N-type TOPCon battery front silver aluminum paste, preparation method thereof and battery
By using silver-aluminum paste composed of aluminum powder, silver powder, nano-alloy powder, etc., the problem of ejector pin printing in N-type TOPCon batteries during electroluminescence testing is solved, the filling efficiency and overall efficiency of the battery are improved, and lower contact is achieved resistivity and higher battery quality.
Patent Information
- Application Number
- CN202310327586.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing N-type TOPCon batteries use high-resistance dense gate technology, which causes problems with ejector pin marks during electroluminescence testing, affecting battery grade, yield and economic benefits.
The silver-aluminum paste is composed of aluminum powder, silver powder, nano-alloy powder, organic binder, glass powder and organic additives. The nano-alloy powder is nano-silver aluminum alloy powder, nano-aluminum boron alloy powder and nano-scale aluminum-silicon alloy powder. Prepared by grinding and dispersing technology to form an efficient front-side silver-aluminum paste, which reduces the sintering temperature and improves the contact between the silver-aluminum fine grid and the battery.
It effectively avoids the appearance of ejector pin marks, improves the filling efficiency and overall efficiency of the battery, reduces the contact resistivity, and improves the quality and economic benefits of the battery.
Smart Images

Figure CN118762860A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of crystalline silicon solar cell manufacturing, and in particular to an N-type TOPCon cell front silver-aluminum paste and a preparation method thereof and a cell. Background Art
[0002] Currently, N-type TOPCon cells in crystalline silicon solar cells are widely used due to their small attenuation, obvious advantages in overall cell efficiency and power generation.
[0003] In order to improve the efficiency of the battery, most of the existing N-type TOPCon batteries use a high-resistance dense grid technology solution. The front diffusion concentration is low, which increases the contact resistivity between the front silver-aluminum fine grid and the battery cell. As a result, the contact between the front silver-aluminum fine grid and the sintered mesh belt will show pin marks of different sizes during the electroluminescent (EL) test, affecting the battery grade, yield and economic benefits. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide an N-type TOPCon battery front silver aluminum paste and a preparation method thereof and a battery, so as to solve the problem that the existing N-type TOPCon battery is prone to ejector pin marks during EL testing due to the use of high-resistance dense grid technology.
[0005] In order to solve the above problems, the present invention is achieved through the following technical solutions:
[0006] The present invention proposes a silver-aluminum paste for the front side of an N-type TOPCon battery, wherein the components of the silver-aluminum paste include aluminum powder, silver powder, nano alloy powder, an organic binder, glass powder and an organic additive, wherein the nano alloy powder is one or more of nano silver aluminum alloy powder, nano aluminum boron alloy powder and nano-grade aluminum silicon alloy powder.
[0007] Furthermore, in the silver-aluminum paste of the front side of the N-type TOPCon battery, the mass fractions of the silver powder, aluminum powder, nano-alloy powder, organic binder, glass powder and organic additive are 78-84%, 1-3%, 0.1-0.5%, 9.7-19.6%, 1-2% and 0.3-0.8%, respectively.
[0008] Furthermore, in the silver-aluminum paste on the front side of the N-type TOPCon battery, the organic additive includes one or more of Digo 655, BYK109, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, laurel phosphate, silicone oil, and a mixture of dibasic acid esters.
[0009] Furthermore, in the silver-aluminum paste on the front side of the N-type TOPCon battery, the silver powder includes micron-spherical silver powder and nano-spherical silver powder, and the aluminum powder includes micron-spherical aluminum powder and nano-spherical aluminum powder.
[0010] Furthermore, in the silver-aluminum paste on the front side of the N-type TOPCon battery, the organic binder includes a high molecular polymer and an organic solvent;
[0011] The mass fraction of the high molecular weight polymer in the organic binder is 7 to 11%;
[0012] The mass fraction of the organic solvent in the organic binder is 89-93%.
[0013] Furthermore, in the silver-aluminum paste on the front side of the N-type TOPCon battery, the organic solvent is 4 or more of pineneol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85, alcohol ester twelve, turpentine, triethyl citrate, acetylated tributyl citrate, alcohol ester twelve, lecithin, and diethylene glycol ethyl ether.
[0014] Furthermore, in the silver-aluminum paste on the front side of the N-type TOPCon battery, the D50 of the glass powder is 1.2 to 1.8 μm.
[0015] Furthermore, in the silver-aluminum paste on the front side of the N-type TOPCon battery, the glass powder is obtained by sintering and crushing 20-25% Bi2O3, 6-8% Al2O3, 10-12% SiO2, 5-29% PbO, 15-20% Sb2O5, 5-8% B2O3, 15-22% TiO2, and 2-4% V2O5 by mass fraction.
[0016] The present invention also proposes a method for preparing a front silver-aluminum paste for an N-type TOPCon battery, which comprises:
[0017] Mixing silver powder, aluminum powder, nano alloy powder, organic binder and glass powder to obtain a mixture, wherein the nano alloy powder is one or more of nano silver aluminum alloy powder, nano aluminum boron alloy powder and nano aluminum silicon alloy powder;
[0018] After grinding the mixture, an organic additive is added to obtain the front silver-aluminum paste of the N-type TOPCon battery.
[0019] The present invention also provides an N-type solar cell, wherein a plurality of grid lines are attached to the front side of the N-type solar cell, and the grid lines are prepared by the above-mentioned silver-aluminum paste.
[0020] Compared with the prior art, the embodiments of the present invention have the following advantages:
[0021] In the embodiment of the present invention, the provided N-type TOPCon battery front silver aluminum paste comprises aluminum powder, silver powder, nano alloy powder, organic binder, glass powder and organic additive, wherein the nano alloy powder is one or more of nano silver aluminum alloy powder, nano aluminum boron alloy powder and nano aluminum silicon alloy powder. Because nano silver aluminum alloy powder, nano aluminum boron alloy powder and nano aluminum silicon alloy powder all have the characteristics of nanometer particle size, high tap density, low oxygen content and high activity, the front silver aluminum paste with the addition of the nano alloy powder can quickly form a good alloy with silicon under low sintering temperature conditions, reduce the contact resistivity between the front silver aluminum fine grid and the battery, not only avoid the occurrence of ejector pin marks during EL testing, but also improve the filling of the battery and the efficiency of the battery.
[0022] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a flow chart of a method for preparing silver-aluminum paste for the front side of an N-type TOPCon battery provided by an embodiment of the present invention;
[0024] Figure 2 It is a flow chart of a method for preparing silver-aluminum paste on the front side of an N-type TOPCon battery provided by another embodiment of the present invention. DETAILED DESCRIPTION
[0025] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0026] The applicant of the present invention has found that most of the existing N-TOPCon batteries adopt the technical solution of high-resistance dense grid to improve the efficiency of the battery, but it also brings the problem of low front diffusion concentration. The lower front diffusion concentration leads to a larger contact resistivity between the front silver-aluminum fine grid and the battery cell, so that the contact between the front silver-aluminum fine grid and the sintered mesh belt will show black spot-like ejector pin marks of different sizes during the EL test. The presence of ejector pin marks will not only cause battery degradation, but also affect the yield and economic benefits of the battery. Although the problem of severe ejector pin marks can usually be solved by increasing the sintering temperature, increasing the sintering temperature will seriously reduce the efficiency of the N-TOPCon battery, which is contrary to the original intention of using high-resistance dense grids.
[0027] In order to solve the above problems, an embodiment of the present invention provides a silver-aluminum paste for the front side of an N-type TOPCon battery, wherein the components constituting the silver-aluminum paste include aluminum powder, silver powder, nano alloy powder, an organic binder, glass powder and an organic additive, wherein the nano alloy powder is one or more of nano silver aluminum alloy powder, nano aluminum boron alloy powder and nano-grade aluminum silicon alloy powder.
[0028] Among them, silver powder and aluminum powder are the main components; glass powder is an inorganic adhesive, which will melt into liquid under high temperature conditions, and will condense when cooled to play a bonding role; organic adhesives can ensure the overall bonding effect; organic additives can reduce the overall viscosity of the silver paste; because nano silver aluminum alloy powder, nano aluminum boron alloy powder and nano aluminum silicon alloy powder have the characteristics of nanometer particle size, high tap density, low oxygen content and high activity, by adding the nano alloy powder, the front silver aluminum paste can quickly form a good alloy with silicon under lower sintering temperature conditions, reduce the contact resistivity between the front silver aluminum fine grid and the battery, not only avoid the occurrence of ejector pin marks during EL testing, but also improve the battery filling and battery efficiency, thereby effectively solving the problem of ejector pin marks in existing N-type TOPCon batteries due to the use of high-resistance dense grid technology during EL testing.
[0029] Optionally, the organic additives include one or more of Digo 655, BYK109, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl phosphate, silicone oil, and a mixture of dibasic acid esters.
[0030] In the silver-aluminum paste for the front side of the N-type TOPCon battery provided in an embodiment of the present invention, the mass fractions of silver powder, aluminum powder, nano-alloy powder, organic binder, glass powder and organic additive are 78-84%, 1-3%, 0.1-0.5%, 9.7-19.6%, 1-2% and 0.3-0.8%, respectively.
[0031] For example, in the silver-aluminum paste, the mass fractions of silver powder, aluminum powder, nano alloy powder, organic binder, glass powder and organic additive are 78%, 3%, 0.1%, 17.1%, 1% and 0.8% respectively.
[0032] For example, in the silver-aluminum paste, the mass fractions of silver powder, aluminum powder, nano alloy powder, organic binder, glass powder and organic additive are 84%, 1%, 0.5%, 12.2%, 2% and 0.3% respectively.
[0033] For example, in the silver-aluminum paste, the mass fractions of silver powder, aluminum powder, nano alloy powder, organic binder, glass powder and organic additive are 78%, 1%, 0.1%, 19.6%, 1% and 0.3% respectively.
[0034] For example, in the silver-aluminum paste, the mass fractions of silver powder, aluminum powder, nano alloy powder, organic binder, glass powder and organic additive are 84%, 3%, 0.5%, 9.7%, 2% and 0.8% respectively.
[0035] For example, in the silver-aluminum paste, the mass fractions of silver powder, aluminum powder, nano alloy powder, organic binder, glass powder and organic additive are 80%, 2%, 0.3%, 15.7%, 1.5% and 0.5% respectively.
[0036] Optionally, in one embodiment, the mass fraction of aluminum powder in the silver-aluminum paste on the front side of the N-type TOPCon battery is 1-3%.
[0037] In the embodiment of the present invention, the aluminum powder is composed of aluminum powder of different particle sizes (D50=1-5 microns). The combination of aluminum powder of different particle sizes can fully alleviate the action point of aluminum powder activity and glass powder, widen the sintering temperature of the slurry, and improve the average efficiency of the battery.
[0038] In an embodiment of the present invention, the glass powder includes B2O3, Al2O3, PbO, ZnO, BaO, Sb2O3, and SiO2.
[0039] Optionally, in one embodiment, the glass powder is obtained by sintering and crushing 20-25% Bi2O3, 6-8% Al2O3, 10-12% SiO2, 5-29% PbO, 15-20% Sb2O5, 5-8% B2O3, 15-22% TiO2, and 2-4% V2O5 by mass fraction. Among them, Bi2O3 is the main network structure; Al2O3 can adjust the glass stability and increase the viscosity; PbO can adjust the glass corrosion and reduce the glass melting point; Sb2O5 is used to clarify and uniform the glass liquid; SiO2 is used for glass network formation, promoting glass stability and increasing the glass melting point; TiO2 is used for local crystallization.; V2O5 is used to reduce the melting point.
[0040] Among them, D50 of glass powder is 1.2-1.8 μm. If D50 is less than 1.2 μm, the glass activity is too high, and if D50 is greater than 1.8 μm, the glass activity is too low.
[0041] In the silver-aluminum paste on the front side of the N-type TOPCon battery provided in the embodiment of the present invention, the aluminum powder includes micron-sized spherical aluminum powder and nano-sized spherical aluminum powder, and the silver powder includes micron-sized spherical silver powder and nano-sized spherical silver powder. Specifically, the aluminum powder includes micron-sized spherical aluminum powder with a purity of 3 nines and nano-sized spherical aluminum powder with a purity of 3 nines, and the silver powder includes micron-sized spherical silver powder with a purity of 3 nines and nano-sized spherical silver powder with a purity of 3 nines. In the embodiment of the present invention, the above-mentioned silver powder is a micron-sized spherical silver powder with a purity of 3 nines. Among them, because there are gaps between the micron-sized silver powder and the silver powder, and there are gaps between the micron-sized aluminum powder and the aluminum powder, the above-mentioned nano-sized spherical silver powder and the above-mentioned nano-sized spherical aluminum powder can just fill and penetrate into the gaps between the micron-sized ones.
[0042] Optionally, in one embodiment, the nano alloy powder comprises nano-scale spherical high-activity silver aluminum alloy powder with a purity of 2 nines.
[0043] In the silver-aluminum paste for the front side of the N-type TOPCon battery provided in the embodiment of the present invention, the organic binder comprises a polymer and an organic solvent; wherein the polymer is dissolved in the organic solvent so that the organic solvent can be used as an organic binder, that is, the paste plays a role of bonding the powder after drying.
[0044] Optionally, in one embodiment, the mass fraction of the high molecular polymer in the organic binder is 7-11%; the mass fraction of the organic solvent in the organic binder is 89-93%.
[0045] Optionally, in one embodiment, the high molecular weight polymer is one or more of acrylic resin or ethyl cellulose resin;
[0046] The above-mentioned organic solvent is 4 or more of pineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85, alcohol ester twelve, turpentine, triethyl citrate, acetylated tributyl citrate, alcohol ester twelve, lecithin, and diethylene glycol ethyl ether.
[0047] The embodiment of the present invention also provides a method for preparing silver-aluminum paste on the front side of an N-type TOPCon battery, such as Figure 1 As shown, it includes steps 101 to 102:
[0048] Step 101: Mix silver powder, aluminum powder, nano alloy powder, organic binder and glass powder to obtain a mixture, wherein the nano alloy powder is one or more of nano silver aluminum alloy powder, nano aluminum boron alloy powder and nano aluminum silicon alloy powder;
[0049] Step 102: Grind the mixture and add an organic additive to obtain the silver-aluminum paste for the front side of an N-type TOPCon battery.
[0050] In the above step 101, 78-84% of silver powder, 1-3% of aluminum powder, 0.1-0.5% of nano alloy powder, 9.7-19.6% of organic binder, and 1-2% of glass powder are weighed and mixed, accounting for 78-84% of the total mass of the raw materials, and dispersed by a disperser to obtain the above mixture.
[0051] In the above step 102, the above mixture is ground and then an organic additive accounting for 0.3-0.8% of the total mass of the raw materials is added, and after high-speed dispersion, the high-efficiency N-TOPCon front silver-aluminum paste with improved top pin printing is obtained.
[0052] Optionally, the silver powder includes micron spherical silver powder and nano spherical silver powder, and the aluminum powder includes micron spherical aluminum powder and nano spherical aluminum powder.
[0053] Optionally, in one embodiment, the step 101 includes: mixing the organic binder, nano silver powder, nano aluminum powder, and nano alloy powder, dispersing them using a disperser, adding micron silver powder, micron aluminum powder, and glass powder, and then dispersing them using a disperser to obtain the mixture.
[0054] Optionally, in the above preparation method, the organic additive includes one or more of Digo 655, BYK109, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl phosphate, silicone oil, and a mixture of dibasic acid esters.
[0055] Optionally, in the above preparation method, the silver powder includes micron spherical silver powder and nano spherical silver powder, and the aluminum powder includes micron spherical aluminum powder and nano spherical aluminum powder.
[0056] Optionally, in the above preparation method, the organic binder comprises a high molecular polymer and an organic solvent;
[0057] The mass fraction of the high molecular weight polymer in the organic binder is 7 to 11%;
[0058] The mass fraction of the organic solvent in the organic binder is 89-93%.
[0059] Optionally, in the above preparation method, the organic solvent is 4 or more of pineol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85, alcohol ester twelve, turpentine, triethyl citrate, acetylated tributyl citrate, alcohol ester twelve, lecithin, and diethylene glycol ethyl ether.
[0060] Optionally, in the above preparation method, D50 of the glass powder is 1.2-1.8 μm.
[0061] Optionally, in the above preparation method, the glass powder is obtained by sintering and crushing Bi2O3 with a mass fraction of 20-25%, Al2O3 with a mass fraction of 6-8%, SiO2 with a mass fraction of 10-12%, PbO with a mass fraction of 5-29%, Sb2O5 with a mass fraction of 15-20%, B2O3 with a mass fraction of 15-22%, TiO2 with a mass fraction of 2-4%.
[0062] The present invention also provides another method for preparing the front silver-aluminum paste of an N-type TOPCon battery. Figure 2 As shown, it includes steps 201 to 202:
[0063] Step 201, mixing nano alloy powder, organic binder, glass powder and organic additive to obtain a mixture; wherein the nano alloy powder is one or more of nano silver aluminum alloy powder, nano aluminum boron alloy powder and nano aluminum silicon alloy powder;
[0064] Step 202: Add silver powder and aluminum powder to the mixture, disperse and grind the mixture to obtain silver-aluminum paste for the front side of an N-type TOPCon battery.
[0065] In this embodiment, nano alloy powder, organic binder, glass powder and organic additives are mixed, and then silver powder and aluminum powder are added and ground to obtain the above-mentioned high-efficiency N-TOPCon front silver-aluminum paste with improved ejector pin print.
[0066] The present invention also proposes an N-type TOPCon cell, wherein a plurality of grid lines are attached to the front side of the N-type solar cell, and the grid lines are prepared from the above-mentioned silver-aluminum paste.
[0067] The present invention is described in detail below by way of examples.
[0068] Example 1
[0069] (1) Preparation of glass powder:
[0070] Weigh 22 parts of Bi2O3, 7 parts of Al2O3, 10 parts of SiO2, 20 parts of PbO, 18 parts of Sb2O5, 5 parts of B2O3, 15 parts of TiO2, and 3 parts of V2O5 by mass, mix them evenly with a mixer, sinter and crush them to obtain glass powder, whose D50 is 1.2-1.8 μm;
[0071] (2) Preparation of silver-aluminum paste on the front side of N-type TOPCon cells:
[0072] Weigh 78 parts of micron spherical silver powder with a purity of more than 3 9, 4 parts of nano spherical silver powder with a purity of more than 3 9, 1.5 parts of micron spherical aluminum powder with a purity of more than 3 9, 0.5 parts of nano spherical aluminum powder with a purity of more than 3 9, 0.2 parts of nano silver aluminum alloy powder, 13.8 parts of organic binder, and 1.5 parts of glass powder by mass, mix them evenly with a disperser, grind them with a three-roll grinder to less than 10 microns, and then add 0.5 parts of organic additives to obtain the silver aluminum paste for the front side of an N-type TOPCon battery;
[0073] Among them, organic additives include laurel phosphate and BYKl09;
[0074] The organic binder includes 8% by mass of a high molecular polymer and 92% by mass of an organic solvent;
[0075] The high molecular polymer is ethyl cellulose-N50, a polymer with low sintering residual viscoelastic modulus; and the organic solvent includes terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate and Span 85.
[0076] The silver-aluminum paste on the front side of the N-type TOPCon cell is screen-printed with 480 mesh on a single crystal N-TOPCon silicon wafer of 182mm×182mm to form a silver fine grid, which is then sintered in a sintering furnace with a peak sintering temperature of 766°C.
[0077] After sintering, the electrical properties tested were: open circuit voltage 0.715V, short circuit current 13.731A, fill factor 83.8%, photoelectric conversion efficiency 24.919%, EL ejector pin print ratio 0.02%, which is 2.32% lower than the conventional front silver aluminum paste EL ejector pin print ratio.
[0078] Example 2
[0079] (1) Preparation of glass powder:
[0080] Weigh 22 parts of Bi2O3, 7 parts of Al2O3, 10 parts of SiO2, 20 parts of PbO, 18 parts of Sb2O5, 5 parts of B2O3, 15 parts of TiO2, and 3 parts of V2O5 by mass, mix them evenly with a mixer, sinter and crush them to obtain glass powder, whose D50 is 1.2-1.8 μm;
[0081] (2) Preparation of silver-aluminum paste on the front side of N-type TOPCon cells:
[0082] Weigh 78 parts of micron spherical silver powder with a purity of more than 3 9, 3 parts of nano spherical silver powder with a purity of more than 3 9, 1.5 parts of micron spherical aluminum powder with a purity of more than 3 9, 1 part of nano spherical aluminum powder with a purity of more than 3 9, 0.3 parts of nano silver aluminum alloy powder, 14.1 parts of organic binder, and 1.5 parts of glass powder by mass, mix them evenly with a disperser, grind them to less than 10 microns with a three-roll grinder, and then add 0.6 parts of organic additives to obtain the silver aluminum paste for the front side of an N-type TOPCon battery;
[0083] Among them, organic additives include laurel phosphate and BYKl09;
[0084] The organic binder includes 8% by mass of a high molecular polymer and 92% by mass of an organic solvent;
[0085] The high molecular polymer is ethyl cellulose-N50, a polymer with low sintering residual viscoelastic modulus; and the organic solvent includes terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate and Span 85.
[0086] The silver-aluminum paste on the front side of the N-type TOPCon cell is screen-printed with 480 mesh on a single crystal N-TOPCon silicon wafer of 182mm×182mm to form a silver fine grid, which is then sintered in a sintering furnace with a peak sintering temperature of 772°C.
[0087] After sintering, the electrical properties tested were: open circuit voltage 0.716V, short circuit current 13.741A, fill factor 83.7%, photoelectric conversion efficiency 24.942%, EL ejector pin print ratio 0.01%, which is 2.55% lower than the conventional front silver aluminum paste EL ejector pin print ratio.
[0088] Example 3
[0089] (1) Preparation of glass powder:
[0090] Weigh 22 parts of Bi2O3, 7 parts of Al2O3, 10 parts of SiO2, 20 parts of PbO, 18 parts of Sb2O5, 5 parts of B2O3, 15 parts of TiO2, and 3 parts of V2O5 by mass, mix them evenly with a mixer, sinter and crush them to obtain glass powder, whose D50 is 1.2-1.8 μm;
[0091] (2) Preparation of silver-aluminum paste on the front side of N-type TOPCon cells:
[0092] Weigh 78 parts of micron spherical silver powder with a purity of more than 3 9, 3 parts of nano spherical silver powder with a purity of more than 3 9, 1.5 parts of micron spherical aluminum powder with a purity of more than 3 9, 1 part of nano spherical aluminum powder with a purity of more than 3 9, 0.3 parts of nano aluminum-boron alloy powder, 14.1 parts of organic binder, and 1.5 parts of glass powder by mass, mix them evenly with a disperser, grind them to less than 10 microns with a three-roll grinder, and then add 0.6 parts of organic additives to obtain the silver-aluminum paste for the front side of an N-type TOPCon battery;
[0093] Among them, organic additives include laurel phosphate and BYKl09;
[0094] The organic binder includes 8% by mass of a high molecular polymer and 92% by mass of an organic solvent;
[0095] The high molecular polymer is ethyl cellulose-N50, a polymer with low sintering residual viscoelastic modulus; and the organic solvent includes terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate and Span 85.
[0096] The silver-aluminum paste on the front side of the N-type TOPCon cell is screen-printed with 480 mesh on a single crystal N-TOPCon silicon wafer of 182mm×182mm to form a silver fine grid, which is then sintered in a sintering furnace with a peak sintering temperature of 765°C.
[0097] After sintering, the electrical properties tested were: open circuit voltage 0.7165V, short circuit current 13.685A, fill factor 83.85%, photoelectric conversion efficiency 24.903%, EL ejector pin print ratio 0.01%, which is 2.28% lower than the conventional front silver aluminum paste EL ejector pin print ratio.
[0098] Example 4
[0099] (1) Preparation of glass powder:
[0100] Weigh 22 parts of Bi2O3, 7 parts of Al2O3, 10 parts of SiO2, 20 parts of PbO, 18 parts of Sb2O5, 5 parts of B2O3, 15 parts of TiO2, and 3 parts of V2O5 by mass, mix them evenly with a mixer, sinter and crush them to obtain glass powder, whose D50 is 1.2-1.8 μm;
[0101] (2) Preparation of silver-aluminum paste on the front side of N-type TOPCon cells:
[0102] Weigh 78 parts of micron spherical silver powder with a purity of more than 3 9, 3 parts of nano spherical silver powder with a purity of more than 3 9, 1.5 parts of micron spherical aluminum powder with a purity of more than 3 9, 1 part of nano spherical aluminum powder with a purity of more than 3 9, 0.3 parts of nano-grade aluminum silicon alloy powder, 14.1 parts of organic binder, and 1.5 parts of glass powder by mass, mix them evenly with a disperser, grind them to less than 10 microns with a three-roll grinder, and then add 0.6 parts of organic additives to obtain the silver-aluminum paste for the front side of an N-type TOPCon battery;
[0103] Among them, organic additives include laurel phosphate and BYKl09;
[0104] The organic binder includes 8% by mass of a high molecular polymer and 92% by mass of an organic solvent;
[0105] The high molecular polymer is ethyl cellulose-N50, a polymer with low sintering residual viscoelastic modulus; and the organic solvent includes terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate and Span 85.
[0106] The silver-aluminum paste on the front side of the N-type TOPCon cell is screen-printed with 480 mesh on a single crystal N-TOPCon silicon wafer of 182mm×182mm to form a silver fine grid, which is then sintered in a sintering furnace with a peak sintering temperature of 770°C.
[0107] After sintering, the electrical properties tested were: open circuit voltage 0.7172V, short circuit current 13.722A, fill factor 83.56%, photoelectric conversion efficiency 24.908%, EL ejector pin print ratio 0.02%, which is 2.25% lower than the conventional front silver aluminum paste EL ejector pin print ratio.
[0108] Comparative Example 1
[0109] (1) Preparation of glass powder:
[0110] Weigh 22 parts of Bi2O3, 7 parts of Al2O3, 10 parts of SiO2, 20 parts of PbO, 18 parts of Sb2O5, 5 parts of B2O3, 15 parts of TiO2, and 3 parts of V2O5 by mass, mix them evenly with a mixer, sinter and crush them to obtain glass powder, whose D50 is 1.2-1.8 μm;
[0111] (2) Preparation of silver-aluminum paste on the front side of N-type TOPCon cells:
[0112] Weigh 78 parts of micron spherical silver powder with a purity of more than 3 9, 3 parts of nano spherical silver powder with a purity of more than 3 9, 1.5 parts of micron spherical aluminum powder with a purity of more than 3 9, 1 part of nano spherical aluminum powder with a purity of more than 3 9, 14.1 parts of organic binder, and 1.5 parts of glass powder by mass, mix them evenly with a disperser, grind them with a three-roll grinder to less than 10 microns, and then add 0.6 parts of organic additives to obtain the silver-aluminum paste for the front side of an N-type TOPCon battery;
[0113] Among them, organic additives include laurel phosphate and BYKl09;
[0114] The organic binder includes 8% by mass of a high molecular polymer and 92% by mass of an organic solvent;
[0115] The high molecular polymer is ethyl cellulose-N50, a polymer with low sintering residual viscoelastic modulus; and the organic solvent includes terpineol, butyl carbitol, butyl carbitol acetate, tributyl citrate and Span 85.
[0116] The silver-aluminum paste on the front side of the N-type TOPCon cell is screen-printed with 480 mesh on a single crystal N-TOPCon silicon wafer of 182mm×182mm to form a silver fine grid, which is then sintered in a sintering furnace with a peak sintering temperature of 772°C.
[0117] After sintering, the electrical properties tested were as follows: open circuit voltage 0.7143V, short circuit current 13.711, fill factor 83.8%, photoelectric conversion efficiency 24.858%, EL pin print ratio 0.05%.
[0118] Experimental data show that, compared with Comparative Example 1, the silver-aluminum paste on the front side of the N-type TOPCon battery provided in Examples 1 to 4 can effectively improve the battery efficiency and reduce the EL top pin print ratio while ensuring the fill factor.
[0119] In summary, in this embodiment, the provided N-type TOPCon battery front silver aluminum paste comprises aluminum powder, silver powder, nano alloy powder, organic binder, glass powder and organic additives, wherein the nano alloy powder is one or more of nano silver aluminum alloy powder, nano aluminum boron alloy powder and nano aluminum silicon alloy powder. Because nano silver aluminum alloy powder, nano aluminum boron alloy powder and nano aluminum silicon alloy powder all have the characteristics of nanometer particle size, high tap density, low oxygen content and high activity, the front silver aluminum paste with the addition of the nano alloy powder can quickly form a good alloy with silicon under low sintering temperature conditions, reduce the contact resistivity between the front silver aluminum fine grid and the battery, not only avoid the occurrence of ejector pin marks during EL testing, but also improve the filling of the battery and the efficiency of the battery.
[0120] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concept. Therefore, the claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present invention.
[0121] The above is a detailed introduction to the silver-aluminum paste for the positive side of an N-type TOPCon battery, its preparation method and the battery provided by the present invention. Specific examples are used in this article to illustrate the principle and implementation mode of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of the present invention, there will be changes in the specific implementation mode and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.
Claims
1. A silver-aluminum paste for the front side of an N-type TOPCon battery, characterized in that: The components constituting the silver-aluminum paste include aluminum powder, silver powder, nano alloy powder, organic binder, glass powder and organic additives, wherein the nano alloy powder is one or more of nano silver aluminum alloy powder, nano aluminum boron alloy powder and nano aluminum silicon alloy powder.
2. The front silver-aluminum paste of N-type TOPCon battery according to claim 1, characterized in that: The mass fractions of the silver powder, aluminum powder, nano alloy powder, organic binder, glass powder and organic additive are 78-84%, 1-3%, 0.1-0.5%, 9.7-19.6%, 1-2% and 0.3-0.8% respectively.
3. The front silver-aluminum paste for N-type TOPCon battery according to claim 1, characterized in that: The organic additives include one or more of Digo 655, BYK109, aluminate coupling agent, silane coupling agent, zirconium aluminate coupling agent, lauryl phosphate, silicone oil, and a mixture of dibasic acid esters.
4. The front silver-aluminum paste for N-type TOPCon battery according to claim 1, characterized in that: The silver powder includes micron spherical silver powder and nano spherical silver powder, and the aluminum powder includes micron spherical aluminum powder and nano spherical aluminum powder.
5. The front silver-aluminum paste for N-type TOPCon battery according to claim 1, characterized in that: The organic binder includes a high molecular polymer and an organic solvent; The mass fraction of the high molecular weight polymer in the organic binder is 7 to 11%; The mass fraction of the organic solvent in the organic binder is 89-93%.
6. The front silver-aluminum paste for N-type TOPCon battery according to claim 5, characterized in that: The organic solvent is 4 or more of pineneol, butyl carbitol, butyl carbitol acetate, tributyl citrate, Span 85, alcohol ester twelve, turpentine, triethyl citrate, acetylated tributyl citrate, alcohol ester twelve, lecithin, and diethylene glycol ethyl ether.
7. The silver-aluminum paste for the front side of an N-type TOPCon battery according to claim 1, characterized in that: The D50 of the glass powder is 1.2-1.8 μm.
8. The front silver-aluminum paste for N-type TOPCon battery according to claim 1, characterized in that: The glass powder is obtained by sintering and crushing 20-25% Bi2O3, 6-8% Al2O3, 10-12% SiO2, 5-29% PbO, 15-20% Sb2O5, 5-8% B2O3, 15-22% TiO2 and 2-4% V2O5 by mass fraction.
9. A method for preparing silver-aluminum paste for the front side of an N-type TOPCon battery, characterized in that: include: Mixing silver powder, aluminum powder, nano alloy powder, organic binder and glass powder to obtain a mixture, wherein the nano alloy powder is one or more of nano silver aluminum alloy powder, nano aluminum boron alloy powder and nano aluminum silicon alloy powder; After grinding the mixture, an organic additive is added to obtain the front silver-aluminum paste of the N-type TOPCon battery.
10. An N-type TOPCon battery, characterized in that: A plurality of grid lines are attached to the front side of the N-type TOPCon, and the grid lines are prepared by using the silver-aluminum paste described in any one of claims 1 to 8.
Citation Information
Patent Citations
Abrasion-resistant nanometer conductive silver paste
CN104575668A
Front silver paste for preparing PERC silicon solar cells
CN109659066A
Solar cell silver paste and preparation method thereof
CN112289480A
N-TOPCon front silver-aluminum paste, preparation method thereof and N-TOPCon battery
CN115705933A