Processing method of coreless arbitrary-layer packaging substrate
By plating an inert metal layer and a copper layer on the metal sheet, performing multiple laminations and circuit layer production, and using van der Waals force separation technology, the problem of material waste and high manufacturing cost of coreless arbitrary layer packaging substrates is solved, and the carrier board is realized recycling and efficient manufacturing.
Patent Information
- Application Number
- CN202410828848.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-11
AI Technical Summary
Existing preparation methods for coreless arbitrary layer packaging substrates require the use of disposable ultra-thin copper foil carrier boards, which results in material waste and high manufacturing costs. The depaneling process is complex and difficult to recycle.
A metal sheet is used as the carrier board, and an inert metal layer is first plated on the surface, and then a copper layer and an insulating layer are formed through chemical deposition. Multiple lamination and circuit layer production are performed, and the van der Waals force of the copper layer and the inert metal layer is used to combine. separation to achieve multiple recycling of the load-bearing plate.
It effectively reduces process manufacturing costs, solves the problems of difficulty in plate separation and material waste, improves manufacturing efficiency, and provides a new packaging substrate manufacturing method.
Smart Images

Figure CN118763002A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to packaging substrate technology, and in particular to a processing method for a coreless arbitrary-layer packaging substrate. Background Art
[0002] With the continuous development of information technology, mobile phones and various electronic products are becoming thinner and smaller. The thinning of electronic products has given rise to coreless packaging substrates, which are not only thinner than core packaging substrates, but also have superior electrical performance, providing new solutions for chips and devices with increasingly higher integration requirements. Since coreless boards can make the package size thinner and smaller, the processing efficiency is increased by 100%, which is an advantage that is difficult to obtain over traditional multi-layer packaging substrates. Therefore, they have broad application prospects.
[0003] The conventional preparation method of coreless arbitrary-layer packaging substrate needs to be based on a peelable CCL (Dummy copper-clad laminate, which only serves as the center board and has a 3μm or 5μm ultra-thin copper foil on it) with ultra-thin copper foil. After the outermost layer is pressed together, the boards are separated to obtain two identical arbitrary-layer packaging substrates. Although this method can effectively avoid the problem of insufficient line processing thin-plate capacity and improve manufacturing efficiency by 100%, because the ultra-thin copper foil of the CCL has been used as a conductor structure of the packaging substrate, the CCL cannot be recycled multiple times, resulting in material waste. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for processing a coreless arbitrary-layer packaging substrate, wherein the carrier plate used in the processing can be recycled multiple times, thereby reducing the manufacturing cost of the process.
[0005] In order to achieve the above-mentioned invention object, the technical scheme adopted is as follows:
[0006] A method for processing a coreless arbitrary layer packaging substrate comprises the following steps:
[0007] S1. A layer of inert metal is plated on the upper and back sides of the metal sheet to form a carrier plate;
[0008] S2. Depositing a copper layer on the upper and back sides of the carrier plate by chemical deposition to form a center plate, laying an insulating layer and a copper foil layer on the upper and lower sides of the center plate in sequence, and performing a high-temperature vacuum pressing process;
[0009] S3, making a via hole, and making a circuit layer on the copper foil layer, wherein the circuit layer is electrically connected to the copper layer through the via hole;
[0010] S4, laying an insulating layer and a copper foil layer on the circuit layer in sequence, performing a high-temperature vacuum pressing process, and repeating the step of S3 once;
[0011] S5, then repeat the step S4 multiple times to obtain a substrate having N upper and lower circuit layers, where N is an integer greater than 1;
[0012] S6, performing solder resist treatment on the circuit layer to form a solder resist layer, and then coating a protective layer at a position where no solder resist layer is provided;
[0013] S7, separating the carrier plate from the entire substrate, so as to obtain two coreless packaging substrates and the carrier plate.
[0014] The present invention adopts a metal sheet for the first time, and lays an inert metal layer on it by sputtering or evaporation to form a carrier board. The coated inert metal layer has a strong bonding force with the metal sheet substrate, and the inert metal layer will not be destroyed by the subsequent chemical deposition (the chemical deposition process involves the participation of acidic substances). Then, a copper layer is coated on the carrier board by chemical deposition to obtain a central plate of the substrate conductor. After several times of lamination of insulating materials and copper foil, and the circuit layer is made, a substrate with N upper and lower circuit layers is formed as a whole, where N is an integer greater than 1. Finally, the copper layer and the inert metal layer are only bonded by van der Waals force and are easy to separate, so that the board can be easily separated to obtain the carrier board and the coreless packaging substrate containing the copper layer at the bottom. The peeled carrier board can also be reused, which further reduces the manufacturing cost of the process and can solve the problems of difficult board separation and easy warping of the inherent process.
[0015] The processing method of a coreless arbitrary-layer packaging substrate provided by the present invention provides a new manufacturing method, idea and structure for the entire packaging substrate industry.
[0016] Furthermore, the surface roughness of the metal sheet is 0.05 μm, and the metal sheet is a copper sheet or a stainless steel sheet.
[0017] The present invention adopts a metal sheet with a surface roughness of 0.05 μm, which has excellent flatness, is conducive to plating an inert metal layer, and enhances the bonding force between the inert metal layer and the metal sheet substrate.
[0018] Furthermore, the inert metal is one of titanium, chromium, tungsten, silver or gold.
[0019] In the present invention, inert metals such as titanium, chromium, tungsten, silver, and gold are selected to obtain an inert metal layer through sputtering. The inert metal layer has a strong bonding strength with the substrate and is highly corrosion-resistant and will not be corroded by subsequent chemical deposition (the chemical deposition process involves acidic substances), thereby facilitating the formation of a recyclable carrier plate.
[0020] Furthermore, the thickness of the inert metal layer is 50 nm-2 μm.
[0021] Generally, when the base film layer is formed by using magnetron sputtering technology, the thickness of the base film layer is between 0.1 and 0.15 μm. The main function of the film layer is to provide sufficient bonding force between the metallization layer and the anodized insulating layer. Using magnetron sputtering technology, this bonding force can reach 1000N / c㎡, making the connection between the two layers more firm and stable. In addition, the inert metal layer also has good high-temperature thermal resistance properties, and can ensure that there is no foaming and peeling when the temperature is higher than 320℃ / 10s. Therefore, it is completely suitable for lead-free soldering technology for subsequent packaging substrate production.
[0022] In the present invention, firstly, the inert metals sputtered on the present invention are very expensive, and the thicker the layer, the higher the cost; secondly, the processing efficiency itself is very low, and the thicker the layer, the lower the production capacity. Therefore, the thickness of the inert metal layer of the present invention is selected to be 50nm-2μm, which can provide sufficient bonding strength between the inert metal layer and the substrate without being too costly.
[0023] Furthermore, the thickness of the copper layer is 0.4-2 μm. In the packaging substrate industry, the common copper layer thickness is 0.4-2 μm. Because it only serves to start conduction, it does not need to be too thick. The thicker it is, the lower the production capacity, the higher the cost, and it is not conducive to the production of fine circuits.
[0024] Furthermore, the copper foil layer has a thickness not exceeding 15 μm.
[0025] Furthermore, the protective layer is one of a nickel-gold layer, a nickel-silver layer, a nickel-silver-gold layer or a tin layer, and the thickness of the protective layer is 3-15 μm.
[0026] Furthermore, the temperature of the high-temperature pressing treatment is 150-240° C., and the vacuum degree is ≤30 mbar.
[0027] Furthermore, the solder resist layer is a solder resist ink layer, and the thickness of the solder resist ink layer is 10-40 μm.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The present invention adopts a metal sheet for the first time, and lays an inert metal layer on the upper and back sides thereof by sputtering or evaporation to form a carrier board. The coated inert metal layer has a strong bonding force with the metal sheet substrate, and the inert metal layer will not be destroyed by the subsequent chemical deposition (the chemical deposition process involves the participation of acidic substances). Then, a copper layer is coated on the carrier board by chemical deposition to obtain a center plate of the substrate conductor. After several times of lamination of insulating materials and copper foil, and the production of circuit layers, a substrate with N upper and lower circuit layers is formed, where N is an integer greater than 1. Finally, the copper layer and the inert metal layer are only bonded by van der Waals force and are easy to separate, so that the board can be easily separated, and the carrier board and the coreless packaging substrate containing the copper layer at the bottom are separated. The peeled carrier board can be reused, further reducing the manufacturing cost of the process, and solving the problems of difficult board separation and easy warping in the inherent process.
[0030] (2) The method provided by the present invention provides a new manufacturing method, idea and structure for the entire packaging substrate industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The present invention is a schematic flow chart of a method for processing a coreless arbitrary-layer packaging substrate.
[0032] Reference numerals:
[0033] 1. Carrier board; 11. Metal sheet; 12. Inert metal layer; 3. Insulation layer; 4. Copper foil layer; 5. Via hole; 7. Circuit layer; 8. Solder mask layer; 9. Protective layer; 10. Coreless package substrate. DETAILED DESCRIPTION
[0034] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0035] The metal sheets in the following embodiments are all copper sheets.
[0036] Example 1
[0037] like Figure 1 As shown, this embodiment provides a method for processing a coreless arbitrary layer packaging substrate, comprising the following steps:
[0038] S1, a 50nm inert metal layer 12 is plated on the upper and back sides of the metal sheet 11 to make a carrier plate 1;
[0039] In this step, the method of forming the inert metal layer 12 on the metal sheet 11 can be sputtering, evaporation or other methods. The inert metal layer thus applied has a strong bonding force with the metal sheet substrate. The inert metal is one of titanium, chromium, tungsten, silver or gold. The inert metal layer in this embodiment is a titanium layer.
[0040] S2. A 0.4 μm copper layer 21 is deposited on the upper and back surfaces of the carrier board 1 by chemical deposition to form a center board 2. An insulating layer 3 and a copper foil layer 4 are sequentially laid on the upper and lower surfaces of the center board 2, and a lamination process is performed at 150° C. and a vacuum of 15 mbar;
[0041] In this step, the insulating layer 3 is a PP layer with a thickness of 25-30 μm, and the copper foil layer 4 is a copper foil layer with a thickness of no more than 15 μm. In this embodiment, the thickness of the copper foil layer is 10 μm.
[0042] S3, making a via hole 5, and making a circuit layer 7 on the copper foil layer, wherein the circuit layer 7 and the copper layer 21 can be electrically connected through the via hole 5;
[0043] In this step, laser drilling and hole metallization processes can be used to make the via hole 5, which can specifically include: first, a laser drilling process is used to process a blind hole reaching the center plate 2 from the designed position on one side of the outer layer, wherein the window can be etched and opened at the designed position first, and then the laser drilling can be performed after the insulating layer is exposed, or the laser drilling can be performed directly at the designed position. Then, a copper plating process is used to form a thin copper plating layer on the hole wall of the blind hole as a basis for electroplating; finally, the via hole is filled with electroplating to obtain the via hole 5; wherein, the full-board electroplating process or the graphic electroplating process can be used for the hole filling electroplating. Optionally, the via hole 5 produced in this step can be one or more, and in this embodiment, it is more than one.
[0044] In this step, a pattern electroplating process may be used to form the circuit layer 7, and the specific process may include: film-lamination-exposure-development-film removal; wherein,
[0045] The film pasting is to paste an anti-plating film, such as an anti-plating dry film, on the surface of the copper foil layer 4;
[0046] Exposure is the process of transferring the circuit pattern on the film or other transparent material to the anti-coating film using ultraviolet rays emitted by the exposure machine;
[0047] Development is to place the whole after the above steps in a developer to remove the resist film that has not undergone photopolymerization reaction, and the remaining resist film is on the copper foil layer 4 to define the circuit pattern on the surface;
[0048] Film stripping is the process of removing the anti-plating film with a chemical solution.
[0049] After the above steps, the portion of the copper foil layer 4 that is not etched away forms a circuit layer 7. Optionally, the height of the circuit layer 7 is 12 μm.
[0050] S4-S5, None
[0051] S6, performing solder resist treatment on the circuit layer 7 to form a solder resist layer 8, and then coating a protective layer 9 at a position where the solder resist layer 8 is not provided;
[0052] In this step, the solder resist treatment is to set a solder resist layer 8 such as green oil on the top of the circuit layer 7 to protect the circuit layer 7; the protective layer 9 is plated to form a film layer at the part of the circuit layer 7 that needs to be exposed to the outside, so as to improve the surface performance, for example, electroplating hard gold or soft gold on the surface of the pad to form a gold-plated layer. In this embodiment, the thickness of the solder resist layer 8 is 10μm.
[0053] S7, separating the carrier plate 1 from the entire substrate, so as to obtain two coreless packaging substrates 10 and the carrier plate 1.
[0054] Example 2 (The specific operation process of each step is referred to Example 1 and will not be repeated one by one)
[0055] This embodiment provides a method for processing a coreless arbitrary layer packaging substrate, comprising the following steps:
[0056] S1. A 1 μm inert metal layer 12 is plated on the upper and back sides of the metal sheet 11. The inert metal layer in this embodiment is a titanium layer to form a carrier plate 1. S2. A 2 μm copper layer 21 is deposited on the upper and back sides of the carrier plate 1 by chemical deposition to form a center plate 2. An insulating layer 3 and a copper foil layer 4 are sequentially laid on the upper and lower sides of the center plate 2, and a lamination process is performed at 150° C. and a vacuum of 15 mbar.
[0057] S3, making a via hole 5, and making a circuit layer 7 on the copper foil layer, wherein the circuit layer 7 and the copper layer 21 can be electrically connected through the via hole 5;
[0058] S4-S5, None
[0059] S6, performing solder resist treatment on the circuit layer 7 to form a solder resist layer 8 with a thickness of 20 μm, and then coating a protective layer 9 at a position where the solder resist layer 8 is not provided;
[0060] S7, separating the carrier plate 1 from the entire substrate, so as to obtain two coreless packaging substrates and the carrier plate 1.
[0061] Example 3 (the specific operation process of each step is the same as that of Example 1)
[0062] This embodiment provides a method for processing a coreless arbitrary layer packaging substrate, comprising the following steps:
[0063] S1, a 50nm thick inert metal layer 12 is plated on the upper and back sides of the metal sheet 11, wherein the inert metal layer in this embodiment is a chromium layer, to form a carrier plate 1;
[0064] S2. A 2 μm copper layer 21 is deposited on the upper and back surfaces of the carrier board 1 by chemical deposition to form a center board 2. An insulating layer 3 and a copper foil layer 4 are laid on the upper and lower surfaces of the center board 2 in sequence, and a lamination process is performed at 150° C. and a vacuum of 15 mbar;
[0065] S3, making a via hole 5, and making a circuit layer 7 on the copper foil layer, wherein the circuit layer 7 and the copper layer 21 can be electrically connected through the via hole 5;
[0066] S4, repeatedly laying the insulating layer 3 and the copper foil layer 4 on the circuit layer 7 in sequence, and then repeating the step of S3 once to obtain a substrate having two upper and lower circuit layers;
[0067] S5, None
[0068] S6, performing solder resist treatment on the circuit layer 7 to form a solder resist layer 8 with a thickness of 15 μm, and then coating a protective layer 9 at a position where the solder resist layer 8 is not provided;
[0069] S7, separating the carrier plate 1 from the entire substrate, so as to obtain two coreless packaging substrates and the carrier plate 1.
[0070] Example 4 (the specific operation process of each step is referred to Example 1)
[0071] This embodiment provides a method for processing a coreless arbitrary layer packaging substrate, comprising the following steps:
[0072] S1, a 2 μm inert metal layer 12 is plated on the upper and back sides of the metal sheet 11. The inert metal layer in this embodiment is a tungsten layer to form a carrier plate 1;
[0073] S2, depositing a copper layer 21 on the upper and back sides of the carrier board 1 by chemical deposition to form a center board 2, laying an insulating layer 3 and a copper foil layer 4 on the upper and lower sides of the center board 2 in sequence, and performing a lamination process at 150° C. and a vacuum of 15 mbar;
[0074] S3, making a via hole 5, and making a circuit layer 7 on the copper foil layer, wherein the circuit layer 7 and the copper layer 21 can be electrically connected through the via hole 5;
[0075] S4, laying the insulating layer 3 and the copper foil layer 4 on the circuit layer 7 in sequence, and then repeating the step S3 once;
[0076] S5, then repeat step S4 three times to obtain a substrate with upper and lower circuit layers of 5;
[0077] S6, performing solder resist treatment on the circuit layer 7 to form a solder resist layer 8 with a thickness of 15 μm, and then coating a protective layer 9 at a position where no solder resist layer is provided;
[0078] S7, combining the carrier board 1 and the substrates with 2 upper and lower layers, so as to obtain two coreless packaging substrates and the carrier board 1.
[0079] Comparative Example
[0080] Patent CN106409688A discloses a method for manufacturing an arbitrary layer packaging substrate.
[0081] By comparing the manufacturing processes of Examples 1-4 and Comparative Example 1, it can be seen that the embodiments of the present invention utilize the characteristics that the copper layer and the inert metal layer are only bound by van der Waals force and are easy to separate, and it is very easy to separate the board, separating the carrier board and the coreless packaging substrate containing the copper layer at the bottom. Therefore, in addition to obtaining two packaging substrates, the present invention can also obtain a recyclable carrier board, which not only has a manufacturing efficiency of 100%, but also reduces the manufacturing cost of the process. In Comparative Example 1, the ultra-thin copper foil has been used as a conductor structure of the packaging substrate, resulting in the CCL being unable to be recycled multiple times, and there is a problem of material waste.
[0082] The embodiments provided by the present invention are described in detail above. Specific examples are used herein to describe the principles and implementation methods of the present invention, and the description of the above embodiments is only used to help understand the core idea of the present invention. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for processing a coreless arbitrary layer packaging substrate, characterized in that: The steps include: S1, coating an inert metal layer (12) on the upper and back sides of a metal sheet (11) to form a carrier plate (1); S2, depositing a copper layer (21) on the upper and back sides of the carrier plate (1) by chemical deposition to form a center plate (2), laying an insulating layer (3) and a copper foil layer (4) on the upper and lower sides of the center plate (2) in sequence, and performing a high-temperature vacuum pressing process; S3, making a via hole (5), and making a circuit layer (7) on the copper foil layer (4), wherein the circuit layer (7) is electrically connected to the copper layer (21) through the via hole (5); S4, laying an insulating layer (3) and a copper foil layer (4) on the circuit layer (7) in sequence, performing a high-temperature vacuum pressing process, and repeating the step of S3 once; S5, then repeat the step S4 multiple times to obtain a substrate having N upper and lower circuit layers, where N is an integer greater than 1; S6, performing solder resist treatment on the circuit layer (7) to form a solder resist layer (8), and then plating a protective layer (9) at a position where the solder resist layer (8) is not formed; S7, separating the carrier plate (1) from the entire substrate, thereby obtaining two coreless packaging substrates (10) and the carrier plate (1).
2. The processing method of the coreless arbitrary layer packaging substrate according to claim 1, characterized in that: The surface roughness of the metal sheet (11) is 0.05 μm, and the metal sheet is a copper sheet or a stainless steel sheet.
3. The processing method of the coreless arbitrary layer packaging substrate according to claim 1, characterized in that: The inert metal is one of titanium, chromium, tungsten, silver or gold.
4. The method for processing a coreless arbitrary layer packaging substrate according to claim 3, characterized in that: The thickness of the inert metal layer (12) is 50 nm-2 μm.
5. The method for processing a coreless arbitrary layer packaging substrate according to claim 1, characterized in that: The thickness of the copper layer (21) in step S2 is 0.4-2 μm.
6. The method for processing a coreless arbitrary layer packaging substrate according to claim 1, characterized in that: The copper foil layer (4) is a copper foil with a thickness not exceeding 15 μm.
7. The method for processing a coreless arbitrary layer packaging substrate according to claim 1, characterized in that: The protective layer (9) is one of a nickel-gold layer, a nickel-silver layer, a nickel-silver-gold layer or a tin layer.
8. The method for processing a coreless arbitrary layer packaging substrate according to claim 1, characterized in that: The temperature of the high-temperature vacuum pressing process is 150-240° C., and the vacuum degree is ≤30 mbar.
9. The method for processing a coreless arbitrary layer packaging substrate according to claim 1, characterized in that: The solder resist layer (8) is a solder resist ink layer.
Citation Information
Patent Citations
Processing method of ultrathin coreless package substrate and structure
CN106409688A