (dissolved in 5 g of water) was added, and the mixture was stirred at 80° C. for 2.5 h to obtain a polymer of isocyanurate and maleic anhydride;

[0069] (2) Add 3.8 g of tetrakis(hydroxymethyl)phosphine sulfate and 1.5 g of tris(hydroxymethyl)aminomethane to the system of step (1), adjust the pH to 7-8 with sodium hydroxide, stir and react at 75° C. for 1.5 h, add 3.6 g of γ-aminopropyltriethoxysilane, stir and react at 60° C. for 1.5 h, then add 1.8 g of reinforcing material A, stir and react at 90° C. for 1.5 h, then add 2 g of sodium dialdehyde carboxymethyl cellulose, stir and react at 65° C. for 35 min, and obtain the nitrogen-phosphorus-silicon flame retardant;

[0070] (3) Weigh 21 g of aminoacetic acid and 35 g of 1,4-dioxane, stir and mix, adjust the pH to 8 with a 30% by mass aqueous sodium hydroxide solution, remove water by distillation under reduced pressure, add 23.2 g of cyanuric chloride to the system three times, each time with an interval of 15 minutes, heat the reaction system to 110° C. to reflux the reaction system (maintain the pH of the system at 8), and react at this temperature for 4 hours, cool naturally to room temperature, acidify the solution to pH = 3 with 15% by mass dilute hydrochloric acid, stir vigorously throughout the whole process, and the solution becomes turbid when the dilute hydrochloric acid is added. Stirring is maintained for 45 minutes, centrifuge the mixed solution, wash with 60 mL of water, 30 mL of 95% alcohol and 40 mL of anhydrous methanol, respectively, and vacuum dry to obtain cyanuric chloride flame retardant;

[0071] (4) 15 g of the product obtained in step (3) was dissolved in 75.00 mL of a mixed solution consisting of N,N-dimethylacetamide and methanol in a volume ratio of 4:1, 9.5 g of chromium chloride and 10 drops of ammonia were added thereto, the mixed solution was stirred for 10 min until there were no solid particles in the system, the mixed system was transferred to a polytetrafluoroethylene liner, reacted at 120 ° C for 30 h, and programmed cooling to obtain the MOFs product.

[0072] (5) Add 2.1 g of the MOFs product obtained in step (4) to step (2), and react at 75° C. for 1.5 h to obtain a MOFs-modified nitrogen-phosphorus-silicon flame retardant.

[0073] The reinforcing material A is prepared by dropping 16.5 g of phosphorus oxychloride into 11 g of phenol, controlling the reaction temperature to 35° C., protecting with nitrogen, adding for 35 min, stirring for 1.5 h, adjusting the pH to 7, adding 19 g of α,ω-dihydroxypolydimethylsiloxane to the system, stirring and reacting at 60° C. for 35 min, adding 3.8 g of aluminum sulfate, 2.0 g of zirconium sulfate and 6.8 g of sodium ethylenediamine di-o-phenylacetate, stirring and reacting at 45° C. for 35 min, controlling the pH to neutral during the reaction, completing the reaction, vacuum filtering, and drying the product to obtain a light yellow product, which is the reinforcing material A;

[0074] The dialdehyde sodium carboxymethyl cellulose is prepared by accurately weighing 1.6 g of sodium carboxymethyl cellulose and placing it in a beaker containing 30 mL of deionized water, stirring and dissolving to obtain an aqueous solution of sodium carboxymethyl cellulose, adding 20 mL of a 0.2 g / L NaIO4 solution, adjusting the pH of the system to 4, reacting under stirring conditions at 55° C. in the dark for 1.5 hours, pouring the product after the reaction into 22.5 mL of anhydrous ethanol to filter the precipitate, collecting the filter cake, washing the filter cake alternately with deionized water and anhydrous ethanol, and drying the washed filter cake at 65° C. for 3.5 hours to obtain the dialdehyde sodium carboxymethyl cellulose;

[0075] The application process of cotton fabric is as follows: (a) Flame retardant pretreatment process of cotton fabric: cut the cotton fabric into several square cotton fabrics of 25 cm × 25 cm for use, pour the pretreatment liquid into a plastic beaker, place the cut fabric flat under the liquid surface, soak for 2 hours, take out and wash, and dry at 75°C;

[0076] The preparation method of the pretreatment liquid is as follows: 92g of water, 0.75g of KOH (30% aqueous solution by mass), and 0.55g of Fit C surface treatment agent are added and stirred to obtain the pretreatment liquid;

[0077] (b) Process of flame retardant treatment of cotton fabric: the flame retardant finishing liquid is transferred to a conical flask, immersed in the cotton fabric of step (a), and placed in a water bath constant temperature oscillator for 30 min at a temperature of 75° C. and a rotation speed of 45 rpm. After the oscillation is completed, the fabric is taken out and the water is squeezed out with a liquid squeezing rate of 70%. The fabric is dried in an electric constant temperature blast drying oven at 75° C. The above operation is repeated twice. The dried cotton fabric is baked at 103° C. for 5.5 min and taken out to obtain a flame retardant cotton fabric.

[0078] The preparation method of the flame retardant finishing liquid is as follows: 9 g of the MOFs-modified nitrogen-phosphorus-silicon flame retardant described in step (2), 91 g of distilled water, 3 g of aziridine-modified isocyanate crosslinking agent, 1.05 g of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine and 0.6 g of benzylamine are placed in a beaker, and after the reagents are completely dissolved, the pH value is adjusted to 7.5 with KOH to obtain a flame retardant finishing liquid.

[0079] Washing process of flame-retardant cotton fabrics: The experiment simulates the environment of home machine washing. A small washing machine is used to wash the samples in batches for 50 times, adding 3 drops of laundry detergent each time, washing for 12 minutes, rinsing for 3 minutes, dehydrating and drying. After washing 50 times, the fabric is naturally dried to obtain the flame-retardant cotton fabric after washing.

[0080] The flame-retardant cotton fabric prepared according to the embodiment of the present invention and the cotton fabric treated with the existing commercially available flame retardant CP were tested and compared with the results of the master's thesis of Wang Qiyan of our team. The test data are shown in the following table.

[0081] Vertical burning test is one of the important indicators for evaluating the flame retardant properties of materials. The test items include the material's flaming burning time, flameless burning time, damaged length, etc.

[0082] According to GB / T 8746-2009 "Textiles - Combustion Performance - Determination of Ignition Ease of Vertical Specimens", the flame-retardant treated fabric is cut into the required size and placed in a constant temperature and humidity chamber (controlled temperature 21°C, humidity 65%) for testing. The fabric is fixed on the fixture and the vertical combustion test is performed using the CZF-3 horizontal vertical combustion tester produced by Nanjing Shangyuan Analytical Instrument Co., Ltd. Observe the combustion of the sample, record the flame burning time and flameless burning time of the sample, and measure its damaged length.

[0083] The limiting oxygen index refers to the minimum oxygen ratio required to support the complete combustion of a sample within 3 minutes when it is ignited in a nitrogen and oxygen mixed gas atmosphere. Generally speaking, the higher the limiting oxygen index value, the higher the oxygen concentration required for the sample to burn, that is, the more difficult the sample is to burn.

[0084] According to TB / T 2919-1998 "Test Method for Fabric Combustion Oxygen Index", cut the flame-retardant fabric into 5cm×15cm size and put it into a constant temperature and humidity chamber (temperature set at 21℃, humidity set at 60%) for more than 24 hours for testing. Fix the sample in the fixture, cover it with a glass cover, ignite above the sample to ensure that the sample can burn evenly from top to bottom, and then remove the fire source.

[0085] The residual carbon rate refers to the percentage of the remaining sample mass to the original sample mass after high-temperature burning.

[0086] One of the evaluation indicators of flame retardant performance of materials. Generally speaking, the higher the value of residual carbon rate, the better the flame retardant effect of the material.

[0087] Place the sample in an electric constant temperature blast drying oven and dry it to constant weight. Weigh about 1g of the sample to be tested into a 30mL ceramic crucible, record the mass of the empty crucible as m0, and the mass of the sample as m. Place the crucible in a muffle furnace, and heat it from room temperature to 200℃ at a rate of 10℃ / min, and keep it warm for 30min. Take out the sample, cool it to room temperature in a dryer, and weigh it. Repeat the above operation, starting from 200℃, at a rate of 10℃ / min, and a residual carbon rate of 500℃.

[0088] The total mass of the crucible and the remaining sample after each cooling is recorded as mi (i=1, 2, 3, . . . ).

[0089] The test instrument used was Sansi Zongheng UTM4103 universal testing machine. The test standard referred to GB / T3923.1-2013 "Tensile properties of textile fabrics Part 1: Determination of breaking strength and elongation at break (Strip method)", the original gauge length was 200mm, and the tensile speed was 100mm / min.

[0090] Smoke suppression performance: According to ISO5659 standard, the fabrics before and after finishing were flamelessly heated using FTT0064 test chamber, with a heating temperature of 560°C, a time of 700s, and a radiation power of 25kw / m 2 . Sample size: 80×80mm 2 , take the maximum combustion smoke for comparison (suppressed smoke).

[0091] Table 1 Comparison of properties of cotton fabrics after flame retardant treatment

[0092]

[0093] As can be seen from Table 1 above, the flame-retardant cotton fabric prepared by the present invention is superior to Example 1 and Example 2 in terms of oxygen index, afterflaming time and smoldering time. "—" indicates that the damaged length is almost non-existent. The greater the maximum value of smoke suppression performance, that is, smoke density, the more smoke is released.

[0094] Table 2 Comparison of properties of cotton fabrics after flame retardant treatment

[0095]

[0096]

[0097] Wang Qiyan's master's thesis at Yantai University (the limiting oxygen index in the previous results of this team may also be 32.5, and there is a proper difference each time the comparison is made). From the research data in Table 2 combined with Table 1, it can be found that the current results of this team are better than the previous results of this team and the flame retardant CP on the market.

[0098] Table 3 Oxygen index of cotton fabrics treated with different flame retardants after 50 times

[0099]

[0100] It can be found from Table 3 that after the flame retardant cotton treated with different flame retardants was washed 50 times, the oxygen index of the improved one was the highest. At the same time, it was found from the experiment that due to the low pH in the flame retardant synthesized by our team in the early stage, the cotton fabric had almost no strength and could not be formed normally, while the flame retardancy of CP decreased, but it could be formed. The smoke suppression performance of the present invention decreased less than that of the previous one. Our team did not measure the smoke suppression in the early stage, but made up for it in the later stage, and found that the residual carbon rate was not high. The flame retardancy of the present invention was significantly better than the above two, and the strength could be maintained at a tensile strength of 10.23Mpa.

[0101] Table 4 Limiting oxygen index of cotton fabrics treated with different flame retardants after 50 times (without adding some materials, taking Example 2 as an example)

[0102] project Limiting oxygen index / % Without addition of tris(2-hydroxyethyl)isocyanurate 34.4 No (maleic anhydride) added 33.3 No (sodium ethylenediamine di-o-phenylacetate) added 33.6 No (aluminum sulfate) added 34.6 No (sodium carboxymethyl cellulose) added 33.8 No (zirconium sulfate) added 32.4

[0103] It can be found from Table 4 that the oxygen index of the cotton fabric obtained without adding tri(2-hydroxyethyl)isocyanurate, maleic anhydride, sodium ethylenediamine di-o-phenylacetate, aluminum sulfate, zirconium sulfate and sodium carboxymethyl cellulose was greatly reduced after washing, so the above substances played a special role.

[0104] Table 5 Carbon residue rate and smoke performance of cotton fabrics treated with different flame retardants (without adding some materials, taking Example 2 as an example)

[0105] project Residual carbon rate / % Smoke suppression (max) No aminoacetic acid added 32.1 27.8 No cyanuric chloride added 28.6 29.8 No chromium chloride added 24.6 46.8

[0106] It can be found from Table 5 that the carbon residue rate decreases and the smoke suppression performance decreases when aminoacetic acid, cyanuric chloride and chromium trichloride are not added, so the above substances play a flame retardant effect.

[0107] The limiting oxygen index without adding N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine and aniline is shown in Table 6.

[0108] Table 6 Comparison of some material effects

[0109]

[0110] From Table 6, N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine and aniline have a strong supporting effect on enhancing the flame retardant treatment performance of cotton fabrics.

[0111] The flame retardant synthesized earlier by our team (the flame retardant of Wang Qiyan's master's thesis) and CP flame retardant (Beijing Cleansun High-Tech Co., Ltd.) were dried, and the carbon residue rate and expansion height were compared with the flame retardant of Example 2 of the present invention to comprehensively compare the flame retardant performance.

[0112] Table 7 Flame retardant data comparison

[0113]

[0114]

[0115] The expansion height needs to measure the expansion height at the residual carbon rate at 500°C. From Table 7, it can be found that the flame retardant prepared by the present invention is superior to the flame retardant synthesized by the team in the early stage and the traditional CP flame retardant for cotton in terms of residual carbon rate and expansion height. Taking the flame retardant prepared in Example 2 as an example, the influence of various factors on flame retardancy is studied.

[0116] Table 8 Flame retardant changes of the following materials are not added

[0117] project Example 2 Residual carbon rate / % (without addition) tris(2-hydroxyethyl)isocyanurate 31.5 Swelling height / cm (without addition) tris(2-hydroxyethyl)isocyanurate 1.23 Carbon Residue Rate / % (without addition)Tetrakis Hydroxymethyl Phosphate 32.4 Swelling height / cm (without addition)Tetrakis(hydroxymethyl)phosphonium sulfate 1.36

[0118] It can be seen from Table 8 that the absence of tris(2-hydroxyethyl)isocyanurate and tetrakis(hydroxymethyl)phosphonium sulfate will affect the carbon residue rate of the material and the corresponding expansion height.

Claims

1. MOFs modified nitrogen-phosphorus-silicon flame retardant is used for cotton fabric, characterized in that: The flame retardant treatment process of MOFs modified nitrogen phosphorus silicon flame retardant for cotton fabric is as follows: (a) Flame retardant pretreatment process of cotton fabric: Cut the cotton fabric into several square cotton fabrics of 25 cm × 25 cm and set aside. Pour the pretreatment liquid into a plastic beaker, place the cut cotton fabric flat under the liquid surface, soak for 1-3 h, take out and wash with water, and dry the cotton fabric at 60-90℃; The preparation method of the pretreatment liquid is as follows: add 90-95g of water, 0.5-1g of alkali, and 0.4-0.7g of Fit C surface treatment agent, and stir evenly to obtain the pretreatment liquid; (b) Process of flame retardant treatment of cotton fabric: transfer the flame retardant finishing liquid to a conical flask, immerse the cotton fabric of step (a), place it in a water bath constant temperature oscillator and oscillate for 20-40 minutes at a temperature of 60-90°C and a rotation speed of 30-60 rpm. After the oscillation is completed, take out the fabric, squeeze out the water, and squeeze out the liquid at a rate of 70%. Dry it in an electric constant temperature blast drying oven at 60-90°C. Repeat the above operation 2-5 times. Bake the dried cotton fabric at 103-110°C for 4-7 minutes and take it out to obtain a flame retardant cotton fabric. The preparation method of the flame retardant finishing liquid is as follows: 8-10 g of the MOFs-modified nitrogen-phosphorus-silicon flame retardant of claim 1, 89-93 g of distilled water, 2-4 g of aziridine-modified isocyanate crosslinking agent, 0.5-1.6 g of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine and 0.2-1.0 g of benzylamine are added to a beaker, and after the reagents are completely dissolved, the pH value is adjusted to 7.5 with an alkali to obtain a flame retardant finishing liquid; The reinforcing material A is prepared by dropping 15-18 g of phosphorus oxychloride into 11 g of phenol, controlling the reaction temperature at 30-40° C., protecting with nitrogen, adding for 20-50 min, stirring for 1-2 h, adjusting the pH to 7, adding 16-22 g of α,ω-dihydroxypolydimethylsiloxane to the system, stirring and reacting at 50-70° C. for 30-40 min, adding 3.1-4.6 g of aluminum sulfate, 1.6-2.4 g of zirconium sulfate and 6.3-7.3 g of sodium ethylenediamine di-o-phenylacetate, stirring and reacting at 40-50° C. for 30-40 min, controlling the pH to be neutral during the reaction, completing the reaction, filtering under reduced pressure, and drying the product to obtain a light yellow product, which is the reinforcing material A.

2. The MOFs-modified nitrogen-phosphorus-silicon flame retardant according to claim 1 is used for cotton fabric, wherein the preparation of the MOFs-modified nitrogen-phosphorus-silicon flame retardant comprises the following process: (1) Add 16-20 g of distilled water to 26 g of tris(2-hydroxyethyl)isocyanurate and 9.8-11.2 g of maleic anhydride, stir and react at 55-75°C for 1-3 h, then add 0.3-0.4 g of initiator, stir and react at 75-85°C for 2-3 h to obtain a polymer of isocyanurate and maleic anhydride; (2) Add 3.5-4.2 g of tetrakis(hydroxymethyl)phosphonium sulfate and 1-2 g of tris(hydroxymethyl)aminomethane to the system of step (1), adjust the pH to 7-8, stir and react at 60-90° C. for 1-2 h, add 3.2-4.1 g of organosilicon, stir and react at 50-70° C. for 1-2 h, then add 1.2-2.5 g of reinforcing material A, stir and react at 90° C. for 1-2 h, then add 1.6-2.4 g of sodium dialdehyde carboxymethyl cellulose, stir and react at 60-70° C. for 30-40 min, to obtain the nitrogen-phosphorus-silicon flame retardant; (3) Weigh 21 g of aminoacetic acid and 35 g of 1,4-dioxane, stir and mix, adjust the pH to 8 with 30% by mass sodium hydroxide, remove water by vacuum distillation, add 16.6-29.8 g of cyanuric chloride to the system three times, each time with an interval of 15 minutes, heat the reaction system to 110°C to make the reaction system reach reflux state, and react at this temperature for 3-5 hours, cool naturally to room temperature, acidify the solution to pH = 3 with 15% by mass dilute hydrochloric acid, maintain stirring for 30-60 minutes, centrifuge the mixed solution, and then wash with 60 mL of water, 30 mL of 95% alcohol and 40 mL of anhydrous methanol respectively, and vacuum dry to obtain cyanuric chloride flame retardant; (4) Dissolve 15 g of the product obtained in step (3) in 75.00 mL of a mixed solution consisting of N,N-dimethylacetamide and methanol in a volume ratio of 4:1, add 7.5-11.6 g of chromium chloride and 10 drops of ammonia water, stir the mixed solution for 10 min until there are no solid particles in the system, transfer the mixed system to a polytetrafluoroethylene-lined reactor, react at 120°C for 24-36 h, and program cooling to obtain the MOFs product; (5) Add 2.1 g of the MOFs product obtained in step (4) to step (2), and react at 70-80° C. for 1-2 h to obtain a MOFs-modified nitrogen-phosphorus-silicon flame retardant.

3. The MOFs modified nitrogen-phosphorus-silicon flame retardant as claimed in claim 1 is used for cotton fabric, wherein the initiator is any one of ammonium persulfate and potassium persulfate.

4. The MOFs modified nitrogen-phosphorus-silicon flame retardant as claimed in claim 2 is used for cotton fabric, wherein the organosilicon is any one of γ-aminopropyltriethoxysilane and biterminal alcohol hydroxy silicone oil IOTA 2110.

5. The MOFs-modified nitrogen-phosphorus-silicon flame retardant as claimed in claim 2 is used for cotton fabrics, wherein the dialdehyde sodium carboxymethyl cellulose is prepared by weighing 1.6 g of sodium carboxymethyl cellulose and placing it in a beaker containing 30 mL of deionized water, stirring and dissolving to obtain an aqueous solution of sodium carboxymethyl cellulose, and then adding 20 mL of 0.2 g / L NaIO4 solution, adjusting the pH of the system to 4, reacting under stirring conditions at 50-60° C. in the dark for 1-2 h, pouring the product after the reaction into 15-30 mL of anhydrous ethanol to filter the precipitate, collecting the filter cake, washing the filter cake alternately with deionized water and anhydrous ethanol, and drying the washed filter cake at 60-70° C. for 2-5 h to obtain dialdehyde sodium carboxymethyl cellulose.

6. The MOFs modified nitrogen-phosphorus-silicon flame retardant as claimed in claim 1 is used for cotton fabric, and the alkali in the flame retardant pretreatment process can be any one of NaOH, KOH, etc.