Nickel-sulfur alloy grain corrosion method
Through the steps of primary grinding, secondary grinding, electrolytic polishing and corrosion treatment, the complex and residual problems of nickel-sulfur alloy grain corrosion methods are solved, and the crystal grains are clearly displayed and detection efficiency is improved.
Patent Information
- Application Number
- CN202411005539.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the existing technology, the grain corrosion method of nickel-sulfur alloy is complicated and easy to leave residues. There is no effective display method and it is difficult to meet the needs of practical applications.
Adopt the steps of primary grinding, secondary grinding, electrolytic polishing and corrosion treatment, grind and polish with water sandpaper and electrolytic polisher, use a mixture of ethanol, 2-butoxyethanol and perchloric acid for electrolytic polishing, and then use A mixture of hydrofluoric acid, nitric acid and pure water is used for corrosion treatment to ensure clear display of crystal grains.
It achieves clear display of grains in the alloy, stable operation process, short detection time, avoids the generation of defective products, and improves detection efficiency.
Smart Images

Figure CN118758700A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal grain detection and relates to a grain corrosion method for a nickel-sulfur alloy. Background Art
[0002] Metal materials are very small in size, but still contain many small crystals inside. Since these small crystals with basically the same lattice phase are irregular in shape and granular, they are called "grains". The size and shape of the grains have a significant impact on the properties of the material. Generally, the finer and more uniform the grains, the better the overall performance of the material.
[0003] The prior art solution discloses a method for etching cast grains of a nickel-based alloy, wherein the cast metallographic sample of the nickel-based alloy is mechanically ground, polished, cleaned, and blown dry, and then placed in a heat treatment furnace for oxidation treatment at 600-800°C for 1-3 hours, and after being air-cooled out of the furnace, the original polished surface is directly moderately polished and cleaned and blown dry, and then the polished surface is immersed in a newly prepared copper sulfate etching solution with a ratio of copper sulfate pentahydrate: water: concentrated hydrochloric acid: concentrated sulfuric acid = 20g: 80mL: 150mL: 5mL for etching, and the etching is carried out for 10-30s. After cleaning and drying, a clear and complete grain boundary can be obtained.
[0004] The prior art solution also discloses a preparation method of a nickel-based alloy metallographic etchant and a corrosion method thereof. In a well-ventilated fume hood, 15 g of ammonium sulfate powder is weighed and added to 50 mL of distilled water and stirred thoroughly. 50 g of ferric chloride powder is weighed and added to 100 mL of concentrated hydrochloric acid and stirred thoroughly. The ammonium sulfate solution is mixed with the hydrochloric acid-ferric chloride solution, and the prepared mixed solution is stirred evenly. Finally, 30 mL of concentrated nitric acid is added to the mixed solution, stirred evenly, and the nickel-based alloy metallographic etchant is prepared after standing.
[0005] The prior art solution also discloses a metallographic etchant for precipitation-strengthening high-temperature alloy and a method for using the same, comprising an acid substance and an organic corrosion inhibitor, wherein the volume ratio of the acid substance to the organic corrosion inhibitor is 32.3-44.3:40-51. The acid substance is a mixture of perchloric acid, acetic acid, citric acid and phosphoric acid, or a mixture of sulfuric acid, acetic acid, citric acid and phosphoric acid, or a mixture of perchloric acid, sulfuric acid, citric acid and phosphoric acid, or a mixture of perchloric acid, acetic acid, citric acid and sulfuric acid. The mechanically polished sample is placed in the prepared metallographic etchant for electrochemical corrosion, and the γ′ phase in the structure is observed and analyzed by scanning electron microscopy.
[0006] However, the existing technology still has the problem that the metallographic corrosion scheme is complicated and easily leaves residues. More importantly, there is no method for grain corrosion and display of nickel-sulfur alloys. Therefore, it is urgent to design a method for grain corrosion of nickel-sulfur alloys to overcome the defects of the existing technology and meet the needs of practical applications. Summary of the invention
[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a grain corrosion method for nickel-sulfur alloys. In the present invention, the specific steps of the grain corrosion method are designed to make the display of the grains in the alloy clearer, and the operating process of the overall method is stable and can be reused, the detection time is short, the results can be obtained efficiently, and the generation of defective products is effectively avoided.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] The present invention provides a method for grain corrosion of a nickel-sulfur alloy, the method comprising:
[0010] The alloy to be tested is subjected to primary grinding, secondary grinding, electrolytic polishing and corrosion treatment in sequence to obtain an alloy sample, and the alloy sample is placed in a metallographic microscope to observe and analyze the grains.
[0011] In the present invention, by designing the specific steps of the grain corrosion method, the display of the grains in the alloy is clearer, and the operation process of the overall method is stable and can be reused, the detection time is short, the results can be obtained efficiently, and the generation of defective products can be effectively avoided.
[0012] It should be noted that the present invention does not specifically limit the specific model and operation mode of the metallographic microscope, and those skilled in the art may make adaptive adjustments according to actual conditions.
[0013] As a preferred technical solution of the present invention, the first grinding is performed using water sandpaper.
[0014] It should be noted that the water sandpaper in the present invention is water-based sandpaper, which is a well-known material to those skilled in the art.
[0015] Preferably, the roughness of the water sandpaper is 200-400#, for example, it can be 200#, 300#, 400#, etc., but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0016] Preferably, the grinding time is 5 to 6 minutes, for example, it can be 5 minutes, 5.1 minutes, 5.2 minutes, 5.3 minutes, 5.4 minutes, 5.5 minutes, 5.6 minutes, 5.7 minutes, 5.8 minutes, 5.9 minutes, 6 minutes, etc., but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] The roughness of the water sandpaper in the present invention is 200-400# and the grinding time is 5-6min, because the rough grinding effect is good within this range. If it is not within this range, the grinding effect will be poor, because the surface cannot be removed if the time is short, and it is unnecessary if the time is too long.
[0018] As a preferred technical solution of the present invention, the secondary grinding is performed using water sandpaper.
[0019] Preferably, the roughness of the water sandpaper is 1000-1500#, for example, it can be 1000#, 1200#, 1400#, 1500#, etc., but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0020] Preferably, the secondary grinding time is 7 to 10 minutes, for example, it can be 7 minutes, 7.5 minutes, 8 minutes, 8.5 minutes, 9 minutes, 9.5 minutes, 10 minutes, etc., but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] The roughness of the water sandpaper in the present invention is 1000-1500# and the secondary grinding time is 7-10min, because the grinding effect is good within this range. If it is not within this range, the grinding effect will be poor, because the larger scratches cannot be removed if the time is short, and it is unnecessary if the time is too long.
[0022] As a preferred technical solution of the present invention, the electrolytic polishing is performed using an electrolytic polishing machine.
[0023] It should be noted that the present invention does not specifically limit the specific model and operation mode of the electrolytic polishing machine, and those skilled in the art can make adaptive adjustments according to actual conditions.
[0024] Preferably, the processing voltage of the electrolytic polishing machine is 36-40V, for example, it can be 36V, 36.5V, 37V, 37.5V, 38V, 38.5V, 39V, 39.5V, 40V, etc., but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] The processing voltage of the electrolytic polishing machine in the present invention is 36-40V because the electrolysis effect is good within this range. If it is not within this range, the electrolysis surface will be defective and rough. This is because the scratches cannot be removed if the voltage is too low, and excessively high voltage will cause over-polishing, and black stains will appear on the surface of the grain.
[0026] Preferably, the processing time of the electrolytic polishing machine is 50 to 60 s, for example, it can be 50s, 51s, 52s, 53s, 54s, 55s, 56s, 57s, 58s, 59s, 60s, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] The processing time of the electrolytic polishing machine in the present invention is 50 to 60 seconds because the electrolysis effect is good within this range. If it is not within this range, the electrolytic polishing surface will be rough. This is because if the time is too short, the polishing surface will be scratched, and if the time is too long, it will cause over-polishing.
[0028] As a preferred technical solution of the present invention, the electrolyte used in the electrolytic polishing is a mixture of ethanol, 2-butoxyethanol and perchloric acid.
[0029] It should be noted that the purity of ethanol in the present invention can be selected from 95% ethanol solution, and the perchloric acid can be selected from 30% perchloric acid solution, and the sources of ethanol, 2-butoxyethanol and perchloric acid can be 99.7% anhydrous ethanol, 99% 2-butoxyethanol and 70%-72% perchloric acid, respectively.
[0030] Preferably, the volume ratio of the ethanol, the 2-butoxyethanol and the perchloric acid is (7-8):1:(2-3), for example, it can be 7:1:2, 7:1:3, 8:1:2, 8:1:3, 7.5:1:2.5, 7.5:1:2, 7.5:1:3, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] In the present invention, the volume ratio of ethanol, 2-butoxyethanol and perchloric acid is (7-8):1:(2-3) because the electrolytic polishing effect is good within this range. If it is not within this range, the electrolytic polishing effect will be deteriorated. This is because the electrolytic polishing effect is inconsistent due to different chemical ratios.
[0032] As a preferred technical solution of the present invention, after the electrolytic polishing process, the electrolytically polished alloy needs to be cleaned.
[0033] Preferably, the cleaning process is performed by flushing with clean water.
[0034] It should be noted that the clean water in the present invention can be pure water, ultrapure water, etc., and those skilled in the art can make adaptive adjustments according to actual conditions.
[0035] As a preferred technical solution of the present invention, the corrosion treatment is carried out in the following manner:
[0036] The etchant is dropped onto the polished surface of the electrolytically polished alloy, and then washed after etching for a certain period of time.
[0037] As a preferred technical solution of the present invention, the etchant is a mixture of hydrofluoric acid, nitric acid and pure water.
[0038] It should be noted that the sources of the hydrofluoric acid, nitric acid and pure water in the present invention can be respectively hydrofluoric acid with a concentration of 40%, nitric acid with a concentration of 65%-68% and homemade pure water.
[0039] Preferably, the volume ratio of the hydrofluoric acid, the nitric acid and the pure water is 1:(10-12):(20-23), for example, it can be 1:10:20, 1:10:22, 1:10:23, 1:11:20, 1:11:23, 1:12:20, 1:12:21, 1:12:23, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0040] In the present invention, the volume ratio of hydrofluoric acid, nitric acid and pure water is 1:(10-12):(20-23) because the corrosion effect is good within this range. If it is not within this range, the corrosion effect will be worse. This is because different corrosion effects are caused by different chemical ratios.
[0041] As a preferred technical solution of the present invention, the titration time is 60 to 90 s, for example, it can be 60 s, 62 s, 65 s, 68 s, 70 s, 75 s, 78 s, 80 s, 84 s, 88 s, 90 s, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] The titration time in the present invention is 60 to 90 seconds because the corrosion effect is good within this range. If it is not within this range, the corrosion effect will be poor. This is because if the time is too short, the corrosion is incomplete, and if the time is too long, it will lead to over-corrosion, and there will be large black spots in the microscopic picture.
[0043] Preferably, pure water is used in the cleaning process.
[0044] As a preferred technical solution of the present invention, the grain corrosion method specifically includes:
[0045] The alloy to be tested is subjected to primary grinding, secondary grinding, electrolytic polishing and corrosion treatment in sequence to obtain an alloy sample, and the alloy sample is placed in a metallographic microscope to observe and analyze the grains;
[0046] The first grinding is performed using water sandpaper, the roughness of the water sandpaper is 200-400#, and the time of the first grinding is 5-6min;
[0047] The secondary grinding is performed using water sandpaper, the roughness of the water sandpaper is 1000-1500#, and the secondary grinding time is 7-10min;
[0048] The electrolytic polishing is performed by an electrolytic polishing machine, the processing voltage of the electrolytic polishing machine is 36-40V, the processing time of the electrolytic polishing machine is 50-60s, the electrolyte used in the electrolytic polishing is a mixed solution of ethanol, 2-butoxyethanol and perchloric acid, and the volume ratio of the ethanol, the 2-butoxyethanol and the perchloric acid is (7-8):1:(2-3);
[0049] After the electrolytic polishing process, the electrolytically polished alloy needs to be cleaned, and the cleaning process is performed by flushing with clean water;
[0050] The corrosion treatment is carried out as follows: dripping an etchant on the polished surface of the electrolytically polished alloy, etching for a certain period of time and then washing;
[0051] The etching agent is a mixture of hydrofluoric acid, nitric acid and pure water, the volume ratio of the hydrofluoric acid, the nitric acid and the pure water is 1:(10-12):(20-23), the titration time is 60-90s, and pure water is used in the cleaning process.
[0052] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0053] Compared with the prior art, the present invention has the following beneficial effects:
[0054] In the present invention, by designing the specific steps of the grain corrosion method, the display of the grains in the alloy is clearer, and the operation process of the overall method is stable and can be reused, the detection time is short, the results can be obtained efficiently, and the generation of defective products can be effectively avoided. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 This is an observation diagram of the metallographic structure of the grains provided in Example 1 of the present invention;
[0056] Figure 2 This is an observation diagram of the metallographic structure of the grains provided in Example 2 of the present invention;
[0057] Figure 3 This is an observation diagram of the metallographic structure of the grains provided in Example 3 of the present invention;
[0058] Figure 4 This is an observation diagram of the metallographic structure of the grains provided in Example 4 of the present invention;
[0059] Figure 5 This is an observation diagram of the metallographic structure of the grains provided in Example 5 of the present invention;
[0060] Figure 6 This is an observation diagram of the metallographic structure of the grains provided in Example 6 of the present invention;
[0061] Figure 7 This is an observation diagram of the metallographic structure of the grains provided in Example 7 of the present invention;
[0062] Figure 8 This is an observation diagram of the metallographic structure of the grains provided in Example 8 of the present invention;
[0063] Fig. 9 This is an observation diagram of the metallographic structure of the grains provided in Example 9 of the present invention;
[0064] Fig.10 This is an observation diagram of the metallographic structure of the grains provided in Example 10 of the present invention;
[0065] Fig.11 This is an observation diagram of the metallographic structure of the grains provided in Example 11 of the present invention;
[0066] Fig.12 This is an observation diagram of the metallographic structure of the grains provided in Example 12 of the present invention;
[0067] Fig.13 This is an observation diagram of the metallographic structure of the grains provided in Example 13 of the present invention;
[0068] Fig.14 This is an observation diagram of the metallographic structure of the grains provided in Example 14 of the present invention;
[0069] Fig.15 This is an observation diagram of the metallographic structure of the grains provided in Example 15 of the present invention;
[0070] Fig.16 This is an observation diagram of the grain metallographic structure provided for Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0071] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0072] Example 1
[0073] This embodiment provides a method for grain corrosion of a nickel-sulfur alloy, comprising:
[0074] The alloy to be tested is subjected to primary grinding, secondary grinding, electrolytic polishing and corrosion treatment in sequence to obtain an alloy sample, and the alloy sample is placed in a metallographic microscope to observe and analyze the grains.
[0075] The first grinding is done with water sandpaper, the roughness of the water sandpaper is 200#, and the grinding time is 6 minutes.
[0076] The secondary grinding is carried out with water sandpaper, the roughness of the water sandpaper is 1000#, and the secondary grinding time is 10 minutes.
[0077] Electrolytic polishing is carried out using an electrolytic polishing machine. The processing voltage of the electrolytic polishing machine is 36V, the processing time of the electrolytic polishing machine is 60s, and the electrolyte used for electrolytic polishing is a mixture of ethanol, 2-butoxyethanol and perchloric acid. The volume ratio of ethanol, 2-butoxyethanol and perchloric acid is 7:1:2.
[0078] After the electrolytic polishing process, the electrolytically polished alloy needs to be cleaned by rinsing with clean water.
[0079] The etching treatment is carried out as follows: an etchant is dropped onto the polished surface of the electrolytically polished alloy, and the surface is etched for a certain period of time and then washed off.
[0080] The etchant is a mixture of hydrofluoric acid, nitric acid and pure water, the volume ratio of hydrofluoric acid, nitric acid and pure water is 1:10:20, the certain time is 90s, and pure water is used in the cleaning process.
[0081] Example 2
[0082] This embodiment provides a method for grain corrosion of a nickel-sulfur alloy, comprising:
[0083] The alloy to be tested is subjected to primary grinding, secondary grinding, electrolytic polishing and corrosion treatment in sequence to obtain an alloy sample, and the alloy sample is placed in a metallographic microscope to observe and analyze the grains.
[0084] The first grinding is done with water sandpaper, the roughness of the water sandpaper is 300#, and the grinding time is 5.5 minutes.
[0085] The secondary grinding is carried out with water sandpaper, the roughness of the water sandpaper is 1200#, and the secondary grinding time is 8.5min.
[0086] Electrolytic polishing is carried out using an electrolytic polishing machine. The processing voltage of the electrolytic polishing machine is 38V. The processing time of the electrolytic polishing machine is 54s. The electrolyte used for electrolytic polishing is a mixture of ethanol, 2-butoxyethanol and perchloric acid. The volume ratio of ethanol, 2-butoxyethanol and perchloric acid is 7.5:1:2.6.
[0087] After the electrolytic polishing process, the electrolytically polished alloy needs to be cleaned by rinsing with clean water.
[0088] The etching treatment is carried out as follows: an etchant is dropped onto the polished surface of the electrolytically polished alloy, and the surface is etched for a certain period of time and then washed off.
[0089] The etchant is a mixture of hydrofluoric acid, nitric acid and pure water, the volume ratio of hydrofluoric acid, nitric acid and pure water is 1:11:22, the certain time is 80s, and pure water is used in the cleaning process.
[0090] Example 3
[0091] This embodiment provides a method for grain corrosion of a nickel-sulfur alloy, comprising:
[0092] The alloy to be tested is subjected to primary grinding, secondary grinding, electrolytic polishing and corrosion treatment in sequence to obtain an alloy sample, and the alloy sample is placed in a metallographic microscope to observe and analyze the grains.
[0093] The first grinding is done with water sandpaper, the roughness of the water sandpaper is 400#, and the grinding time is 5 minutes.
[0094] The secondary grinding is carried out with water sandpaper, the roughness of the water sandpaper is 1500#, and the secondary grinding time is 7 minutes.
[0095] Electrolytic polishing is carried out using an electrolytic polishing machine. The processing voltage of the electrolytic polishing machine is 40V. The processing time of the electrolytic polishing machine is 50s. The electrolyte used for electrolytic polishing is a mixture of ethanol, 2-butoxyethanol and perchloric acid. The volume ratio of ethanol, 2-butoxyethanol and perchloric acid is 8:1:3.
[0096] After the electrolytic polishing process, the electrolytically polished alloy needs to be cleaned by rinsing with clean water.
[0097] The etching treatment is carried out as follows: an etchant is dropped onto the polished surface of the electrolytically polished alloy, and the surface is etched for a certain period of time and then washed off.
[0098] The etchant is a mixture of hydrofluoric acid, nitric acid and pure water, the volume ratio of hydrofluoric acid, nitric acid and pure water is 1:12:23, the certain time is 60s, and pure water is used in the cleaning process.
[0099] Example 4
[0100] This embodiment provides a method for grain corrosion of nickel-sulfur alloy. The difference from Embodiment 1 is that the grinding time is 4 minutes, and the other parameters and test conditions are the same as those in Embodiment 1.
[0101] Example 5
[0102] This embodiment provides a method for grain corrosion of nickel-sulfur alloy. The difference from Embodiment 1 is that the grinding time is 7 minutes, and the other parameters and test conditions are the same as those in Embodiment 1.
[0103] Example 6
[0104] This embodiment provides a method for grain corrosion of nickel-sulfur alloy. The difference from Example 1 is that the processing voltage of the electrolytic polishing machine is 35V, and the other parameters and test conditions are the same as those in Example 1.
[0105] Example 7
[0106] This embodiment provides a method for grain corrosion of nickel-sulfur alloy. The difference from Example 1 is that the processing voltage of the electrolytic polishing machine is 42V, and the other parameters and test conditions are the same as those in Example 1.
[0107] Example 8
[0108] This embodiment provides a method for grain corrosion of a nickel-sulfur alloy. The difference from Embodiment 1 is that the processing time of the electrolytic polishing machine is 45 seconds, and the other parameters and test conditions are the same as those in Embodiment 1.
[0109] Example 9
[0110] This embodiment provides a method for grain corrosion of a nickel-sulfur alloy. The difference from Embodiment 1 is that the processing time of the electrolytic polishing machine is 65 seconds, and the other parameters and test conditions are the same as those in Embodiment 1.
[0111] Example 10
[0112] This embodiment provides a method for grain corrosion of a nickel-sulfur alloy. The difference from Embodiment 1 is that the volume ratio of ethanol, 2-butoxyethanol and perchloric acid is 6:1:1, and the other parameters and test conditions are the same as those in Embodiment 1.
[0113] Embodiment 11
[0114] This embodiment provides a method for grain corrosion of a nickel-sulfur alloy. The difference from Embodiment 1 is that the volume ratio of ethanol, 2-butoxyethanol and perchloric acid is 9:1:1.5, and the other parameters and test conditions are the same as those in Embodiment 1.
[0115] Example 12
[0116] This embodiment provides a method for grain corrosion of a nickel-sulfur alloy. The difference from Embodiment 1 is that the volume ratio of hydrofluoric acid, nitric acid and pure water is 1:10:18, and the other parameters and test conditions are the same as those in Embodiment 1.
[0117] Example 13
[0118] This embodiment provides a method for grain corrosion of nickel-sulfur alloy. The difference from Embodiment 1 is that the volume ratio of hydrofluoric acid, nitric acid and pure water is 1:13:30, and the other parameters and test conditions are the same as those in Embodiment 1.
[0119] Embodiment 14
[0120] This embodiment provides a method for grain corrosion of nickel-sulfur alloy. The difference from Embodiment 1 is that the titration time is 58 s, and the other parameters and test conditions are the same as those in Embodiment 1.
[0121] Embodiment 15
[0122] This embodiment provides a method for grain corrosion of nickel-sulfur alloy. The difference from Embodiment 1 is that the titration time is 93 s, and the other parameters and test conditions are the same as those in Embodiment 1.
[0123] Comparative Example 1
[0124] This comparative example provides a method for grain corrosion of a nickel-sulfur alloy. The difference from Example 1 is that there is no secondary grinding, and the other parameters and test conditions are the same as those of Example 1.
[0125] The alloy grains after treatment in the above-mentioned embodiment and comparative example were observed using a metallographic microscope, and the results are shown in Table 1 below:
[0126] Table 1 Observation results of alloy grains in Examples and Comparative Examples
[0127] Observations Example 1 The grain surface is uniform and flawless Example 2 The grain surface is uniform and flawless Example 3 The grain surface is uniform and flawless Example 4 There are scratches and black pits on the surface of the grain Example 5 There are scratches on the surface of the grain and more black pits Example 6 There are scratches on the surface of the grain and the surface turns black Example 7 There are scratches on the surface of the grain, and the surface becomes increasingly darker Example 8 There are scratches on the surface of the grain and the surface turns black Example 9 There are scratches on the surface of the grain, and the surface becomes increasingly darker Example 10 Poor grain display effect Embodiment 11 Poor grain display effect Example 12 The grains are not obvious and there are signs of blackening. Example 13 The grains are not obvious and there are signs of blackening. Embodiment 14 The grains are not obvious and there are signs of blackening. Embodiment 15 The grains are not obvious and the degree of blackening increases Comparative Example 1 The grains are not obvious, messy, and have signs of blackening
[0128] From Table 1 above, we know that:
[0129] The grain display effect in Examples 1-3 is better than that in Examples 4 and 5, because the present invention limits the grinding time to 5 to 6 minutes. Figure 1 , Figure 2 , Figure 3 , Figure 4 and Figure 5 As shown, if the sample grinding time is too short, scratches will appear on the surface, and if it is too long, water sandpaper particles will remain on the surface of the product, resulting in black pits in the metallographic image.
[0130] The grain display effect in Examples 1-3 is better than that in Examples 6 and 7, because the present invention limits the processing voltage of the electrolytic polishing machine to 36-40V. Figure 6 and Figure 7 As shown in the figure, if the voltage of the electrolytic polishing machine is too low, scratches cannot be removed, and if the voltage is too high, the surface of the product will turn black.
[0131] The grain display effect in Examples 1-3 is better than that in Examples 8 and 9, because the present invention limits the processing time of the electrolytic polishing machine to 50 to 60 seconds. Figure 8 and Fig. 9 As shown in the figure, if the polishing time is too low, the product surface will be scratched, and if it is too long, the product surface will turn black.
[0132] The grain display effect in Examples 1-3 is better than that in Examples 10 and 11, because the volume ratio of ethanol, 2-butoxyethanol and perchloric acid is limited to (7-8):1:(2-3). Fig.10 and Fig.11 As shown, although the polishing liquid that does not belong to this volume ratio can be polished, the grain display effect is poor.
[0133] The grain display effect in Examples 1-3 is better than that in Examples 12 and 13, because the volume ratio of hydrofluoric acid, nitric acid and pure water is limited to 1: (10-12): (20-23). Fig.12 and Fig.13 As shown, under the same titration time, if there is too much pure water, the product grains will not be obvious, and if there is too much acid, the product will be over-corroded and the grains will turn black.
[0134] The grain display effect in Examples 1-3 is better than that in Examples 14 and 15, because the present invention limits the titration time to 60 to 90 seconds. Fig.14 and Fig.15 As shown, under the same concentration of etching solution, if the titration time is too short, the product grains will not be obvious, and if the time is too long, the product will be over-corroded and the grains will turn black.
[0135] The grain display effect in Examples 1-3 is better than that in Comparative Example 1, because the present invention defines a specific method for grain corrosion, such as Fig.16 As shown, the display of the grains in the alloy is clearer, and the operation process of the overall method is stable and can be reused, the detection time is short, and the results can be obtained efficiently.
[0136] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
[0137] The present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for grain corrosion of nickel-sulfur alloy, It is characterized in that The grain corrosion method comprises: The alloy to be tested is subjected to primary grinding, secondary grinding, electrolytic polishing and corrosion treatment in sequence to obtain an alloy sample, and the alloy sample is placed in a metallographic microscope to observe and analyze the grains.
2. The grain etching method according to claim 1, It is characterized in that The primary grinding is performed using water sandpaper; The roughness of the water sandpaper is 200-400#; The time of one grinding is 5 to 6 minutes.
3. The grain etching method according to claim 1, It is characterized in that The secondary grinding is performed using water sandpaper; The roughness of the water sandpaper is 1000-1500#; The secondary grinding time is 7 to 10 minutes.
4. The grain etching method according to claim 1, It is characterized in that The electrolytic polishing is performed using an electrolytic polishing machine; The processing voltage of the electrolytic polishing machine is 36-40V; The processing time of the electrolytic polishing machine is 50 to 60 seconds.
5. The grain etching method according to claim 1, It is characterized in that The electrolyte used in the electrolytic polishing is a mixture of ethanol, 2-butoxyethanol and perchloric acid; The volume ratio of the ethanol, the 2-butoxyethanol and the perchloric acid is (7-8):1:(2-3).
6. The grain etching method according to claim 1, It is characterized in that After the electrolytic polishing process, the electrolytically polished alloy needs to be cleaned; The cleaning process is performed by flushing with clean water.
7. The grain etching method according to claim 1, It is characterized in that The corrosion treatment is carried out as follows: The etchant is dropped onto the polished surface of the electrolytically polished alloy, and then washed after etching for a certain period of time.
8. The grain etching method according to claim 7, It is characterized in that The etchant is a mixture of hydrofluoric acid, nitric acid and pure water; The volume ratio of the hydrofluoric acid, the nitric acid and the pure water is 1:(10-12):(20-23).
9. The grain etching method according to claim 7, It is characterized in that The certain time is 60 to 90 seconds; The cleaning process uses pure water.
10. The grain etching method according to claim 1, It is characterized in that The grain corrosion method specifically comprises: The alloy to be tested is subjected to primary grinding, secondary grinding, electrolytic polishing and corrosion treatment in sequence to obtain an alloy sample, and the alloy sample is placed in a metallographic microscope to observe and analyze the grains; The first grinding is performed using water sandpaper, the roughness of the water sandpaper is 200-400#, and the time of the first grinding is 5-6min; The secondary grinding is performed using water sandpaper, the roughness of the water sandpaper is 1000-1500#, and the secondary grinding time is 7-10min; The electrolytic polishing is performed by an electrolytic polishing machine, the processing voltage of the electrolytic polishing machine is 36-40V, the processing time of the electrolytic polishing machine is 50-60s, the electrolyte used in the electrolytic polishing is a mixed solution of ethanol, 2-butoxyethanol and perchloric acid, and the volume ratio of the ethanol, the 2-butoxyethanol and the perchloric acid is (7-8):1:(2-3); After the electrolytic polishing process, the electrolytically polished alloy needs to be cleaned, and the cleaning process is performed by flushing with clean water; The corrosion treatment is carried out as follows: dripping an etchant on the polished surface of the alloy after electrolytic polishing, etching for a certain period of time and then washing; The etching agent is a mixture of hydrofluoric acid, nitric acid and pure water, the volume ratio of the hydrofluoric acid, the nitric acid and the pure water is 1:(10-12):(20-23), the certain time is 60-90s, and pure water is used in the cleaning process.
Citation Information
Patent Citations
Metallographical corrosion method cleaning displaying austenite boundary of nickel base alloy
CN106908301A
Metallographic etchant and metallographic structure display method of nickel-titanium alloy
CN108663257A
Preparation method of NiV alloy metallographic specimen
CN111707513A
Crystal grain corrosion and display method of 304 stainless steel
CN118376616A
Method for observing microscopic structure of stainless steel
CN1916597A