Carbon brush for winding type motor and preparation method of carbon brush

By using materials such as graphene-coated graphite powder, carbon fiber and zinc powder in the carbon brush, combined with lubricants, the problem of insufficient conductivity and wear resistance of the carbon brush is solved, achieving high conductivity, low resistance, long life and Anti-oxidation properties, suitable for large motor applications.

CN118763472AActive Publication Date: 2024-10-11JIAMUSI ELECTRIC MACHINE
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411219548.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-10-11
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

Existing carbon brushes in large megawatt motors have poor electrical conductivity, poor wear resistance and short service life. They are prone to corrosion, especially in humid environments, resulting in increased wear and noise.

Method used

Graphene-coated graphite powder, carbon fiber and zinc powder are combined with electrolytic copper powder to prepare carbon brushes through powder metallurgy. Lubricant is added during the preparation process to improve uniformity and wear resistance and form a protective layer to prevent corrosion.

Benefits of technology

Significantly improves the electrical conductivity and mechanical properties of the carbon brush, reduces the resistance coefficient and friction coefficient, extends the service life, is suitable for humid environments, reduces noise and wear, the current density reaches 23A/cm2, and the service life can reach more than 2 years .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763472A_ABST
    Figure CN118763472A_ABST
Patent Text Reader

Abstract

The invention provides a carbon brush for a winding type motor and a preparation method of the carbon brush, and relates to the technical field of carbon brushes. The carbon brush for the winding type motor comprises electrolytic copper powder, asphalt adhesive graphite powder, graphene coated graphite powder, carbon fibers, zinc powder and a lubricant. Graphene-coated graphite powder and carbon fibers are added at the same time to generate a synergistic effect, so that the wear resistance of the carbon brush is ensured while the bearing capacity of the carbon brush is met, the resistance coefficient can be reduced, and the conductivity and mechanical properties of the carbon brush are greatly enhanced; due to the addition of the lubricant, the friction coefficient between the carbon brush and the ring surface can be reduced, and a layer of uniform, moderate and stable oxide film is formed on the surface of the collector ring, so that the effects of lubricating, reducing abrasion and reducing noise can be achieved; the zinc powder can form a protective layer on the oxidized surface of the carbon brush, so that the corrosion of the carbon brush is reduced, and the service life of the carbon brush is prolonged; and the addition of the asphalt adhesive graphite powder is beneficial to improving the adhesion among the powder, is beneficial to the uniform mixing and dispersion of the powder, and improves the uniform stability of the carbon brush.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of carbon brushes, and in particular to a carbon brush for a wound-rotor motor and a preparation method thereof. Background Art

[0002] Carbon brushes are mostly made of electrolytic copper and graphite. Depending on the needs of use, silver powder, aluminum powder, lead powder and other metals are sometimes used. This type of carbon brush has both the friction characteristics of graphite and the high conductivity of metal. It is suitable for low-voltage motors with high loads and low commutation requirements.

[0003] With the development of society and technological innovation in the application field, the current application scenarios of carbon brushes are mostly concentrated in large-megawatt motors, and small units are gradually decreasing. Large-megawatt motors mean that carbon brushes need to have better current carrying capacity and wear resistance at the same time. Most of the current carrying capacity problems are solved by adding metals (copper or silver, etc.), but copper powder has a high friction coefficient and poor wear resistance. The conductivity and wear resistance of copper / graphite carbon brushes restrict each other. Especially when the proportion of copper powder added is too large, the friction coefficient between the carbon brush and the ring surface will increase, thereby increasing the amount of wear, reducing the service life of the carbon brush, and increasing the noise of the equipment. In addition, the gradual development of the application environment has led to carbon brushes also facing humid environments. For example, the salt mist formed by the evaporation of salt from coastal seawater has a serious corrosion on the carbon brushes. The generated oxides make the carbon brushes and the collector rings in poor contact, which will cause serious corrosion and wear, and reduce the service life of the carbon brushes. Summary of the invention

[0004] The problem solved by the invention is how to solve the problems of poor electrical conductivity, poor wear resistance and short service life of the carbon brush.

[0005] In order to solve the above problems, the present invention provides a carbon brush for a wound-rotor motor and a preparation method thereof.

[0006] In a first aspect, the present invention provides a carbon brush for a wound-rotor motor, wherein the composition of the carbon brush for the wound-rotor motor comprises: 65-85 parts of electrolytic copper powder, Asphalt adhesive graphite powder 5-20 parts, 5-20 parts of graphene-coated graphite powder, 1-5 parts of carbon fiber, 1-5 parts of zinc powder, 1-5 parts of lubricant.

[0007] Optionally, the graphene-coated graphite powder is prepared by uniformly stirring 1 part by mass of an organic solvent, 30-40% by mass of graphene in the organic solvent, and 3 parts by mass of graphite powder using a stirrer.

[0008] Optionally, the graphene-coated graphite powder is prepared by the following steps: Mixing: first add 1 part by mass of organic solvent into a stirrer, start stirring at 150rpm / min at room temperature, slowly add graphene accounting for 30-40% of the mass of the organic solvent, the first stirring time is 30-60min, then slowly add 3 parts by mass of graphite powder, continue stirring for 60-120min, stir and mix to obtain powder, stop the stirrer and place the powder at room temperature for 12-24 hours to dry, then put it into an oven at a temperature of 60-90°C for 6-12 hours, and crush and sieve the powder after the oven cools naturally; Grinding and sieving: adding the powder into a grinding machine for grinding, setting a 0.5 mm aperture sieve at the discharge port of the grinding machine for preliminary sieving to obtain a coarse powder; passing the coarse powder through a 60-mesh sieve to obtain graphene-coated graphite powder.

[0009] Optionally, the lubricant is one or more of stearic acid, metal stearate, phthalates, and high molecular weight complex esters.

[0010] Optionally, the metal stearate is one or more of calcium stearate, magnesium stearate, zinc stearate and barium stearate; the phthalates are one or more of dimethyl phthalate, dioctyl phthalate, diisooctyl phthalate and dibutyl phthalate; and the polymer composite ester is a composite ester obtained by esterification condensation and saponification of polyols, dicarboxylic acids and higher fatty acids.

[0011] In a second aspect, the present invention provides a method for preparing a carbon brush for a wound-rotor motor as described in any one of the above items, comprising the following steps: S1: Mixing: First, sieve the asphalt binder graphite powder, graphene-coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder, weigh the sieved asphalt binder graphite powder, graphene-coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder, and add them into the mixer in sequence. After mixing, stop the machine and discharge the materials to obtain mixed material powder; S2: Pressing: Pressing the mixed powder into a shape to form a primary carbon brush; S3: Heat treatment: The primary carbon brush is placed in a crucible and sintered in a furnace at a temperature of 800-1100° C. to obtain a carbon brush for a wound-type motor.

[0012] Optionally, the asphalt adhesive graphite powder, graphene-coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder are sieved through a 50-mesh sieve.

[0013] Optionally, in step S1, the asphalt adhesive graphite powder, graphene-coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder are closed and mixed in a mixer for 100-200 minutes.

[0014] Optionally, the pressure applied during the pressing process in step S2 is 200MPa-250MPa.

[0015] Optionally, step S3: spread a layer of sand coke on the bottom of the crucible, place the primary carbon brushes on the sand coke at fixed intervals, stack them up after they are fully spread, and isolate them with the sand coke, vibrate them, cover them with iron plates, and seal them with refractory mud. Apply a layer of foamed alkali refractory mud on the outer surface of the crucible with the primary carbon brush and dry it, then place the crucible in a furnace at a temperature of 800-1100°C for sintering, and the sintering time is 30-41 hours; after sintering is completed, take out the crucible and cool it naturally to room temperature to obtain a carbon brush for a wound motor.

[0016] The beneficial effects of the carbon brush for a wound-rotor motor and the preparation method thereof of the present invention are as follows: Graphene is a carbon brush composed of carbon atoms in the form of sp 2 Hybridized orbitals form a hexagonal honeycomb lattice of two-dimensional nanomaterials. Graphene has excellent optical, electrical and mechanical properties. Carbon fiber has the characteristics of high temperature resistance, high strength, high hardness and light weight. Adding graphene to carbon brushes is beneficial to enhancing the conductivity of carbon brushes; however, there are strong van der Waals forces and π-π interactions between graphene sheets, which make them easy to stack and agglomerate. Carbon brushes prepared by directly adding graphene powder by powder metallurgy will have the problem of poor uniformity inside the brush body. In order to overcome the problem of difficulty in uniform dispersion in composite materials due to the agglomeration of graphene itself, graphene is coated with graphite powder to achieve the addition of graphene to carbon brushes, which solves the problem of difficulty in adding graphene powder due to agglomeration. Title: Graphene-coated graphite powder and carbon fiber are added at the same time to produce a synergistic effect, which can meet the load-bearing capacity of the carbon brush while ensuring its wear resistance, reduce the adhesive wear of the carbon brush, and reduce the resistivity, greatly enhancing the conductivity and mechanical properties of the carbon brush; the addition of lubricant can reduce the friction coefficient between the carbon brush and the ring surface, and form a uniform, moderate and stable oxide film on the surface of the collector ring, which can play a role in lubrication, wear reduction and noise reduction; zinc powder can form a protective layer on the oxidized surface of the carbon brush, which is beneficial to reduce the corrosion of the carbon brush and increase the service life of the carbon brush; adding asphalt adhesive graphite powder is beneficial to improve the adhesion between the powders, facilitate the mixing and dispersion of the powders, and improve the uniform stability of the carbon brushes. The current density of the carbon brush for the wound motor can reach 23A / cm 2 , has good current gathering performance, good oxidation resistance, low resistivity, low energy loss, low noise during operation and not easy to break; the maximum service life of carbon brushes for wound-type motors can reach more than 2 years, which greatly reduces the operation and maintenance costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 Flow chart of the method for preparing the carbon brush for the wound-rotor motor of this embodiment. DETAILED DESCRIPTION

[0018] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.

[0019] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application; The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.

[0020] In view of the problems existing in the above-mentioned related technologies, this embodiment provides a carbon brush for a wound-rotor motor and a preparation method thereof.

[0021] An embodiment of the present invention provides a carbon brush for a wound-rotor motor, and the composition of the carbon brush for the wound-rotor motor includes: 65-85 parts of electrolytic copper powder, Asphalt adhesive graphite powder 5-20 parts, 5-20 parts of graphene-coated graphite powder, 1-5 parts of carbon fiber, 1-5 parts of zinc powder, 1-5 parts of lubricant.

[0022] In this embodiment, graphene is a carbon atom in the form of sp 2Hybridized orbitals form a hexagonal honeycomb lattice of two-dimensional nanomaterials. Graphene has excellent optical, electrical and mechanical properties. Carbon fiber has the characteristics of high temperature resistance, high strength, high hardness and light weight. Adding graphene to carbon brushes is beneficial to enhancing the conductivity of carbon brushes; however, there are strong van der Waals forces and π-π interactions between graphene sheets, which make them easy to stack and agglomerate. Carbon brushes prepared by directly adding graphene powder by powder metallurgy will have the problem of poor uniformity inside the brush body. In order to overcome the problem of difficulty in uniform dispersion in composite materials due to the agglomeration of graphene itself, graphene is coated with graphite powder to achieve the addition of graphene to carbon brushes, which solves the problem of difficulty in adding graphene powder due to agglomeration. Topic: Graphene-coated graphite powder and carbon fiber are added at the same time to produce a synergistic effect, which can meet the load-bearing capacity of the carbon brush while ensuring its wear resistance, reduce the adhesive wear of the carbon brush, and reduce the resistivity, greatly enhancing the conductivity and mechanical properties of the carbon brush; the addition of lubricant can reduce the friction coefficient between the carbon brush and the ring surface, and form a uniform, moderate and stable oxide film on the surface of the collector ring, which can play a role in lubrication, wear reduction and noise reduction; zinc powder can form a protective layer on the oxidized surface of the carbon brush, which is beneficial to reduce the corrosion of the carbon brush and increase the service life of the carbon brush; adding asphalt adhesive graphite powder is beneficial to improve the adhesion between powders, facilitate the uniform mixing and dispersion of powders, and improve the uniformity and stability of the carbon brush.

[0023] Optionally, the graphene-coated graphite powder is prepared by uniformly stirring 1 part by mass of an organic solvent, 30-40% by mass of graphene in the organic solvent, and 3 parts by mass of graphite powder using a stirrer.

[0024] Specifically, the organic solvent is a mixture of one or more of methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, 2-methyl-2-butanol, 3-methyl-2-butanol, 3-methyl-1-butanol, 2,2-dimethyl-1-propanol, n-hexanol, ethylene glycol, propylene glycol, glycerol, benzyl alcohol, ether, dichloromethane, chloroform, acetone, tetrahydrofuran, ethyl acetate, benzene, toluene, xylene, acetonitrile, pyridine, ethylenediamine, dimethyl sulfoxide, N-methylpyrrolidone, N-methylformamide and petroleum ether.

[0025] In this optional embodiment, graphene is coated on graphite powder to achieve the addition of graphene to the carbon brush, which overcomes the problem of graphene being difficult to disperse evenly in the composite material due to its own agglomeration, and solves the problem of difficulty in adding powdered graphene due to agglomeration. The graphene-coated graphite powder has good conductivity and high lithium storage performance.

[0026] Optionally, the graphene-coated graphite powder is prepared by the following steps: Mixing: First, add 1 part by mass of organic solvent into a stirrer, start stirring at 150 rpm / min at room temperature, slowly add graphene accounting for 30 - 40% of the mass of the organic solvent, with the first stirring time being 30 - 60 min, then slowly add 3 parts by mass of graphite powder, and continue stirring for 60 - 120 min. After stirring and mixing, a powder material is obtained. Stop the stirrer and let the powder material stand at room temperature for 12 - 24 hours to dry, then put it into an oven and dry at a temperature of 60 - 90 °C for 6 - 12 hours. After the oven cools naturally, crush and screen the powder material; Grinding and screening: Add the powder material into a grinding machine for grinding, set a sieve mesh with a pore diameter of Φ0.5 mm at the discharge port of the grinding machine for preliminary screening to obtain a coarse powder material; Pass the coarse powder material through a 60 - mesh sieve to obtain graphene - coated graphite powder.

[0027] In this alternative embodiment, the preparation process flow is simple, economical, mechanically operated, and is easy for large - scale mass production.

[0028] Optionally, the asphalt adhesive graphite powder is prepared by the following steps: Crushing: First, use a flat hammer to crush the asphalt into uniform size, and then use a special crusher to crush it into particles with uniform particle size; Hot mixing: Weigh 1 part by mass of graphite powder, asphalt accounting for 15 - 35% of the mass of graphite, and water accounting for 10 - 15% of the mass of graphite respectively; Then add the graphite powder, asphalt, and water into the mixing pot in sequence, and keep stirring during the adding process. After closing the lid, start hot mixing; Control the temperature of the mixer at 150 - 200 °C, and carry out hot mixing for 90 - 120 minutes. A large amount of water vapor flows out after mixing for 60 minutes. When the water vapor decreases and the gas color is slightly yellowish, stop the machine and open the lid to measure the temperature of the powder material. When the temperature of the powder material t < 180 °C, continue to close the lid for hot mixing. When 180 °C < t < 190 °C, continue to close the lid for hot mixing for 15 minutes, then stop heating, and then close the lid and mix for 30 - 60 minutes. Stop the machine and discharge the material. Place the hot - mixed powder material in an iron sheet box and let it cool freely; Grinding and screening: Add the mixed powder material through the feeding port for grinding, set a Φ0.5 - mm iron sheet sieve at the discharge port for preliminary screening to obtain a coarse powder material; Pass the coarse powder material through a cage - type sieve powder machine with a 60 - mesh sieve until all of it passes through, so as to obtain the available asphalt adhesive graphite powder.

[0029] In this alternative embodiment, the preparation process flow is simple, economical, mechanically operated, and is easy for large - scale mass production.

[0030] Optionally, the lubricant is one or more of stearic acid, metal stearate, phthalate esters, and polymer composite esters.

[0031] In this optional embodiment, the above lubricant is selected to reduce the friction coefficient between the carbon brush and the ring surface, and form a uniform, moderate and stable oxide film on the surface of the collector ring, thereby playing a role in lubrication, reducing wear and reducing noise.

[0032] Optionally, the metal stearate is one or more of calcium stearate, magnesium stearate, zinc stearate, and barium stearate. The phthalates are one or more of dimethyl phthalate, dioctyl phthalate, diisooctyl phthalate, and dibutyl phthalate. The polymer composite ester is a composite ester obtained by esterification condensation and saponification of polyols, dicarboxylic acids, and higher fatty acids.

[0033] like Figure 1 As shown, a method for preparing a carbon brush for a wound-rotor motor as described above is provided in an embodiment of the present invention, comprising the following steps: S1: Mixing: First, sieve the asphalt binder graphite powder, graphene-coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder, weigh the sieved asphalt binder graphite powder, graphene-coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder, and add them into the mixer in sequence. After mixing, stop the machine and discharge the materials to obtain mixed material powder; S2: Pressing: Pressing the mixed powder into a shape to form a primary carbon brush; S3: Heat treatment: The primary carbon brush is placed in a crucible and sintered in a furnace at a temperature of 800 to 1100° C. to obtain a carbon brush for a wound-type motor.

[0034] In this embodiment, the preparation process is simple, economical, mechanically operated, and easy to mass-produce. The current density of the wound-type motor carbon brush can reach 23A / cm 2 , has good current gathering performance, good oxidation resistance, low resistivity, low energy loss, low noise during operation and not easy to break; the maximum service life of carbon brushes for wound-type motors can reach more than 2 years, which greatly reduces the operation and maintenance costs.

[0035] Optionally, the asphalt adhesive graphite powder, graphene-coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder are sieved through a 50-mesh sieve.

[0036] Optionally, in step S1, the asphalt adhesive graphite powder, graphene-coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder are closed and mixed in a mixer for 100-200 minutes.

[0037] Optionally, the pressure applied during the pressing process in step S2 is 200MPa-250MPa.

[0038] Optionally, step S3: Lay a layer of sand coke at the bottom of the crucible, place the primary carbon brushes on the sand coke at fixed intervals, stack them up after covering the entire area, isolate them with sand coke, tamp them down, cover with an iron plate, and seal it tightly with refractory mortar. Apply a layer of sodium silicate refractory mortar on the outer surface of the crucible with the primary carbon brushes installed and let it dry. Then place the crucible in a furnace at a temperature of 800 - 1100 °C for sintering, and the sintering time is 30 - 41 hours. After sintering is completed, take out the crucible and let it cool naturally to room temperature, thus obtaining the carbon brushes for wound-rotor motors.

[0039] The present invention will be further described below in conjunction with specific embodiments.

[0040] Example 1 Preparation of the asphalt binder graphite powder used: Pour 100 kg of graphite powder into the hot mixing pot, start the double paddle, and without stopping the machine, evenly sprinkle 18.3 kg of mashed asphalt into the pot, then add 8 kg of clear water, close the lid and conduct hot mixing. Adjust the control temperature of the temperature controller of the mixing machine to 150 - 200 °C. Conduct hot mixing with the lid closed for 90 - 120 minutes. After mixing for 60 minutes, a large amount of water vapor flows out. When the water vapor decreases and the gas color is slightly yellowish, stop the machine and open the lid to measure the temperature of the powder. When the powder temperature t < 180 °C, continue to heat with the lid closed for mixing. When the powder temperature is 180 °C < t < 190 °C, continue to heat with the lid closed for mixing for 15 minutes, stop heating and continue to mix with the lid closed for 30 - 60 minutes, then stop the machine and discharge the material. If the powder temperature t > 190 °C, immediately stop heating, and the total mixing time should be controlled to 180 minutes. Let the mixture after heating and mixing cool naturally in an iron sheet box. Then install an iron sheet sieve with a Φ0.5 hole in the grinding machine, close the machine door, tie up the bag mouth of the discharge port, start the machine for grinding. Further, grind the powder until it all passes through a cage vibration sieve equipped with a 60-mesh screen, and after sieving, pack it in a plastic bag and seal it for storage.

[0041] Preparation of the graphene-coated graphite powder used: First, pour 15 kg of organic solvent weighed into the stirrer, start stirring at 150 rpm / min at room temperature, slowly add 5 kg of graphene, stir for 30 minutes, and finally slowly add 45 kg of graphite powder and continue to stir for 120 minutes. Stop the machine and let the powder dry at room temperature for 12 hours, then put it into a special oven and dry it at 60 °C for 12 hours, and let the oven cool naturally. Then install an iron sheet sieve with a Φ0.5 hole in the grinding machine, close the machine door, tie up the bag mouth of the discharge port, start the machine for grinding. Further, grind the powder until it all passes through a cage vibration sieve equipped with a 60-mesh screen, and after sieving, pack it in a plastic bag and seal it for storage.

[0042] Preparation of the carbon brushes for wound-rotor motors: 65 kg of electrolytic copper powder Graphene coated graphite powder 20kg Asphalt adhesive graphite powder 20 kg Carbon fiber 2 kg Zinc powder 3 kg Lubricant 2 kg Mixing: first sieve the asphalt adhesive graphite powder, graphene coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder through a 50-mesh sieve, then weigh 20 kg of asphalt adhesive graphite powder, 20 kg of graphene coated graphite powder, 2 kg of lubricant, 2 kg of carbon fiber, 3 kg of zinc powder and 65 kg of electrolytic copper powder, and add them into the mixer together, mix in a closed state for 100-200 minutes, stop the machine and discharge the material to obtain the mixed material powder.

[0043] Pressing: Press the mixed powder under a pressure of 230MPa±10% to form a primary carbon brush.

[0044] Heat treatment: First, spread a layer of sand coke on the bottom of the crucible, and place the primary carbon brushes on the sand coke at fixed intervals. After it is fully spread, it can be stacked up as needed and isolated by sand coke. Then, vibrate it, cover it with an iron plate, and seal it with refractory mud. Then, apply a layer of foamed alkali refractory mud on the surface of the crucible with the primary carbon brush installed and dry it. Then, sinter the crucible in a furnace at a temperature of 800-1100℃ for 30-41 hours. After sintering, drag the crucible out and cool it naturally to room temperature to obtain carbon brush products for wound motors.

[0045] Example 2 The difference between this embodiment and embodiment 1 is that 70 kg of electrolytic copper powder, 12 kg of asphalt adhesive graphite powder, 10 kg of graphene-coated graphite powder, 2 kg of carbon fiber, 3 kg of zinc powder, and 3 kg of lubricant are used. The remaining steps are the same as those in embodiment 1.

[0046] Example 3 The difference between this embodiment and embodiment 1 is that 70 kg of electrolytic copper powder, 10 kg of asphalt adhesive graphite powder, 12 kg of graphene-coated graphite powder, 5 kg of carbon fiber, 1 kg of zinc powder, and 5 kg of lubricant are used. The remaining steps are the same as those in embodiment 1.

[0047] Example 4 The difference between this embodiment and embodiment 1 is that 80 kg of electrolytic copper powder, 8 kg of asphalt adhesive graphite powder, 5 kg of graphene-coated graphite powder, 2 kg of carbon fiber, 3 kg of zinc powder, and 1 kg of lubricant are used. The remaining steps are the same as those in embodiment 1.

[0048] Example 5 The difference between this embodiment and embodiment 1 is that 85 kg of electrolytic copper powder, 5 kg of asphalt adhesive graphite powder, 5 kg of graphene-coated graphite powder, 1 kg of carbon fiber, 5 kg of zinc powder, and 2 kg of lubricant are used. The remaining steps are the same as those in embodiment 1.

[0049] Comparative Example 1 The difference between this comparative example and Example 1 is that the carbon brush is composed of 65 kg of electrolytic copper powder, 33 kg of asphalt adhesive powder, and 2 kg of lubricant, and the remaining steps are the same as Example 1.

[0050] Comparative Example 2 The difference between this comparative example and Example 1 is that the carbon brush is composed of 65 kg of electrolytic copper powder, 28 kg of asphalt adhesive powder, 2 kg of carbon fiber, 3 kg of zinc powder, and 2 kg of lubricant, and the remaining steps are the same as Example 1.

[0051] Comparative Example 3 The difference between this comparative example and Example 1 is that the carbon brush is composed of 65 kg of electrolytic copper powder, 15 kg of asphalt adhesive powder, 15 kg of graphene-coated graphite powder, 3 kg of zinc powder, and 2 kg of lubricant, and the remaining steps are the same as Example 1.

[0052] Comparative Example 4 The difference between this comparative example and Example 1 is that the carbon brush is composed of 65 kg of electrolytic copper powder, 16 kg of asphalt adhesive powder, 15 kg of graphene-coated graphite powder, 2 kg of carbon fiber, and 2 kg of lubricant, and the remaining steps are the same as Example 1.

[0053] The products prepared in Examples 1-5 and Comparative Examples 1-4 were tested for performance respectively, and the test methods were conventional methods in the art. The Rockwell hardness, contact voltage drop, and 50-hour wear value can be directly tested, and the current density is obtained from the type test results. The resistivity, friction coefficient, and volume density are calculated, and the specific calculation formula is as follows: Resistivity: ρ=UbW / (IL μ ) (1) Where: r —Resistivity, in microohm-meter (μΩ·m); U —The voltage drop between the potential needles, in millivolts (mV); I —The current passing through the sample, in ampere (A); b —Thickness of the specimen, in millimeters (mm); W —Width of the specimen, in millimeters (mm); Lμ —The distance between potential pins, in millimeters (mm).

[0054] Friction coefficient: μ=(PP) 0 ) / (NF R v) (2) Where: m — friction factors; P —The load power of the sample and the short-circuit commutator at the end, in watts (W); P 0—no-load power when the sample is lifted, unit is (W); N —Number of samples; F R —Radial force of each specimen, in Newton (N); v —Linear speed during operation, in meters per second (m / s).

[0055] Bulk Density: p=m / v (3) Where: r - Bulk density, in grams per cubic centimeter (g / cm 3 ); m —The mass of the sample, in grams (g); v —The volume of the sample, in cubic centimeters (cm 3 ).

[0056] The test results of Examples 1-5 are shown in Table 1, and the test results of Comparative Examples 1-4 are shown in Table 2.

[0057] Table 1 Performance test results of Examples 1-5

[0058] Table 2 Performance test results of comparative examples 1-4

[0059] From Table 1 and Table 2, it can be seen that the resistivity of the carbon brushes prepared by the graphene-coated graphite powder, carbon fiber and zinc powder obtained in Examples 1-5 is much lower than the resistivity of the carbon brushes in Comparative Examples 1-4 without adding the corresponding raw materials, indicating that the addition of graphene and carbon fiber plays an important role in reducing the resistance. The carbon brushes in the comparative examples are mainly suitable for small megawatt units, and cannot meet their use requirements in large megawatt models. The carbon brushes of the present invention have greatly improved current density, service life and application scenarios compared to those in the comparative examples, can be used in humid environments, and have good antioxidant properties. The current density of the carbon brushes of the present invention is from 18A / cm 2 Increased to 23A / cm 2 The current density is increased by 27%. When used in large units under the same working conditions, the service life of the carbon brush of the present invention can be increased to two years, and the temperature rise of the carbon brush is low, which can greatly reduce the subsequent maintenance cost and can meet the use of large and small megawatt models.

[0060] Based on the above, the carbon brush for wound-rotor motor of the present invention has the advantages of low resistance, good oxidation resistance, low friction coefficient, large current density and small wear. By preparing graphene-coated graphite powder and adding it to the carbon brush, the problem of graphene agglomeration is successfully solved, and a carbon brush containing graphene is prepared. At the same time, by adding graphene and carbon fiber, the wear resistance of the carbon brush is guaranteed while meeting the load-bearing capacity of the carbon brush. The addition of graphene and carbon fiber can reduce the adhesive wear of the carbon brush, and the lubricant can reduce the friction coefficient between the carbon brush and the annular surface, and promote the formation of a suitable oxide film between the friction pair, thereby achieving the effect of reducing wear. The addition of zinc powder can form a protective layer on the surface of the brush body to protect the inside of the carbon brush from severe corrosion. Adding asphalt adhesive graphite powder is beneficial to improving the adhesion between powders, facilitating the uniform mixing and dispersion of powders, and improving the uniform stability of the product.

[0061] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A carbon brush for a wound-rotor motor, characterized in that: The composition of the carbon brush for the wound-rotor motor comprises: 65-85 parts of electrolytic copper powder, Asphalt adhesive graphite powder 5-20 parts, 5-20 parts of graphene-coated graphite powder, 1-5 parts of carbon fiber, 1-5 parts of zinc powder, 1-5 parts of lubricant.

2. The carbon brush for a wound-rotor motor according to claim 1, characterized in that: The graphene-coated graphite powder is prepared by uniformly stirring 1 part by mass of an organic solvent, 30-40% by mass of graphene in the organic solvent, and 3 parts by mass of graphite powder using a stirrer.

3. The carbon brush for a wound-rotor motor according to claim 2, characterized in that: The graphene-coated graphite powder is prepared by the following steps: Mixing: first add 1 part by mass of the organic solvent into the stirrer, start stirring at 150 rpm / min at room temperature, slowly add the graphene accounting for 30-40% of the mass of the organic solvent, the first stirring time is 30-60 minutes, then slowly add 3 parts by mass of the graphite powder, continue stirring for 60-120 minutes, stir and mix to obtain powder, stop the stirrer and place the powder at room temperature for 12-24 hours to dry, then put it in an oven at a temperature of 60-90° C. and dry it for 6-12 hours, and crush and sieve the powder after the oven is naturally cooled; Grinding and sieving: adding the powder into a grinding machine for grinding, setting a 0.5 mm aperture sieve at the discharge port of the grinding machine for preliminary sieving to obtain a coarse powder; passing the coarse powder through a 60-mesh sieve to obtain the graphene-coated graphite powder.

4. The carbon brush for a wound-rotor motor according to claim 1, characterized in that: The lubricant is one or more of stearic acid, metal stearate, phthalates, and polymer composite esters.

5. The carbon brush for a wound-rotor motor according to claim 4, characterized in that: The metal stearate is one or more of calcium stearate, magnesium stearate, zinc stearate and barium stearate; the phthalates are one or more of dimethyl phthalate, dioctyl phthalate, diisooctyl phthalate and dibutyl phthalate; the polymer composite ester is a composite ester obtained by esterification condensation and saponification of polyols, dicarboxylic acids and higher fatty acids.

6. A method for preparing a carbon brush for a wound-rotor motor according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: Mixing: First, sieve the asphalt binder graphite powder, graphene-coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder, weigh the sieved asphalt binder graphite powder, graphene-coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder, and add them into the mixer in sequence. After mixing, stop the machine and discharge the materials to obtain mixed material powder; S2: Pressing: Pressing the mixed material powder to form a primary carbon brush; S3: Heat treatment: placing the primary carbon brush in a crucible and sintering it in a furnace at a temperature of 800-1100° C. to obtain a carbon brush for a wound-rotor motor.

7. The method for preparing a carbon brush for a wound-rotor motor according to claim 6, characterized in that: The asphalt adhesive graphite powder, graphene-coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder are sieved through a 50-mesh sieve.

8. The method for preparing a carbon brush for a wound-rotor motor according to claim 6, characterized in that: In the step S1, the asphalt adhesive graphite powder, graphene-coated graphite powder, lubricant, carbon fiber, zinc powder and electrolytic copper powder are closed and mixed in the mixer for 100-200 minutes.

9. The method for preparing a carbon brush for a wound-rotor motor according to claim 6, characterized in that: The pressure applied during the molding process in step S2 is 200MPa-250MPa.

10. The method for preparing a carbon brush for a wound-rotor motor according to claim 6, characterized in that: The step S3: spreading a layer of sand coke on the bottom of the crucible, placing the primary carbon brushes on the sand coke at fixed intervals, stacking them up after they are fully spread, and isolating them with sand coke, compacting them, covering them with iron plates, and sealing them with refractory mud, brushing a layer of foamed alkali refractory mud on the outer surface of the crucible with the primary carbon brush installed and drying it, and then placing the crucible in the furnace at a temperature of 800-1100°C for sintering, and the sintering time is 30-41 hours; after sintering is completed, taking out the crucible and naturally cooling it to room temperature, thereby obtaining the carbon brush for the wound-type motor.

Citation Information

Patent Citations

  • Special carbon brush for wind-driven generators and preparation method thereof

    CN106159623A

  • Graphene coated artificial graphite negative electrode material preparation method

    CN107507963A

  • Copper-graphite-graphene brush and preparation method thereof

    CN108512006A

  • Preparation method of high-conductivity and high-strength wear-resistant copper-based material