Diaphragm, battery and preparation method thereof
By using a core-shell structure modified resin binder layer in the lithium battery separator, the energy consumption and cost problems caused by the hot pressing process in the preparation of the lithium battery separator are solved, achieving efficient battery manufacturing and meeting environmental protection requirements.
Patent Information
- Application Number
- CN202410756436.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-11
AI Technical Summary
Existing lithium battery separators require a hot pressing process during the preparation process, which leads to increased energy consumption and equipment costs, and does not comply with environmental protection policies.
Modified resin with a core-shell structure is used as the adhesive layer material. The difference in glass transition temperature of the modified resin is used to achieve the bonding of the separator and the pole piece under cold pressing or hot pressing, replacing traditional thermoplastics such as PVDF and PMMA. Material.
It reduces the energy consumption and equipment cost of the hot-pressing process during the cell preparation process, which complies with environmental protection policies. It also improves the adhesion between the separator and the pole piece, achieving efficient battery manufacturing.
Smart Images

Figure BDA0004889646310000141 
Figure BDA0004889646310000151 
Figure BDA0004889646310000161
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a diaphragm, a battery, and a method for preparing the same. Background Art
[0002] As a crucial component of lithium-ion batteries, the separator blocks the passage of electrons while allowing the free movement of lithium ions, thereby preventing contact between the positive and negative electrodes and causing a short circuit. Commercially available separator base materials are primarily polyolefin (PO) separators, primarily made of polyethylene (PE) and polypropylene (PP). Because separator base films inherently have poor heat resistance, they are typically coated with a heat-resistant layer (such as alumina or boehmite) to improve their heat resistance.
[0003] However, the diaphragm base film and the diaphragm with heat-resistant layer are not bonded to the pole piece, which cannot improve the hardness of the battery. To this end, an adhesive layer (glue layer) needs to be applied to the base film or heat-resistant layer. Currently, the diaphragm glue coating process is gradually maturing. For example, PVDF (polyvinylidene fluoride) and PMMA (polymethyl methacrylate) are coated on the PE base film or the CCS (aluminum oxide) coating of the PE film. The battery cell is then wound and pre-pressed and hot-pressed to improve the adhesion between the pole piece and the diaphragm, thereby improving the stiffness of the battery cell and reducing the scratch rate when the battery cell is inserted into the shell.
[0004] However, due to the hot melt adhesive properties of PVDF, PMMA adhesives, etc., a hot pressing process is required during the preparation of battery cells. The hot pressing process causes a serious increase in energy consumption and equipment costs. At the same time, this process is not in line with the country's dual carbon (the abbreviation for carbon peak and carbon neutrality) policy. Summary of the Invention
[0005] In view of this, the present invention provides a diaphragm and a battery and a method for preparing the same. The diaphragm can reduce the energy consumption and equipment cost of the hot pressing process during the preparation of the battery cell.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] In a first aspect, the present invention provides a diaphragm, comprising a base film layer, and an adhesive layer disposed on at least one surface of the base film layer;
[0008] The adhesive layer includes a modified resin and an adhesive;
[0009] The modified resin has a core-shell structure, wherein the core of the modified resin comprises a resin matrix and the shell of the modified resin comprises a grafted monomer;
[0010] The glass transition temperature of the resin matrix is -25℃~10℃;
[0011] The glass transition temperature of the grafted monomer is 90°C to 150°C.
[0012] In an embodiment of the present invention, the resin matrix includes at least one of ethylene-vinyl acetate copolymer (EVA) and vinyl acetate-acrylate copolymer.
[0013] In an embodiment of the present invention, the grafting monomer includes at least one of maleic anhydride, glycidyl methacrylate, and 2-methylbutenedioic anhydride.
[0014] Preferably, the mass percentage of the grafting monomer in the modified resin is 8% to 15%.
[0015] Preferably, the average particle size of the modified resin is 2 to 3 μm.
[0016] Preferably, in the adhesive layer, the mass percentage of the modified resin is 80% to 90%, and the mass percentage of the adhesive is 10% to 20%.
[0017] In an embodiment of the present invention, the binder includes but is not limited to at least one of acrylic acid-acrylonitrile copolymer (PAA-PAN), polyacrylic acid, polyacrylonitrile (PAN), and polyvinyl alcohol (PVA).
[0018] As a preference, the coating amount of the adhesive layer on the base film layer is 0.2 to 0.4 g / m 2 .
[0019] In an embodiment of the present invention, the base membrane layer includes a base membrane or a base membrane composited with a ceramic layer.
[0020] In an embodiment of the present invention, in the base film composited with the ceramic layer, the ceramic layer is provided on at least one surface of the base film.
[0021] In a second aspect, the present invention provides a method for preparing the above-mentioned diaphragm, comprising the following steps:
[0022] Step (1), mixing the modified resin, the binder and the solvent, and performing a dispersion treatment to obtain a binder slurry;
[0023] Step (2) is to apply the adhesive slurry to at least one surface of the base film layer and dry it to obtain a diaphragm.
[0024] In a third aspect, the present invention provides a battery comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator comprises the above-mentioned separator and / or the separator obtained by the above-mentioned preparation method, and the separator is arranged between the positive electrode sheet and the negative electrode sheet.
[0025] In a fourth aspect, the present invention provides a method for preparing the above-mentioned battery, comprising the following steps:
[0026] Step (1), stacking a positive electrode sheet, a separator, and a negative electrode sheet to obtain a battery cell, or stacking a positive electrode sheet, a separator, and a negative electrode sheet and then winding them to obtain a battery cell;
[0027] Step (2), cold pressing or hot pressing the battery cell.
[0028] Preferably, the temperature of the cold pressing treatment is 15-25° C., the pressure is 5-10 MPa, and the time is 20-30 seconds.
[0029] Preferably, the temperature of the hot pressing treatment is 80-100° C., the pressure is 3-8 MPa, and the time is 20-30 seconds.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The present invention introduces a modified resin with a core-shell structure into the adhesive layer of the diaphragm to replace the currently commonly used thermoplastic materials such as PVDF and PMMA as adhesives. This modified resin has a resin matrix with a low glass transition temperature, good adhesiveness at room temperature, and good flexibility as the core. A monomer with a high glass transition temperature and no adhesiveness at room temperature is grafted onto the molecular chain of the resin matrix to form a core-shell structure. This structure has the following advantages:
[0032] On the one hand, in the absence of external force, the grafted monomer shell layer can maintain the structure of the resin matrix and wrap the sticky resin matrix inside the core-shell structure to prevent the separator from rolling up and sticking to each other;
[0033] On the other hand, under the action of external force (such as cold pressing or hot pressing of the diaphragm), the shell layer of the modified resin is crushed, exposing the inner resin matrix, thereby improving the bonding strength between the diaphragm and the electrode.
[0034] Therefore, the diaphragm of the present invention does not need to be hot pressed, and only cold pressed can be performed to achieve bonding between the diaphragm and the electrode, which reduces energy consumption and equipment costs and complies with the country's dual carbon policy.
[0035] (2) When ethylene-vinyl acetate copolymer (EVA) is selected as the resin matrix, the vinyl acetate component in EVA has a very high affinity with the electrolyte and can still maintain a high adhesion (i.e., wet adhesion) in the electrolyte environment. DETAILED DESCRIPTION
[0036] The present invention discloses a diaphragm and a battery and methods for preparing the same. Those skilled in the art may refer to the contents herein and appropriately modify the process parameters to achieve the desired results. It is particularly important to note that all similar substitutions and modifications obvious to those skilled in the art are considered encompassed by the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel will readily be able to modify or appropriately alter and combine the methods and applications described herein to implement and apply the technology of the present invention without departing from the content, spirit, and scope of the present invention.
[0037] Explanation of terms:
[0038] The glass transition temperature (Tg) refers to the temperature at which a material transitions from a glassy state to a highly elastic state. The glass transition is an inherent property of amorphous polymer materials and a macroscopic manifestation of the change in the polymer's motion pattern. It directly affects the material's performance and processing properties. The glass transition temperature is the lowest temperature at which molecular chains can move, and its level is directly related to the flexibility of the molecular chain. The more flexible the molecular chain, the lower the glass transition temperature; the more rigid the molecular chain, the higher the glass transition temperature. The glass transition temperature is one of the characteristic temperatures of polymers. Above the glass transition temperature, polymers exhibit elasticity, while below the glass transition temperature, they become brittle.
[0039] Grafting refers to the reaction of adding appropriate side chains or functional groups to a macromolecular chain through chemical bonds. The resulting product is called a graft copolymer. The grafting formula of a polymer mainly consists of a resin, a grafting monomer, an initiator, and an antioxidant.
[0040] A grafted monomer refers to a molecule that is attached (eg, chemically bonded) to a polymer as a side chain but is not polymerized or copolymerized as part of the polymer backbone.
[0041] The resin matrix refers to the resin component used to form the main body of the modified resin.
[0042] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms can mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A can include a single element or multiple elements. Item B can include a single element or multiple elements. Item C can include a single element or multiple elements.
[0043] The endpoints of the ranges and any values disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range or the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.
[0044] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0045] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0046] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0047] In order to reduce the energy consumption and equipment cost of the hot pressing process during the preparation of the battery cell, the present invention adopts the following technical solutions:
[0048] In a first aspect, the present invention provides a diaphragm, comprising a base film layer, and an adhesive layer disposed on at least one surface of the base film layer;
[0049] The adhesive layer includes a modified resin and an adhesive;
[0050] The modified resin has a core-shell structure, wherein the core of the modified resin comprises a resin matrix and the shell of the modified resin comprises a grafted monomer;
[0051] The glass transition temperature of the resin matrix is -25℃~10℃;
[0052] The glass transition temperature of the grafted monomer is 90°C to 150°C.
[0053] In an embodiment of the present invention, the glass transition temperature of the resin matrix is exemplarily any one of -25°C, -20°C, -15°C, -10°C, -5°C, 0°C, 5°C, 10°C, or any value within a range consisting of any two of the above values. Preferably, it is -5°C to 0°C.
[0054] In an embodiment of the present invention, the glass transition temperature of the grafted monomer is illustratively any one of 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, and 150°C, or any value within a range consisting of any two of the above values. Preferably, it is 100°C to 140°C.
[0055] In an embodiment of the present invention, the resin matrix includes at least one of ethylene-vinyl acetate copolymer (EVA) and vinyl acetate-acrylate copolymer.
[0056] In an embodiment of the present invention, the grafting monomer includes at least one of maleic anhydride, glycidyl methacrylate, and 2-methylbutenedioic anhydride.
[0057] Preferably, the mass percentage of the grafted monomer in the modified resin is 8% to 15%. Exemplarily, the mass percentage of the grafted monomer in the modified resin is any one of 8%, 9%, 10%, 11%, 12%, 13%, 14%, and 15%, or any value within the range of any two of the above values. When the mass percentage of the grafted monomer in the modified resin is greater than 15%, when cold pressing or hot pressing is performed during the preparation of the battery cell, the shell of the modified resin is not easily crushed, and the sticky resin matrix cannot be exposed, resulting in a decrease in the viscosity of the adhesive layer, thereby affecting the bonding force between the diaphragm and the electrode; when the mass percentage of the grafted monomer in the modified resin is less than 8%, the modified resin directly exposes more resin matrix, and when the diaphragm is rolled up during the preparation of the diaphragm, the diaphragms will stick together.
[0058] Preferably, the average particle size of the modified resin is 2 to 3 μm. Exemplarily, the average particle size of the modified resin is any one of 2 μm, 2.1 μm, 2.2 μm, 2.3 μm, 2.4 μm, 2.5 μm, 2.6 μm, 2.7 μm, 2.8 μm, 2.9 μm, and 3 μm, or any value within the range of any two of the above values. When the average particle size of the modified resin is less than 2 μm, the shell of the modified resin is not easily crushed during the cold pressing operation in the battery cell preparation process, and the sticky resin matrix cannot be exposed, resulting in a decrease in the viscosity of the adhesive layer, thereby affecting the bonding force between the diaphragm and the electrode; when the average particle size of the modified resin is greater than 3 μm, the diaphragm will be too thick, which will easily lead to serious misalignment of the pole piece, affecting the quality of the battery cell and the electrical and safety performance of the battery.
[0059] Preferably, in the adhesive layer, the mass percentage of the modified resin is 80% to 90%, and the mass percentage of the binder is 10% to 20%. Exemplarily, the mass percentage of the modified resin in the adhesive layer is any value among 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, or any value within the range consisting of any two of the above values. Exemplarily, the mass percentage of the binder in the adhesive layer is any value among 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, or any value within the range consisting of any two of the above values.
[0060] In embodiments of the present invention, the binder includes, but is not limited to, at least one of acrylic acid-acrylonitrile copolymer (PAA-PAN), polyacrylic acid, polyacrylonitrile (PAN), and polyvinyl alcohol (PVA). The binder serves to adhere the modified resin to the base film layer, forming an adhesive layer on the surface of the base film layer. Acrylic acid-acrylonitrile copolymer (PAA-PAN) is preferred.
[0061] As a preference, the coating amount of the adhesive layer on the base film layer is 0.2 to 0.4 g / m 2 For example, the coating amount of the adhesive layer on the base film layer is 0.2 g / m 2 , 0.22g / m 2 , 0.24g / m 2 , 0.26g / m 2 , 0.28g / m 2 , 0.3g / m 2 , 0.32g / m 2 , 0.34g / m 2 , 0.36g / m 2 , 0.38g / m 2 , 0.4g / m 2 Any value in or any value within the range consisting of any two of the above values.
[0062] In an embodiment of the present invention, the base membrane layer includes a base membrane or a base membrane composited with a ceramic layer.
[0063] In an embodiment of the present invention, in the base film composited with the ceramic layer, the ceramic layer is provided on at least one surface of the base film.
[0064] In an embodiment of the present invention, the base film is at least one selected from a polyethylene film, a polypropylene film, a polyimide film, a polyvinylidene fluoride film, a polyvinylidene fluoride-hexafluoropropylene film, a polyamide film, and a polyethylene terephthalate film.
[0065] In an embodiment of the present invention, the ceramic layer comprises a ceramic material.
[0066] In an embodiment of the present invention, the ceramic material includes at least one of alumina, boehmite, calcium carbonate, hydrotalcite, montmorillonite, titanium dioxide, silicon dioxide, zirconium dioxide, magnesium oxide, magnesium hydroxide, magnesium hydroxide, boron nitride, silicon nitride, aluminum nitride, titanium nitride, boron carbide, silicon carbide, and zirconium carbide.
[0067] In a second aspect, the present invention provides a method for preparing the above-mentioned diaphragm, comprising the following steps:
[0068] Step (1), mixing the modified resin, the binder and the solvent, and performing a dispersion treatment to obtain a binder slurry;
[0069] Step (2) is to apply the adhesive slurry to at least one surface of the base film layer and dry it to obtain a diaphragm.
[0070] In an embodiment of the present invention, the solvent is water.
[0071] In an embodiment of the present invention, the rotation speed of the dispersion treatment is 2000-2500 r / min, and the time is 30-60 min.
[0072] Preferably, the binder slurry has a solid content of 7% to 10%, a viscosity of 30 to 80 mPa·s, and a pH of 6 to 8. The solid content of the binder slurry can be adjusted by changing the amount of solvent used.
[0073] In an embodiment of the present invention, the coating method includes spray coating and / or roller coating.
[0074] In an embodiment of the present invention, the drying temperature is 50-60°C.
[0075] In a third aspect, the present invention provides a battery comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator comprises the above-mentioned separator and / or the separator obtained by the above-mentioned preparation method, and the separator is arranged between the positive electrode sheet and the negative electrode sheet.
[0076] In an embodiment of the present invention, the adhesive layer is disposed on at least one surface of the base film layer, and preferably the adhesive layer is disposed on both sides of the base film layer.
[0077] In an embodiment of the present invention, when the adhesive layer is provided on one surface of the base film layer, it is preferred that the adhesive layer of the separator is in contact with the positive electrode sheet.
[0078] In an embodiment of the present invention, the battery comprises a lithium ion battery or a sodium ion battery.
[0079] In an embodiment of the present invention, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on at least one side of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, a positive electrode conductor and a positive electrode binder.
[0080] In an embodiment of the present invention, the mass percentage of each component in the positive electrode active material layer is: 80 wt% to 99.8 wt% of positive electrode active material, 0.1 wt% to 10 wt% of positive electrode conductor, and 0.1 wt% to 10 wt% of positive electrode binder.
[0081] In an embodiment of the present invention, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on at least one side of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, a negative electrode conductor and a negative electrode binder.
[0082] In an embodiment of the present invention, the mass percentage content of each component in the negative electrode active material layer is as follows: 80 wt% to 99.8 wt% of negative electrode active material, 0.1 wt% to 10 wt% of negative electrode conductive agent, and 0.1 wt% to 10 wt% of negative electrode binder.
[0083] In an embodiment of the present invention, the positive electrode conductive agent or the negative electrode conductive agent includes, but is not limited to, at least one of conductive carbon black, acetylene black, Ketjen black, conductive graphite, conductive carbon fiber, carbon nanotube, metal powder, and carbon fiber.
[0084] In an embodiment of the present invention, the positive electrode binder or the negative electrode binder includes, but is not limited to, at least one of sodium carboxymethyl cellulose, styrene-butadiene latex, polytetrafluoroethylene, and polyethylene oxide.
[0085] In an embodiment of the present invention, the positive electrode active material is selected from one or more of transition metal lithium oxides, lithium iron phosphate, and lithium-rich manganese-based materials.
[0086] In another embodiment of the present invention, the positive electrode active material includes at least one of layered transition metal sodium oxides, sodium vanadium phosphate, sodium fluorovanadate, sodium cobaltate, sodium manganate, sodium nickelate, and Prussian blue.
[0087] In an embodiment of the present invention, the negative electrode active material includes carbon-based negative electrode materials.
[0088] In an embodiment of the present invention, the carbon-based negative electrode materials include at least one of artificial graphite, natural graphite, mesocarbon microbeads, hard carbon, and soft carbon.
[0089] In an embodiment of the present invention, the negative electrode active material may further include silicon-based negative electrode materials.
[0090] In an embodiment of the present invention, the silicon-based negative electrode materials are selected from at least one of nano-silicon, silicon oxide negative electrode materials (SiO x (0 < x < 2)), or silicon-carbon negative electrode materials.
[0091] This application does not particularly limit the preparation methods of the positive electrode sheet and the negative electrode sheet. Those skilled in the art can adopt conventional preparation methods as long as the purposes of this application can be achieved.
[0092] In an embodiment of the present invention, the battery further includes an outer package.
[0093] In an embodiment of the present invention, the battery further includes an electrolyte.
[0094] This application does not particularly limit the organic solvents, electrolyte salts, and additives in the electrolyte. Those skilled in the art can select according to actual needs as long as the purposes of this application can be achieved.
[0095] In a fourth aspect, the present invention provides a method for preparing the above-mentioned battery, comprising the following steps:
[0096] Step (1), stacking a positive electrode sheet, a separator, and a negative electrode sheet to obtain a battery cell, or stacking a positive electrode sheet, a separator, and a negative electrode sheet and then winding them to obtain a battery cell;
[0097] Step (2), cold pressing or hot pressing the battery cell.
[0098] Preferably, the temperature of the cold press treatment is 15 to 25°C, the pressure is 5 to 10 MPa, and the time is 20 to 30 seconds. Exemplarily, the temperature of the cold press treatment is any one of 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, and 25°C, or any value within the range of any two of the above values, such as the temperature at room temperature. Exemplarily, the pressure of the cold press treatment is any one of 5MPa, 6MPa, 7MPa, 8MPa, 9MPa, and 10MPa, or any value within the range of any two of the above values. Exemplarily, the time of the cold press treatment is any one of 20s, 22s, 24s, 26s, 28s, and 30s, or any value within the range of any two of the above values.
[0099] Preferably, the temperature of the hot pressing treatment is 80-100°C, the pressure is 3-8 MPa, and the time is 20-30 seconds. Exemplarily, the temperature of the hot pressing treatment is any one of 80°C, 82°C, 84°C, 86°C, 88°C, 90°C, 92°C, 94°C, 96°C, 98°C, and 100°C, or any value within the range of any two of the above values. Exemplarily, the pressure of the hot pressing treatment is any one of 3MPa, 4MPa, 5MPa, 6MPa, 7MPa, and 8MPa, or any value within the range of any two of the above values. Exemplarily, the time of the hot pressing treatment is any one of 20s, 22s, 24s, 26s, 28s, and 30s, or any value within the range of any two of the above values.
[0100] In an embodiment of the present invention, after the cold pressing treatment or the hot pressing treatment, the process further includes: placing the battery cell in an outer package, and injecting electrolyte into the outer package to obtain the battery of the present invention.
[0101] In the following examples, the glass transition temperatures of the materials used are specifically:
[0102] Ethylene-vinyl acetate copolymer: 0℃;
[0103] Vinyl acetate-acrylate copolymer: -5°C;
[0104] Maleic anhydride: 140℃;
[0105] Glycidyl methacrylate: 100℃;
[0106] 2-Methylbutenedioic anhydride: 140°C.
[0107] The reagents, instruments and materials used in the present invention can be obtained through commercial channels.
[0108] Among them, modified resins such as maleic anhydride-modified EVA resin, glycidyl methacrylate-modified EVA resin, 2-methylbutenedioic anhydride-modified EVA resin, and maleic anhydride-modified vinyl acetate-acrylate copolymer resin are all obtained through commercial channels; they can also be prepared by conventional melt grafting methods.
[0109] The present invention will be further described below in conjunction with the embodiments:
[0110] Example 1:
[0111] 1. The raw material composition of the diaphragm in this embodiment:
[0112] (1) Modified resin: 85 parts of maleic anhydride modified EVA resin;
[0113] (2) Binder solution: 100 parts of a PAA-PAN binder having a solid content of 15%; the PAA-PAN binder comprises 15 parts of an acrylic acid-acrylonitrile copolymer (PAA-PAN) and 85 parts of water;
[0114] (3) Solvent: 1150 parts of water.
[0115] The grafted monomer (maleic anhydride) in the modified resin accounts for 10% by weight, and the average particle size of the modified resin is 2.5 μm.
[0116] 2. Preparation method of the diaphragm in this embodiment:
[0117] (1) The modified resin, binder solution, and solvent were mixed and dispersed at high speed (2500 r / min, 30 min) to obtain a binder slurry with a solid content of 8.3%, a viscosity of 60.8 mPa·s, and a pH of 7.34;
[0118] (2) The adhesive slurry was sprayed on the base film surface and CCS (Ceramic Coated Separator) surface of the diaphragm (purchased from Shanghai Enjie New Materials Technology Co., Ltd., i.e., the base film layer), and dried at 50°C to obtain a diaphragm with a composite adhesive layer. The single-side coating amount of the adhesive layer on the base film layer was 0.3 g / m 2 .
[0119] Example 2a:
[0120] The other conditions of this embodiment are the same as those of embodiment 1. The difference from embodiment 1 is that the ratio of the raw materials of the diaphragm is different.
[0121] (1) Modified resin: 90 parts of maleic anhydride modified EVA resin;
[0122] (2) Binder solution: 66.7 parts of a PAA-PAN binder having a solid content of 15%; the PAA-PAN binder comprises 10 parts of an acrylic acid-acrylonitrile copolymer (PAA-PAN) and 56.7 parts of water;
[0123] (3) Solvent: 1200 parts of water.
[0124] The obtained binder slurry had a solid content of 8.2%, a viscosity of 56.8 mPa·s, and a pH of 7.54.
[0125] Example 2b:
[0126] The other conditions of this embodiment are the same as those of embodiment 1. The difference from embodiment 1 is that the ratio of the raw materials of the diaphragm is different.
[0127] (1) Modified resin: 80 parts of maleic anhydride modified EVA resin;
[0128] (2) Binder solution: 133 parts of a PAA-PAN binder having a solid content of 15%; the PAA-PAN binder comprises 20 parts of an acrylic acid-acrylonitrile copolymer (PAA-PAN) and 113 parts of water;
[0129] (3) Solvent: 1120 parts of water.
[0130] The obtained binder slurry had a solid content of 8.2%, a viscosity of 61.8 mPa·s, and a pH of 7.44.
[0131] Example 3a:
[0132] The other conditions of this embodiment are the same as those of embodiment 1. The difference from embodiment 1 is that the grafting monomer in the modified resin is replaced by glycidyl methacrylate.
[0133] The obtained binder slurry had a solid content of 8.0%, a viscosity of 57.8 mPa·s, and a pH of 7.24.
[0134] Example 3b:
[0135] The other conditions of this embodiment are the same as those of embodiment 1. The difference from embodiment 1 is that the grafting monomer in the modified resin is replaced by 2-methylbutenedioic anhydride.
[0136] The obtained binder slurry had a solid content of 7.9%, a viscosity of 49.7 mPa·s, and a pH of 7.28.
[0137] Example 4a:
[0138] The other conditions of this embodiment are the same as those of embodiment 1. The difference from embodiment 1 is that the weight proportion of the grafted monomer in the modified resin is 8%.
[0139] The obtained binder slurry had a solid content of 8.2%, a viscosity of 52.1 mPa·s, and a pH of 7.21.
[0140] Example 4b:
[0141] The other conditions of this embodiment are the same as those of embodiment 1. The difference from embodiment 1 is that the weight proportion of the grafted monomer in the modified resin is 15%.
[0142] The obtained binder slurry had a solid content of 8.1%, a viscosity of 47.3 mPa·s, and a pH of 7.26.
[0143] Example 5:
[0144] The other conditions of this embodiment remain unchanged from those of embodiment 1. The difference from embodiment 1 is that the resin matrix in the modified resin is replaced by vinyl acetate-acrylate copolymer.
[0145] The obtained adhesive slurry had a solid content of 8.0%, a viscosity of 54.7 mPa·s, and a pH of 7.33.
[0146] The other conditions of this comparative example remain unchanged from those of Example 1, except that the modified resin is replaced by PVDF.
[0147] The obtained adhesive slurry had a solid content of 8.5%, a viscosity of 52.3 mPa·s, and a pH of 7.44.
[0148] The other conditions of this comparative example remain unchanged from those of Example 1, except that the modified resin is replaced by EVA resin.
[0149] The obtained binder slurry had a solid content of 8.1%, a viscosity of 38.3 mPa·s, and a pH of 7.34.
[0150] Comparative Example 3a:
[0151] The other conditions of this comparative example are the same as those of Example 1, except that the weight percentage of the grafted monomer in the modified resin is 5%.
[0152] The obtained binder slurry had a solid content of 8.1%, a viscosity of 44.5 mPa·s, and a pH of 7.32.
[0153] The other conditions of this comparative example are the same as those of Example 1, except that the weight percentage of the grafted monomer in the modified resin is 20%.
[0154] The obtained binder slurry had a solid content of 7.8%, a viscosity of 43.6 mPa·s, and a pH of 7.41.
[0155] Comparative Example 4a:
[0156] The other conditions of this comparative example are the same as those of Example 1, except that the average particle size of the modified resin is 0.7 μm.
[0157] The obtained binder slurry had a solid content of 7.9%, a viscosity of 50.1 mPa·s, and a pH of 7.21.
[0158] The other conditions of this comparative example are the same as those of Example 1, except that the average particle size of the modified resin is 4.5 μm.
[0159] The obtained binder slurry had a solid content of 8.2%, a viscosity of 56.8 mPa·s, and a pH of 7.28.
[0160] Adhesion comparison test
[0161] The diaphragms prepared in the above examples and comparative examples were subjected to a comparative adhesion test. The test method is as follows: the coated diaphragm is passed through a winding machine, the positive and negative electrode sheets and the diaphragm are wound together, and then hot pressed or cold pressed (hot pressing: 90°C, 5MPa, 25s; cold pressing: room temperature, 8MPa, 25s). The 180° peel strength of the electrode sheet and the diaphragm is tested using a universal tensile tester. The test results are as follows:
[0162] Table 1 Peel force test results
[0163]
[0164] Note: Dry adhesion refers to the adhesion strength between the diaphragm and the electrode before being immersed in the electrolyte; wet adhesion refers to the adhesion strength between the diaphragm and the electrode after being immersed in the electrolyte.
[0165] The above results show that the diaphragms and electrode plates prepared in Examples 1 to 5 all have high adhesion. The results of Example 2a, Example 1, and Example 2b show that the adhesion between the diaphragm and the electrode plate gradually decreases as the amount of modified EVA resin used decreases.
[0166] Due to the presence of PVDF, the separator of Comparative Example 1 has almost no adhesion to the electrode without hot pressing.
[0167] The separator in Comparative Example 2, containing unmodified EVA resin, was found to cling together after winding due to its low glass transition temperature, hindering production and usability. Its hot and cold press adhesion was essentially the same. Furthermore, due to the presence of vinyl acetate in the EVA resin, its wet adhesion was higher. Due to the EVA resin's low TG, insufficient intermolecular cohesion resulted in molecular breakage during testing, resulting in slightly lower adhesion than in Example 1.
[0168] In comparative example 3a, the mass proportion of the grafted monomer in the modified resin is too low, and the modified resin directly exposes a large amount of EVA resin. After winding, it is found that the diaphragm sticks together, affecting production and use.
[0169] In comparative example 3b, the mass proportion of the grafted monomer in the modified resin is too high. When the cold pressing operation is performed during the battery cell preparation process, the shell of the modified resin is not easily crushed, and the EVA resin cannot be exposed, resulting in reduced viscosity.
[0170] In comparative example 4a, the average particle size of the modified resin is too small. When the cold pressing operation is performed during the battery cell preparation process, the shell of the modified resin is not easily crushed, and the EVA resin cannot be exposed, resulting in reduced viscosity.
[0171] In Comparative Example 4b, the average particle size of the modified resin is too large, resulting in an overly thick separator and severe tab misalignment, which affects the quality of the battery cell as well as the electrical and safety performance of the battery.
[0172] Diaphragm air permeability test
[0173] The air permeability of the above examples and comparative examples was tested using an air permeometer. The test results are as follows:
[0174] Table 2 Air permeability test results
[0175]
[0176]
[0177] From the above results, it can be seen that the diaphragms prepared in Examples 1-5 all have good air permeability.
[0178] In Comparative Example 2, since the unmodified EVA resin has a low glass transition temperature and is relatively soft, after being subjected to pressure, the permeability of the diaphragm increases severely, the lithium ion shuttle channels decrease, and the diaphragm cannot be used.
[0179] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A diaphragm, characterized in that: The diaphragm includes a base film layer, and an adhesive layer disposed on at least one side surface of the base film layer; The adhesive layer includes a modified resin and an adhesive; The modified resin has a core-shell structure, the core of the modified resin includes a resin matrix, and the shell of the modified resin includes a grafted monomer; The glass transition temperature of the resin matrix is -25°C to 10°C; The glass transition temperature of the grafted monomer is 90°C to 150°C.
2. The diaphragm according to claim 1, characterized in that The resin matrix includes at least one of ethylene-vinyl acetate copolymer and vinyl acetate-acrylate copolymer; Preferably, the grafting monomer includes at least one of maleic anhydride, glycidyl methacrylate, and 2-methylbutenedioic anhydride.
3. The diaphragm according to claim 1, characterized in that The mass percentage of the grafted monomer in the modified resin is 8% to 15%; Preferably, the average particle size of the modified resin is 2 to 3 μm.
4. The diaphragm according to claim 1, characterized in that In the adhesive layer, the mass percentage of the modified resin is 80% to 90%, and the mass percentage of the adhesive is 10% to 20%.
5. The diaphragm according to claim 1, characterized in that The binder includes at least one of acrylic acid-acrylonitrile copolymer, polyacrylic acid, polyacrylonitrile and polyvinyl alcohol.
6. The diaphragm according to claim 1, characterized in that The coating amount of the adhesive layer on the base film layer is 0.2 to 0.4 g / m 2 .
7. The diaphragm according to any one of claims 1 to 6, characterized in that The base film layer includes a base film or a base film composited with a ceramic layer; In the base film composited with a ceramic layer, the ceramic layer is disposed on at least one surface of the base film.
8. A method for preparing the diaphragm according to any one of claims 1 to 7, characterized in that: The steps include: The modified resin, the binder and the solvent are mixed and dispersed to obtain a binder slurry; The binder slurry is applied to at least one surface of the base film layer and dried to obtain a diaphragm.
9. A battery, characterized in that: The battery comprises a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator comprises the separator according to any one of claims 1 to 7 and / or the separator prepared by the preparation method according to claim 8, and the separator is arranged between the positive electrode sheet and the negative electrode sheet.
10. A method for preparing the battery according to claim 9, characterized in that: The steps include: The positive electrode sheet, the separator and the negative electrode sheet are stacked to obtain a battery cell, or the positive electrode sheet, the separator and the negative electrode sheet are stacked and then wound to obtain a battery cell; The battery cell is subjected to cold pressing or hot pressing; Preferably, the temperature of the cold pressing treatment is 15-25°C, the pressure is 5-10MPa, and the time is 20-30s; Preferably, the temperature of the hot pressing treatment is 80-100° C., the pressure is 3-8 MPa, and the time is 20-30 seconds.
Citation Information
Patent Citations
Adhesive resin composition for secondary battery
CN103828114A
Functional coating composition for secondary battery diaphragm, functional coating and application
CN115498361A
Slurry composition for non-aqueous secondary battery adhesive layer, adhesive layer for non-aqueous secondary battery and method for producing same, member for non-aqueous secondary battery, and non-aqueous secondary battery
CN117837014A
Porous film for secondary batteries, method for producing same, electrode for secondary batteries, separator for secondary batteries, and secondary battery
WO2013141140A1
All-optical light field sampling with attosecond resolution
WO2022232210A1
Cited By
Composite diaphragm and secondary battery
CN120320000A
Composite diaphragm and secondary battery
CN120320000B
Winding type electrode assembly and preparation method thereof, battery monomer, battery and power utilization device
CN120933499A
Wound electrode assembly, method of manufacturing the same, battery cell, battery, and power using device
CN120933499B