Far infrared transmitting member and method for manufacturing far infrared transmitting member
By using a high-content ZrO2 film in the outermost layer of the far-infrared transmission component, combined with the design of the intermediate layer and anti-reflection layer, the problem of insufficient scratch resistance of the far-infrared transmission component in the existing technology is solved, and high transmittance and Improved scratch resistance.
Patent Information
- Application Number
- CN202380025574.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-07
- Filing Date
- 2023-02-17
- Publication Date
- 2024-10-11
AI Technical Summary
It is difficult for existing far-infrared ray transmitting members to improve scratch resistance while appropriately transmitting far-infrared rays.
The outermost film mainly composed of ZrO2 is formed on the substrate through sputtering technology to ensure that the content of ZrO2 is above 50% and below 100%, and the refractive index of light at a wavelength of 550nm reaches above 2.05, combined with the middle layer And the design of anti-reflection layer improves transmittance and scratch resistance.
It achieves proper transmission of far-infrared rays and improved scratch resistance, reduces the load in the film-forming process, and at the same time increases the density and indentation hardness of the film.
Smart Images

Figure CN118765267A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a far-infrared ray transmitting member and a method for producing the far-infrared ray transmitting member. Background Art
[0002] For example, when a far infrared sensor is mounted on a vehicle, a far infrared transmission member having a functional film formed thereon is sometimes provided, and the functional film is used to allow far infrared rays to be incident on the far infrared sensor appropriately. For example, Patent Document 1 describes forming an infrared transmission film having zinc oxide as a main component and containing a metal oxide on a substrate.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2017-151408 Summary of the invention
[0006] Problems to be solved by the invention
[0007] Such a far-infrared ray transmitting member is required to appropriately transmit far-infrared rays while improving scratch resistance.
[0008] An object of the present invention is to provide a far-infrared transmitting member and a method for manufacturing the far-infrared transmitting member which can appropriately transmit far-infrared rays and can improve scratch resistance.
[0009] Means used to solve problems
[0010] The far-infrared transmission member disclosed herein comprises a substrate that allows far-infrared transmission and a functional film formed on the substrate, wherein the far-infrared transmission member has an average transmittance of light with a wavelength of 8 μm to 12 μm of 50% or more, and the outermost layer of the functional film is made of ZrO 2 The layer as the main component is ZrO relative to the entire outermost layer. 2 The content of is 50 mass % or more and 100 mass % or less, and the refractive index of the outermost layer of the functional film with respect to light of a wavelength of 550 nm is 2.05 or more.
[0011] The manufacturing method of the far-infrared transmission component disclosed in the present invention is a manufacturing method of the far-infrared transmission component in which a functional film is formed on a substrate that allows far-infrared transmission, wherein the manufacturing method of the far-infrared transmission component comprises: the step of manufacturing the far-infrared transmission component by forming the outermost layer of the functional film on the substrate by sputtering, the average transmittance of the far-infrared transmission component for light with a wavelength of 8 μm to 12 μm is 50% or more, the outermost layer is made of ZrO 2 The layer as the main component is ZrO relative to the entire outermost layer. 2The content of is 50 mass % or more and 100 mass % or less, and the refractive index of the outermost layer with respect to light of a wavelength of 550 nm is 2.05 or more.
[0012] Effects of the Invention
[0013] According to the present invention, far infrared rays can be appropriately transmitted and scratch resistance can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a schematic diagram which shows the state which mounted the vehicle glass of this embodiment on the vehicle.
[0015] Figure 2 It is a schematic plan view of the vehicle glass according to the present embodiment.
[0016] Figure 3 For along Figure 2 Cross-sectional view along line AA.
[0017] Figure 4 For along Figure 2 Cross-sectional view of the BB section.
[0018] Figure 5 It is a schematic cross-sectional view of the far-infrared transmissive member of this embodiment.
[0019] Figure 6 It is a schematic diagram for explaining the manufacturing method of the far-infrared transmissive member of this embodiment. DETAILED DESCRIPTION
[0020] Hereinafter, a suitable embodiment of the present invention will be described in detail with reference to the accompanying drawings. It should be noted that the present invention is not limited to the embodiment, and in addition, when there are multiple embodiments, a mode of combining the embodiments is also included. In addition, the numerical values include the range of rounding.
[0021] (vehicle)
[0022] Figure 1 Schematic diagram showing a state where the vehicle glass of this embodiment is mounted on a vehicle. Figure 1 As shown, the vehicle glass 1 of this embodiment is mounted on a vehicle V. The vehicle glass 1 is a window member applied to the front glass of the vehicle V. That is, the vehicle glass 1 is used as the front window of the vehicle V, in other words, as a windshield. A far-infrared camera CA1 and a visible light camera CA2 are mounted inside (inside) the vehicle V. It should be noted that the inside (inside) of the vehicle V refers to, for example, the interior of the vehicle V where the driver's seat is set.
[0023] The vehicle glass 1, the far-infrared camera CA1 and the visible light camera CA2 constitute the camera unit 100 of the present embodiment. The far-infrared camera CA1 is a camera that detects far-infrared rays, and captures a thermal image of the outside of the vehicle V by detecting far-infrared rays from the outside of the vehicle V. The visible light camera CA2 is a camera that detects visible light, and captures an image of the outside of the vehicle V by detecting visible light from the outside of the vehicle V. It should be noted that the camera unit 100 may also have, for example, LiDAR and millimeter wave radar in addition to the far-infrared camera CA1 and the visible light camera CA2. The far-infrared rays here refer to electromagnetic waves in a wavelength band of, for example, 8μm to 13μm, and the visible light refers to electromagnetic waves in a wavelength band of, for example, 360nm to 830nm. In addition, 8μm to 13μm here refers to 8μm or more and 13μm or less, and 360nm to 830nm refers to 360nm or more and 830nm or less, and the same applies hereinafter. In addition, far infrared rays can be set to electromagnetic waves in a wavelength band of 8 μm to 12 μm.
[0024] (Glass for vehicles)
[0025] Figure 2 It is a schematic plan view of the vehicle glass according to the present embodiment. Figure 3 For along Figure 2 Cross-sectional view along line AA. Figure 4 For along Figure 2 The sectional view of the BB section. Figure 2 As shown, hereinafter, the upper edge of the vehicle glass 1 is referred to as the upper edge portion 1a, the lower edge of the vehicle glass 1 is referred to as the lower edge portion 1b, the side edge of one side of the vehicle glass 1 is referred to as the side edge portion 1c, and the side edge of the other side of the vehicle glass 1 is referred to as the side edge portion 1d. The upper edge portion 1a is an edge portion located on the upper side in the vertical direction when the vehicle glass 1 is mounted on the vehicle V. The lower edge portion 1b is an edge portion located on the lower side in the vertical direction when the vehicle glass 1 is mounted on the vehicle V. The side edge portion 1c is an edge portion located on the lateral side of one side when the vehicle glass 1 is mounted on the vehicle V. The side edge portion 1d is an edge portion located on the lateral side of the other side when the vehicle glass 1 is mounted on the vehicle V.
[0026] Hereinafter, in the direction parallel to the surface of the vehicle glass 1, the direction from the upper edge 1a to the lower edge 1b is set as the Y direction, and the direction from the side edge 1c to the side edge 1d is set as the X direction. In the present embodiment, the X direction is orthogonal to the Y direction. The direction orthogonal to the surface of the vehicle glass 1, that is, the thickness direction of the vehicle glass 1 is set as the Z direction. The Z direction is, for example, the direction from the outer side of the vehicle V to the inner side of the vehicle V when the vehicle glass 1 is mounted on the vehicle V. The X direction and the Y direction are along the surface of the vehicle glass 1, but, for example, when the surface of the vehicle glass 1 is a curved surface, it can also be a direction tangent to the surface of the vehicle glass 1 at the center point O of the vehicle glass 1. The center point O refers to the center position of the vehicle glass 1 when the vehicle glass 1 is observed from the Z direction.
[0027] A light-transmitting area A1 and a light-shielding area A2 are formed on the vehicle glass 1. The light-transmitting area A1 is an area occupying the central part of the vehicle glass 1 when viewed from the Z direction. The light-transmitting area A1 is an area for ensuring the driver's field of vision. The light-transmitting area A1 is an area that transmits visible light. The light-shielding area A2 is an area formed around the light-transmitting area A1 when viewed from the Z direction. The light-shielding area A2 is an area that blocks visible light. A far-infrared ray transmission area B and a visible light transmission area C are formed in the light-shielding area A2a, which is a part on the side of the upper edge 1a in the light-shielding area A2.
[0028] The far-infrared transmission area B is an area where far-infrared rays are allowed to be transmitted, and is an area where the far-infrared camera CA1 is set. That is, the far-infrared camera CA1 is set at a position overlapping with the far-infrared transmission area B when viewed from the optical axis direction of the far-infrared camera CA1. The visible light transmission area C is an area where visible light is transmitted, and is an area where the visible light camera CA2 is set. That is, the visible light camera CA2 is set at a position overlapping with the visible light transmission area C when viewed from the optical axis direction of the visible light camera CA2.
[0029] Since the far-infrared transmission area B and the visible light transmission area C are formed in the light-shielding area A2, the light-shielding area A2 blocks far infrared rays in the area other than the area where the far-infrared transmission area B is formed, and blocks visible light in the area other than the area where the visible light transmission area C is formed. The far-infrared transmission area B and the visible light transmission area C form a light-shielding area A2a around them. By providing the light-shielding area A2a around them, various sensors can be protected from sunlight, which is preferred. Since the wiring of various sensors cannot be seen from the outside of the vehicle, it is also preferred from the perspective of appearance design.
[0030] like Figure 3As shown, the vehicle glass 1 includes a glass substrate 12 (first glass substrate), a glass substrate 14 (second glass substrate), an intermediate layer 16, and a light shielding layer 18. In the vehicle glass 1, the glass substrate 12, the intermediate layer 16, the glass substrate 14, and the light shielding layer 18 are stacked in this order in the Z direction. The glass substrate 12 and the glass substrate 14 are fixed (bonded) to each other by the intermediate layer 16.
[0031] As the glass substrates 12 and 14, for example, soda-lime glass, borosilicate glass, aluminosilicate glass, etc. can be used. The intermediate layer 16 is an adhesive layer that bonds the glass substrate 12 and the glass substrate 14. As the intermediate layer 16, for example, polyvinyl butyral (hereinafter also referred to as PVB) modified materials, ethylene-vinyl acetate copolymer (EVA) materials, polyurethane resin materials, vinyl chloride resin materials, etc. can be used. In more detail, the glass substrate 12 includes a surface 12A and another surface 12B, and the other surface 12B is in contact with a surface 16A of the intermediate layer 16 and fixed (bonded) to the intermediate layer 16. The glass substrate 14 includes a surface 14A and another surface 14B, and the one surface 14A is in contact with the other surface 16B of the intermediate layer 16 and fixed (bonded) to the intermediate layer 16. It can be seen that the vehicle glass 1 is a laminated glass obtained by laminating the glass substrate 12 and the glass substrate 14. However, the vehicle glass 1 is not limited to laminated glass, and may be a structure including only one of the glass substrate 12 and the glass substrate 14. In this case, the intermediate layer 16 may not be provided. Hereinafter, when the glass substrates 12 and 14 are not distinguished, they are described as the glass substrate 10.
[0032] The light-shielding layer 18 includes a surface 18A and another surface 18B, and the surface 18A is in contact with and fixed to the other surface 14B of the glass substrate 14. The light-shielding layer 18 is a layer that blocks visible light. As the light-shielding layer 18, for example, a ceramic light-shielding layer or a light-shielding film can be used. As the ceramic light-shielding layer, for example, a ceramic layer including a conventionally known material such as a black ceramic layer can be used. As the light-shielding film, for example, a light-shielding polyethylene terephthalate (PET) film, a light-shielding polyethylene naphthalate (PEN) film, a light-shielding polymethyl methacrylate (PMMA) film, etc. can be used.
[0033] In the present embodiment, the side of the vehicle glass 1 where the light shielding layer 18 is provided is the inner side (inner side) of the vehicle V, and the side of the vehicle glass 1 where the glass substrate 12 is provided is the outer side (outer side) of the vehicle V, but the present invention is not limited thereto, and the light shielding layer 18 may be the outer side of the vehicle V. In the case of a laminated glass composed of the glass substrates 12 and 14 , the light shielding layer 18 may be formed between the glass substrates 12 and 14 .
[0034] (Shaded area)
[0035] The light-shielding region A2 is formed by providing the light-shielding layer 18 on the glass substrate 10. That is, the light-shielding region A2 is a region where the glass substrate 10 has the light-shielding layer 18. That is, the light-shielding region A2 is a region where the glass substrate 12, the intermediate layer 16, the glass substrate 14, and the light-shielding layer 18 are stacked. On the other hand, the light-transmitting region A1 is a region where the glass substrate 10 does not have the light-shielding layer 18. That is, the light-transmitting region A1 is a region where the glass substrate 12, the intermediate layer 16, and the glass substrate 14 are stacked but the light-shielding layer 18 is not stacked.
[0036] (Far infrared transmission area)
[0037] like Figure 3 As shown, the vehicle glass 1 is formed with an opening 19 that passes through one surface (here, the surface 12A) in the Z direction to the other surface (here, the surface 14B). A far-infrared ray transmitting member 20 is provided in the opening 19. The region where the opening 19 is formed and the far-infrared ray transmitting member 20 is provided is the far-infrared ray transmitting region B. That is, the far-infrared ray transmitting region B is a region where the opening 19 and the far-infrared ray transmitting member 20 arranged in the opening 19 are provided. Since the light shielding layer 18 does not allow far infrared rays to be transmitted, the light shielding layer 18 is not provided in the far-infrared ray transmitting region B. That is, in the far-infrared ray transmitting region B, the glass substrate 12, the intermediate layer 16, the glass substrate 14 and the light shielding layer 18 are not provided, but the far-infrared ray transmitting member 20 is provided in the formed opening 19. The far-infrared ray transmitting member 20 will be described later.
[0038] (Visible light region)
[0039] like Figure 4 As shown, like the light-transmitting region A1, the visible light-transmitting region C is a region where the glass substrate 10 does not have the light-shielding layer 18 in the Z direction. That is, the visible light-transmitting region C is a region where the glass substrate 12, the intermediate layer 16, and the glass substrate 14 are stacked but the light-shielding layer 18 is not stacked.
[0040] like Figure 2As shown, the visible light transmission area C is preferably arranged near the far infrared transmission area B. Specifically, the center of the far infrared transmission area B observed from the Z direction is set as the center point OB, and the center of the visible light transmission area C observed from the Z direction is set as the center point OC. When the shortest distance between the far infrared transmission area B (opening 19) and the visible light transmission area C when observed from the Z direction is set as the distance L, the distance L is preferably greater than 0 mm and less than or equal to 100 mm, and more preferably greater than 10 mm and less than 80 mm. By making the visible light transmission area C relative to the far infrared transmission area B in the range, the image of the near position can be captured by the far infrared camera CA1 and the visible light camera CA2, and the perspective distortion in the visible light transmission area C can be suppressed, so that the image can be properly captured by the visible light camera CA2. By using the far infrared camera CA1 and the visible light camera CA2 to capture the image of the near position, the load when the data obtained from each camera is calculated and processed can be reduced, and the arrangement of the power supply and signal cables also becomes appropriate.
[0041] like Figure 2 As shown in FIG. 1 , the visible light transmission region C and the far infrared transmission region B are preferably located in a position aligned along the X direction. That is, the visible light transmission region C is preferably aligned with the far infrared transmission region B in the X direction, and is not located on the Y direction side of the far infrared transmission region B. By arranging the visible light transmission region C in a manner aligned with the far infrared transmission region B in the X direction, the visible light transmission region C can be arranged near the upper edge portion 1a. Therefore, the field of vision of the driver in the light transmission region A1 can be appropriately ensured.
[0042] (Far infrared ray transmitting member)
[0043] Hereinafter, the far-infrared ray transmitting member 20 provided in the far-infrared ray transmitting region B will be specifically described. Figure 5 FIG. 4 is a cross-sectional schematic diagram of the far-infrared transmission component of this embodiment. Figure 5 As shown, the far-infrared ray transmission member 20 has a substrate 30, a first functional film 32 as a functional film formed on the substrate 30, and a second functional film 38 formed on the substrate 30. In the present embodiment, the first functional film 32 is formed on one surface 30a of the substrate 30. The surface 30a is a surface that becomes the outer side of the vehicle when it is mounted on the vehicle glass 1. In addition, the second functional film 38 is formed on the other surface 30b of the substrate 30. The surface 30b is a surface that becomes the inner side of the vehicle when it is mounted on the vehicle glass 1. However, the second functional film 38 is not an indispensable structure, and a layer other than the substrate 30 may not be provided on the surface 30b.
[0044] In the present embodiment, the far-infrared ray transmitting member 20 is provided in the light shielding area A2 of the vehicle glass 1 as a window member of the vehicle V, but is not limited thereto, and may be provided on an outer member for a pillar of the vehicle V or any outer member of the vehicle V. In addition, the far-infrared ray transmitting member 20 is not limited to being provided on the vehicle V, and may be used for any purpose.
[0045] (Base material)
[0046] The substrate 30 is a component that can transmit far-infrared rays. The internal transmittance of the substrate 30 for light with a wavelength of 10 μm (far-infrared rays) is preferably 50% or more, more preferably 60% or more, and further preferably 70% or more. In addition, the average internal transmittance of the substrate 30 for light with a wavelength of 8 μm to 12 μm (far-infrared rays) is preferably 50% or more, more preferably 60% or more, and further preferably 70% or more. By having the internal transmittance of the substrate 30 for light with a wavelength of 10 μm and the average internal transmittance for light with a wavelength of 8 μm to 12 μm within this numerical range, far-infrared rays can be appropriately transmitted, so that, for example, the performance of the far-infrared camera CA1 can be fully utilized. It should be noted that the average internal transmittance here refers to the average value of the internal transmittance of light of each wavelength in the band (here 8 μm to 12 μm).
[0047] The internal transmittance of the substrate 30 is the transmittance after deducting the surface reflection losses on the incident side and the emission side, and is well known in the art, and can be measured by a commonly performed method. The measurement is performed, for example, as follows.
[0048] A pair of flat plate samples (first sample and second sample) composed of substrates of the same composition and different thicknesses are prepared. The two surfaces of the flat plate samples are parallel to each other and optically polished planes. The external transmittance of the first sample including surface reflection loss is set to T1, the external transmittance of the second sample including surface reflection loss is set to T2, the thickness of the first sample is set to Td1 (mm), and the thickness of the second sample is set to Td2 (mm), where Td1 < Td2. At this time, the internal transmittance τ at the thickness Tdx (mm) can be calculated by the following formula (1).
[0049]
[0050] In addition, the external transmittance of infrared light can be measured by, for example, a Fourier transform infrared spectrometer (manufactured by ThermoScientific, trade name: Nicolet iS10).
[0051] The refractive index of the substrate 30 for light with a wavelength of 10 μm is preferably 1.5 or more and 4.0 or less, more preferably 2.0 or more and 4.0 or less, and further preferably 2.2 or more and 3.5 or less. In addition, the average refractive index of the substrate 30 for light with a wavelength of 8 μm to 12 μm is preferably 1.5 or more and 4.0 or less, more preferably 2.0 or more and 4.0 or less, and further preferably 2.2 or more and 3.5 or less. By having the refractive index and average refractive index of the substrate 30 within this numerical range, far infrared rays can be properly transmitted, so that, for example, the performance of the far infrared camera CA1 can be fully utilized. It should be noted that the average refractive index here refers to the average value of the refractive index of light of each wavelength in the band (here 8 μm to 12 μm). The refractive index can be determined, for example, by fitting an optical model using polarization information obtained using an infrared spectroscopic ellipsometer (manufactured by JA Woollam, IR-VASE-UT) and a spectral transmission spectrum obtained using a Fourier transform infrared spectrometer.
[0052] The thickness D1 of the substrate 30 is preferably 0.5 mm or more and 5 mm or less, more preferably 1 mm or more and 4 mm or less, and further preferably 1.5 mm or more and 3 mm or less. When the thickness D1 is within this range, the strength can be ensured and far infrared rays can be appropriately transmitted. It should be noted that the thickness D1 can also be said to be the length in the Z direction from the surface 30a of the substrate 30 to the surface 30b.
[0053] The material of the substrate 30 is not particularly limited, and examples thereof include Si, Ge, ZnS, and chalcogenide glass. It can be said that the substrate 30 preferably includes at least one material selected from the group consisting of Si, Ge, ZnS, and chalcogenide glass. By using such a material in the substrate 30, far infrared rays can be appropriately transmitted.
[0054] The preferred composition of the chalcogenide glass is as follows, expressed in atomic %, containing: Ge+Ga: 7% to 25%, Sb: 0% to 35%, Bi: 0% to 20%, Zn: 0% to 20%, Sn: 0% to 20%, Si: 0% to 20%, La: 0% to 20%, S+Se+Te: 55% to 80%, Ti: 0.005% to 0.3%, Li+Na+K+Cs: 0% to 20%, F+Cl+Br+I: 0% to 20%. In addition, the glass preferably has a glass transition temperature (Tg) of 140° C. to 550° C.
[0055] It should be noted that Si and ZnS are more preferably used as the material of the substrate 30 .
[0056] (First functional film)
[0057] The first functional film 32 is formed on the surface 30a of the vehicle outer side of the substrate 30. The first functional film 32 includes an intermediate layer 34 and an outermost layer 36. The outermost layer 36 is a layer disposed at a position farthest from the substrate 30 in the first functional film 32, that is, a layer closest to the vehicle outer side in this embodiment. In other words, the outermost layer 36 is a layer at the outermost side of the far-infrared ray transmitting member 20 (the outermost side of the vehicle in this embodiment), and is exposed to the outside.
[0058] The intermediate layer 34 is a layer provided on the substrate 30 side of the outermost layer 36 in the first functional film 32 (in the present embodiment, on the vehicle interior side of the outermost layer 36). That is, the intermediate layer 34 is provided between the substrate 30 and the outermost layer 36. However, the first functional film 32 may not include the intermediate layer 34, and may include only the outermost layer 36.
[0059] (Outermost layer)
[0060] The outermost layer 36 is made of ZrO 2 The main component here means that the content of ZrO in the outermost layer 36 is 50% by mass or more relative to the entire outermost layer 36. 2 The content of ZrO is 50% by mass or more and 100% by mass or less, preferably 70% by mass or more and 100% by mass or less, and more preferably 90% by mass or more and 100% by mass or less. 2 , that is, except for unavoidable impurities, ZrO 2 The content of ZrO is 100 mass%. 2 When the content of is within this range, the outermost layer 36 can appropriately transmit far infrared rays and can improve scratch resistance.
[0061] The outermost layer 36 may contain a secondary component, which is ZrO in addition to the primary component. 2 As the auxiliary component, an oxide that transmits far infrared rays is preferred, and examples thereof include NiO X 、ZnO、Bi 2 O 3 and CuO x At least one of .
[0062] The thickness D2 of the outermost layer 36 is preferably 20 nm or more, more preferably 50 nm or more and 300 nm or less, further preferably 100 nm or more and 300 nm or less, and most preferably 150 nm or more and 250 nm or less. It should be noted that the thickness D2 can be said to be the length in the Z direction from the surface of the outermost layer 36 on the Z direction side to the surface on the side opposite to the Z direction.
[0063] The ratio of the thickness D2 of the outermost layer 36 to the thickness D1 of the substrate 30 is preferably 0.002% to 0.030%, more preferably 0.005% to 0.020%, and further preferably 0.008% to 0.013%.
[0064] In addition, the ratio of the thickness D2 of the outermost layer 36 to the thickness D3 of the first functional film 32 is preferably 1% or more and 25% or less, more preferably 3% or more and 25% or less, further preferably 5% or more and 25% or less, and most preferably 7% or more and 21% or less. It should be noted that the thickness D3 of the first functional film 32 can be said to be the length in the Z direction from the surface of the first functional film 32 on the Z direction side to the surface on the side opposite to the Z direction.
[0065] When the thickness D2 is within this range, far infrared rays can be appropriately transmitted and scratch resistance can be appropriately improved.
[0066] The surface of the outermost layer 36 on the opposite side to the substrate 30 is referred to as the surface 36a. The surface 36a is the surface on the side exposed to the outside, and in the present embodiment, it can be said to be the surface on the outside of the vehicle. In this case, the arithmetic mean roughness Ra (surface roughness) of the surface 36a of the outermost layer 36 is preferably 7.0 nm or less, more preferably 5.0 nm or less, further preferably 4.0 nm or less, and most preferably 3.0 nm or less. By making the arithmetic mean roughness Ra of the surface 36a within this range, the change in the dynamic friction coefficient and the surface roughness before and after scratching can be reduced, and the scratch resistance can be more appropriately improved. It should be noted that the arithmetic mean roughness Ra refers to the arithmetic mean roughness Ra specified in JIS B 0601:2001.
[0067] The outermost layer 36 can transmit far infrared rays. The extinction coefficient of the outermost layer 36 for light of a wavelength of 10 μm is preferably 0.10 or less, more preferably 0.05 or less, and further preferably 0.04 or less. The extinction coefficient can be determined, for example, by fitting an optical model using polarization information obtained using an infrared spectroscopic ellipsometer (manufactured by JA Woollam, IR-VASE-UT) and a spectral transmission spectrum obtained using a Fourier transform infrared spectrometer.
[0068] The refractive index of the outermost layer 36 for light (visible light) with a wavelength of 550 nm is preferably 2.05 or more, more preferably 2.05 or more and 2.40 or less, further preferably 2.10 or more and 2.30 or less, and particularly preferably 2.15 or more and 2.25 or less. When the refractive index of the outermost layer 36 for visible light is within this numerical range, the density of the film of the outermost layer 36 can be improved, and the scratch resistance can be more appropriately improved. The refractive index of light with a wavelength of 550 nm can be determined, for example, by fitting an optical model using polarization information obtained using a spectroscopic ellipsometer (manufactured by JA Woollam, M-2000) and spectral transmittance measured based on JIS R3106.
[0069] (Middle layer)
[0070] The intermediate layer 34 can transmit far infrared rays. In the example of the present embodiment, the intermediate layer 34 includes an anti-reflection layer. In the following description, an example in which the intermediate layer 34 is composed of only one anti-reflection layer is described, but the intermediate layer 34 is not limited thereto, and the intermediate layer 34 may be composed of a plurality of layers stacked.
[0071] (Anti-reflection layer)
[0072] The anti-reflection layer contained in the intermediate layer 34 is made of NiO X The main component of the anti-reflection layer is 50% by mass or more. X The content of NiO is 50% by mass or more and 100% by mass or less, preferably 70% by mass or more and 100% by mass or less, and more preferably 90% by mass or more and 100% by mass or less. X , that is, except for unavoidable impurities, NiO X The content of NiO is 100 mass%. X When the content of is within this range, the antireflection layer can suppress reflection of far-infrared rays and appropriately transmit far-infrared rays.
[0073] It should be noted that nickel oxide is known to have various compositions depending on the valence of nickel, and X can take any value in the range of 0.5 to 2. In addition, the valence may not be a single one, but may be a mixture of two or more valences. In this embodiment, as NiO X , NiO is preferably used. However, the material of the anti-reflection layer is not limited thereto, and is arbitrary, for example, it can be a material containing ZnS, Ge, Si, MgO, ZnO and Bi 2 O 3 at least one layer of.
[0074] The thickness of the anti-reflection layer contained in the intermediate layer 34 is preferably 1000nm or more and 2000nm or less, more preferably 1000nm or more and 1500nm or less, and further preferably 1100nm or more and 1300nm or less. In addition, the ratio of the thickness of the anti-reflection layer to the thickness D2 of the outermost layer 36 is preferably 75% or more and 99% or less, more preferably 75% or more and 97% or less, further preferably 75% or more and 95% or less, and most preferably 79% or more and 93% or less. By the thickness of the anti-reflection layer being within this range, the reflection of far infrared rays can be suppressed and far infrared rays can be appropriately transmitted. It should be noted that the thickness of the anti-reflection layer can also be said to be the length in the Z direction from the surface on the Z direction side of the anti-reflection layer to the surface on the side opposite to the Z direction.
[0075] The anti-reflection layer included in the intermediate layer 34 can transmit far infrared rays. The extinction coefficient of the anti-reflection layer for light with a wavelength of 10 μm is preferably 0.05 or less, more preferably 0.03 or less, further preferably 0.02 or less, and most preferably 0.01 or less. When the extinction coefficient is within this range, far infrared rays can be appropriately transmitted.
[0076] The extinction coefficient of the anti-reflection layer contained in the intermediate layer 34 for light (visible light) with a wavelength of 550 nm is preferably 0.04 or more, more preferably 0.06 or more, further preferably 0.08 or more, and most preferably 0.10 or more. When the extinction coefficient of the anti-reflection layer for visible light is within this numerical range, the reflectance dispersion of visible light can be appropriately suppressed, and an appearance with guaranteed design properties can be achieved.
[0077] (Hue adjustment layer)
[0078] As described above, the intermediate layer 34 may also be provided with a layer other than the anti-reflection layer. In this case, for example, the intermediate layer 34 may be provided with a hue adjustment layer on the side of the outermost layer 36 of the anti-reflection layer. That is, it can be said that in this case, the substrate 30, the anti-reflection layer, the hue adjustment layer, and the outermost layer 36 are stacked in the order of the substrate 30, the anti-reflection layer, the hue adjustment layer, and the outermost layer 36 toward the vehicle outer side. The hue adjustment layer is specifically described below.
[0079] The hue adjustment layer included in the intermediate layer 34 is a layer for suppressing interference color of the far-infrared transmissive member 20 by reducing the difference in reflectance (reflectance dispersion) with respect to visible light of different wavelengths, thereby ensuring design properties.
[0080] The hue adjustment layer included in the intermediate layer 34 can transmit far infrared rays. The extinction coefficient of the hue adjustment layer for light of a wavelength of 10 μm is preferably 0.4 or less, more preferably 0.2 or less, and further preferably 0.1 or less. When the extinction coefficient is within this range, far infrared rays can be appropriately transmitted.
[0081] The thickness of the hue adjustment layer contained in the intermediate layer 34 is preferably 5 nm or more and 100 nm or less, more preferably 10 nm or more and 60 nm or less, and further preferably 20 nm or more and 50 nm or less. In addition, the ratio of the thickness of the hue adjustment layer to the thickness D2 of the outermost layer 36 is preferably 2.5% or more and 100% or less, more preferably 5% or more and 50% or less, further preferably 10% or more and 30% or less, and most preferably 10% or more and 25% or less. By making the thickness of the hue adjustment layer within this range, far infrared rays can be appropriately transmitted, and at the same time, the reflection and dispersion of visible light can be suppressed to make the far infrared transmission component 20 inconspicuous. It should be noted that the thickness of the hue adjustment layer can also be said to be the length in the Z direction from the surface of the hue adjustment layer on the Z direction side to the surface on the side opposite to the Z direction.
[0082] In the present embodiment, the color phase adjustment layer included in the intermediate layer 34 includes a first layer and a second layer provided on the outermost layer 36 side (vehicle outer side) of the first layer.
[0083] In the present embodiment, the first layer is a layer whose material and characteristics are the same as those of the outermost layer 36. The thickness of the first layer is preferably 10 nm or more and 40 nm or less, more preferably 15 nm or more and 35 nm or less, and further preferably 20 nm or more and 30 nm or less. In addition, the ratio of the thickness of the first layer to the thickness D2 of the outermost layer 36 is preferably 1.5% or more and 60% or less, more preferably 3% or more and 30% or less, further preferably 6% or more and 20% or less, and most preferably 6% or more and 15% or less.
[0084] In this embodiment, the second layer is a layer whose material and characteristics are the same as those of the anti-reflection layer contained in the intermediate layer 34. The thickness of the second layer is preferably 5 nm or more and 40 nm or less, more preferably 5 nm or more and 25 nm or less, and further preferably 10 nm or more and 20 nm or less. In addition, the ratio of the thickness of the second layer to the thickness D2 of the outermost layer 36 is preferably 1% or more and 40% or less, more preferably 2% or more and 20% or less, further preferably 4% or more and 12% or less, and most preferably 4% or more and 10% or less.
[0085] It should be noted that in this example, the hue adjustment layer is composed of two layers, the first layer and the second layer, but is not limited to this. Multiple layers may also be stacked in the stack of the first layer and the second layer. The hue adjustment layer is preferably a layer obtained by alternately stacking 2n (n is a natural number greater than 1) layers of the first layer and the second layer from the substrate 30 side. For the film thickness ratio of each layer in the hue adjustment layer, a layer height with a low refractive index for light (visible light) with a wavelength of 550nm is preferred. By keeping the stacking order and the number of layers of the hue adjustment layer within this range, the reflection dispersion of visible light can be suppressed and the far-infrared transmission component 20 can be made inconspicuous.
[0086] The composition of the hue adjustment layer is not limited to a composition including a first layer of the same material as the outermost layer 36 and a second layer of the same material as the anti-reflection layer, and may be any composition. That is, the hue adjustment layer may also be a layer whose refractive index for light (visible light) of a wavelength of 550nm is different from that of both the outermost layer 36 and the anti-reflection layer. The refractive index of the hue adjustment layer for light (visible light) of a wavelength of 550nm is preferably greater than 2.2 and less than 2.5, and more preferably greater than 2.3 and less than 2.4. By having the refractive index of the hue adjustment layer for visible light within this numerical range, the reflection dispersion of visible light can be suppressed and the far-infrared transmission component 20 can be made inconspicuous.
[0087] (Second functional film)
[0088] The second functional film 38 provided on the surface 30b on the vehicle interior side of the substrate 30 is a layer that allows far infrared rays to be transmitted. The configuration of the second functional film 38 may be the same as that of the intermediate layer 34. That is, for example, in the far infrared ray transmitting member 20, the substrate 30 and the anti-reflection layer may be stacked in the order of the substrate 30 and the anti-reflection layer from the substrate 30 to the vehicle interior side. In addition, for example, in the far infrared ray transmitting member 20, the substrate 30, the anti-reflection layer, and the hue adjustment layer (first layer, second layer) may also be stacked in the order of the substrate 30, the anti-reflection layer, and the hue adjustment layer (first layer, second layer) from the substrate 30 to the vehicle interior side.
[0089] (Adhesive film)
[0090] In addition, an adhesive layer (not shown) may be formed between the intermediate layer 34 and the base material 30. The adhesive film is a film that allows the base material 30 and the intermediate layer 34 to adhere to each other, in other words, a film that improves the adhesive force between the base material 30 and the intermediate layer 34.
[0091] The refractive index of the adhesive film for light of a wavelength of 10 μm is preferably 1.0 to 4.3, more preferably 1.5 to 4.3, and even more preferably 1.5 to 3.8. When the refractive index is within this range, reflection of far infrared rays can be appropriately suppressed.
[0092] In addition, the thickness of the adhesive film is preferably 0.05 μm or more and 0.5 μm or less, more preferably 0.05 μm or more and 0.3 μm or less, and further preferably 0.05 μm or more and 0.1 μm or less. When the thickness of the adhesive film is within this range, the reflection of far infrared rays can be appropriately suppressed while the substrate 30 and the intermediate layer 34 can be appropriately adhered. It should be noted that the thickness of the adhesive film can be said to be the length in the Z direction from the surface of the Z direction side of the adhesive film to the surface on the side opposite to the Z direction. In addition, the thickness of the adhesive film is preferably thinner than the thickness of the intermediate layer 34 and the thickness D2 of the outermost layer 36. When the thickness of the adhesive film is thinner than the thickness of these layers, the influence on the optical performance can be reduced.
[0093] The adhesive film can transmit far infrared rays. The extinction coefficient of the adhesive film for light with a wavelength of 10 μm is preferably 0.4 or less, more preferably 0.2 or less, and further preferably 0.1 or less. When the extinction coefficient is within this range, far infrared rays can be appropriately transmitted.
[0094] The material of the adhesive film is arbitrary, and preferably contains a material selected from Si, Ge, MgO, NiO X , CuO x 、ZnS、Al 2 O 3 、ZrO 2 、SiO 2 、TiO 2 , ZnO and Bi 2 O 3 At least one material selected from the group consisting of ZrO 2 By using such a material, the adhesive film can appropriately adhere the base material 30 and the intermediate layer 34.
[0095] It should be noted that the adhesive film may be formed by sputtering similarly to the intermediate layer 34 , but is not limited thereto and may be formed by, for example, vapor deposition.
[0096] (Characteristics of far-infrared transmitting member)
[0097] As described above, the far infrared transmission member 20 has the first functional film 32 having the outermost layer 36 formed on the surface 30a of the base 30. By forming the outermost layer 36, the far infrared transmission member 20 can appropriately transmit far infrared rays while appropriately improving scratch resistance.
[0098] The transmittance of the far-infrared ray transparent member 20 to light with a wavelength of 10 μm is preferably 50% or more, more preferably 65% or more, and further preferably 70% or more. In addition, the average transmittance of the far-infrared ray transparent member 20 to light with a wavelength of 8 μm to 12 μm is preferably 50% or more, more preferably 65% or more, and further preferably 70% or more. When the transmittance and the average transmittance are within this range, the function as an infrared ray transparent member can be appropriately exerted.
[0099] The reflectivity of the far-infrared ray transmitting component 20 to light with a wavelength of 10 μm is preferably 15% or less, more preferably 10% or less, and further preferably 5% or less. In addition, the average reflectivity of the far-infrared ray transmitting component 20 to light with a wavelength of 8 μm to 12 μm is preferably 15% or less, more preferably 10% or less, and further preferably 5% or less. By having the reflectivity and average reflectivity within this range, the function as an infrared ray transmitting component can be properly exerted. It should be noted that the average reflectivity refers to the average value of the reflectivity of light of each wavelength in the band (here 8 μm to 12 μm). The reflectivity can be measured, for example, using a Fourier transform infrared spectrometer (manufactured by Thermo Scientific, Nicolet iS10).
[0100] The indentation hardness of the surface 20A (i.e., the surface 36a of the outermost layer 36) of the far-infrared ray transmitting member 20 on the vehicle outer side is preferably 9.0 GPa or more, more preferably 10.0 GPa or more, further preferably 11.0 GPa or more, particularly preferably 12.0 GPa or more, and most preferably 13.0 GPa or more when the indentation depth is within the range of 90 nm or more and 110 nm or less. When the indentation hardness of the surface 20A is within this range, the scratch resistance can be appropriately improved.
[0101] The indentation hardness of the surface 20A refers to the indentation hardness (indentation hardness) within the range of 90 nm to 110 nm indentation depth measured by a nanoindenter by a nanoindentation method (continuous stiffness measurement method). More specifically, the indentation hardness refers to the value obtained by measuring the displacement-load curve of the indenter from the application of a load to the removal of a load, and is specified in ISO14577.
[0102] The indentation hardness can be measured as follows. Specifically, the indentation depth h (nm) corresponding to the indentation load P (mN) is continuously measured from the start of the load application to the removal of the load at the measurement site using an iMicro nanoindenter manufactured by KLA, thereby creating a Ph curve. Then, based on the created Ph curve, the indentation hardness H (GPa) is calculated as shown in the following formula (2).
[0103] H=P / A・・・(2)
[0104] In formula (2), P is the indentation load (mN), A is the projected area of the indenter (μm 2 ).
[0105] In the present embodiment, the indentation hardness H in the range of indentation depth of 90 nm to 110 nm is taken as the indentation hardness of the surface 20A. That is, in the present embodiment, it can be said that the indentation hardness H preferably satisfies the above range in the entire range of indentation depth of 90 nm to 110 nm.
[0106] Δa of the far-infrared ray transmitting member 20 * b * It is preferably 5 or less, more preferably 4 or less, further preferably 3 or less, particularly preferably 2 or less, and most preferably 1 or less. Δa * b * Refers to the a in the CIE-Lab color system obtained by the 5-degree incident visible light reflection spectrum. * b * The distance from the origin coordinate. That is, Δa * b * It is calculated by the following formula (3). * b * In this range, the visible light reflected from the far-infrared transmissive member 20 becomes a neutral color, and an appearance with secured design properties can be achieved.
[0107] Δa * b * =(a *2 +b *2 ) 0.5 ・・・(3)
[0108] a * and b * It is the chromaticity coordinate of reflected light in the CIE-Lab colorimetric system when the standard light source D65 is used as the illumination light, and can be calculated based on JIS Z 8781-4 using the spectral reflectance measured based on JIS R3106.
[0109] In particular, the far infrared ray transmitting member 20 has NiO whose extinction coefficient in the visible light region changes depending on the degree of oxidation. X In the case of a film, it is possible to suppress the NiO accompanying the humidity test, water resistance test, and heat resistance test. X The oxidation degree of the film varies with a * and b * changes.
[0110] In addition, preferably Figure 3The surface 20A of the vehicle outer side of the far-infrared transmission component 20 shown is formed flush (continuously) with the surface of the vehicle outer side of the shading area A2. In other words, the far-infrared transmission component 20 is installed in a manner that the surface 20A of the vehicle outer side is continuous with the surface 12A of the glass substrate 12. By making the surface 20A of the far-infrared transmission component 20 continuous with the surface 12A of the glass substrate 12 in this way, it is possible to suppress the wiping effect of the wiper from being impaired. In addition, it is possible to suppress the possibility of damaging the design of the vehicle V due to the existence of the height difference, and the accumulation of sand and dust at the height difference. In addition, the far-infrared transmission component 20 is preferably molded in accordance with the curved surface shape of the vehicle glass 1 to which it is applied. There is no particular limitation on the molding method of the far-infrared transmission component 20, and grinding or mold molding can be selected according to the curved surface shape and the component.
[0111] The shape of the far-infrared transmission member 20 is not particularly limited, but it is preferably a plate-like shape that matches the shape of the opening 19. That is, for example, when the opening 19 is circular, the far-infrared transmission member 20 is preferably a disk-like shape (cylindrical shape). In addition, from the perspective of appearance design, the surface shape of the far-infrared transmission member 20 on the outside of the vehicle can be processed to match the curvature of the outer surface shape of the glass substrate 12. In addition, for reasons such as widening the viewing angle of the far-infrared camera CA1 and improving mechanical properties, the far-infrared transmission member 20 can be made into a lens shape. When such a structure is made, even if the area of the far-infrared transmission member 20 is small, far-infrared light can be effectively focused, so it is preferred. In this case, the number of lens-shaped far-infrared transmission members 20 is preferably 1 to 3, and typically preferably 2. In addition, the lens-shaped far-infrared transmission member 20 is particularly preferably pre-aligned and made into a module, and integrated with a housing or bracket that bonds the far-infrared camera CA1 to the vehicle glass 1.
[0112] In the vehicle glass 1 of the present embodiment, it is preferred to have a structure in which the area of the opening 19 on the surface on the vehicle inner side is smaller than the area of the opening 19 on the surface on the vehicle outer side, and the shape of the far-infrared ray transmission member 20 is also corresponding to the area on the surface on the vehicle inner side is smaller than the area on the surface on the vehicle outer side. By making such a structure, the strength against the impact from the vehicle outer side is improved. Further, in the case where the vehicle glass 1 of the present embodiment is a laminated glass having a glass substrate 12 (vehicle outer side) and a glass substrate 14 (vehicle inner side), the opening 19 is formed by overlapping the opening 12a of the glass substrate 12 and the opening 14a of the glass substrate 14. In this case, the area of the opening 12a of the glass substrate 12 can be made larger than the area of the opening 14a of the glass substrate 14, and the far-infrared ray transmission member 20 having the same size as the opening 12a of the glass substrate 12 is arranged in the opening 12a of the glass substrate 12.
[0113] In addition, if Figure 3 As shown, in the far infrared ray transmitting member 20, the length d1 of the longest straight line connecting any two points in the surface of the vehicle outer side is preferably 80 mm or less. The length d1 is more preferably 70 mm or less, and further preferably 65 mm or less. In addition, the length d1 is preferably 60 mm or more. In addition, as Figure 3 As shown, in the opening 19 of the far-infrared transmission area B, the length d2 of the longest straight line connecting any two points in the surface on the outside of the vehicle is preferably 80 mm or less. The length d2 is more preferably 70 mm or less, and further preferably 65 mm or less. In addition, the length d2 is preferably 60 mm or more. The length d2 can also be said to be the length of the longest straight line connecting any two points on the outer periphery of the opening 19 on the surface (surface 12A) on the outside of the vehicle of the vehicle glass 1. By keeping the length d1 of the far-infrared transmission component 20 and the length d2 of the opening 19 within this range, the reduction in the strength of the vehicle glass 1 can be suppressed, and the perspective distortion around the opening 19 can also be suppressed. It should be noted that when the shape of the surface on the outside of the vehicle of the far-infrared transmission component 20 is circular, the lengths d1 and d2 are lengths equivalent to the diameter of the surface on the outside of the vehicle. In addition, the lengths d1 and d2 herein refer to the lengths when the vehicle glass 1 is mounted on the vehicle V. For example, when the glass is bent into a shape to be mounted on the vehicle V, the lengths d1 and d2 are the lengths after the bending process. The same applies to the description of dimensions and positions other than the lengths d1 and d2 unless otherwise specified.
[0114] (Method for manufacturing far-infrared transmitting member)
[0115] Next, the manufacturing method of the far-infrared ray transmitting member 20 is described. When manufacturing the far-infrared ray transmitting member 20, a substrate 30 is prepared, and a first functional film 32 is formed on the surface of the substrate 30. The method for forming the first functional film 32 is arbitrary, but in this embodiment, the first functional film 32 is formed on the surface of the substrate 30 by sputtering. That is, in the example of this embodiment, the intermediate layer 34 is formed on the surface of the substrate 30 by sputtering. Then, the outermost layer 36 is formed on the surface of the substrate 30, that is, on the surface of the intermediate layer 34 here, by sputtering. In this way, the far-infrared ray transmitting member 20 is manufactured. By forming the first functional film 32 by sputtering, the adhesion of the film can be improved. It should be noted that in this embodiment, the second functional film 38 is formed on the surface of the substrate 30 on the opposite side of the first functional film 32 by sputtering.
[0116] It should be noted that the sputtering method may be any method, for example, reactive sputtering or post-oxidation sputtering may be used, and post-oxidation sputtering is preferably used.
[0117] Figure 6 Schematic diagram for explaining the manufacturing method of the far-infrared ray transmitting member of the present embodiment. Hereinafter, although the case where the outermost layer 36 is directly formed on the substrate 30 is taken as an example, in the case where the outermost layer 36 is formed on the intermediate layer 34, the same method as that in the following can be applied except that the substrate 30 having the outermost layer 36 formed on the surface is used.
[0118] like Figure 6 As shown, in the post-oxidation sputtering method, a substrate 30 is arranged in the first space SP1 (step S10). A target T is provided in the first space SP1 and is connected to an inert gas supply unit M1. The target T is a member that is a raw material for the outermost layer 36 stacked on the substrate 30. The substrate 30 is arranged in the first space SP1 in such a manner that the surface 30a on the side forming the outermost layer 36 is opposite to the target T. The inert gas supply unit M1 is a device that supplies an inert gas G into the first space SP1, so that the first space SP1 becomes an inert gas G atmosphere. As the inert gas G, argon gas can be used, but it is not limited thereto. For example, a rare gas other than argon gas can also be used.
[0119] The substrate 30 is arranged in the first space SP1, and then an inert gas G is introduced into the first space SP1 where the target T and the substrate 30 are arranged, thereby performing sputtering, so that Zr contained in the target T is stacked on the surface 30a of the substrate 30 (step S12; stacking step). Specifically, in this step, in a state where the first space SP1 is made vacuous, an inert gas G is introduced into the first space SP1 from the inert gas supply unit M1. Then, by applying a negative voltage to the target T, the inert gas G is ionized, and the ionized inert gas G is caused to collide with the surface of the substrate 30. As a result, the components (atoms, molecules) contained in the target T, in this case, Zr contained in the target T, are ejected from the target T and stacked on the surface 30a of the substrate 30. Hereinafter, the stack containing Zr stacked on the surface 30a of the substrate 30 is described as a stack 36A.
[0120] It should be noted that the component ejected from the target T and stacked in the form of the stacked body 36A is not limited to Zr, and other atoms, molecules, and other components contained in the target T (such as ZrO 2 ) may also be ejected from the target T and stacked in the form of a stacked body 36A. That is, the stacked body 36A can be said to be a layer containing at least Zr.
[0121] In the lamination step, as described above, the inert gas G is introduced into the first space SP1 while the first space SP1 is in a vacuum state. The vacuum here may refer to, for example, a pressure of 10 Pa or less, and the same applies thereto. In addition, in the lamination step, the inert gas G is preferably introduced in such a manner that the pressure in the first space SP1 is preferably less than 0.5 Pa, more preferably less than 0.4 Pa, and further preferably less than 0.3 Pa. That is, in this step, it is preferably set so that the air pressure in the first space SP1 containing the inert gas G is within the above range. By setting the first space SP to such an air pressure, a high-hardness laminate 36A can be formed, and scratch resistance can be improved.
[0122] Next, the base material 30 on which the stacked body 36A is stacked is disposed in the second space SP2 (step S14). The oxygen supply unit M2 is connected to the second space SP2. The oxygen supply unit M2 is a device for supplying oxygen O.
[0123] The substrate 30 is arranged in the second space SP2, and then oxygen plasma (plasma-like oxygen) is generated in the second space SP2, thereby oxidizing the stacked body 36A stacked on the substrate 30, thereby forming the outermost layer 36 on the substrate 30 (step S16; oxidation step). Specifically, in a state where the second space SP2 is made into a vacuum, oxygen O is supplied from the oxygen supply unit M2 into the second space SP2, and the oxygen O in the second space SP2 is plasma-formed, thereby generating oxygen plasma. In the second space SP2, the generated oxygen plasma contacts the stacked body 36A stacked on the substrate 30 and oxidizes the stacked body 36A, thereby forming the outermost layer 36 on the substrate 30. That is, Zr contained in the stacked body 36A is oxidized by the oxygen plasma to become ZrO 2 It is believed that the volume expansion of the film during the oxidation process increases the density and thus increases the hardness. 2 The outermost layer 36 is formed on the substrate 30 by forming the outermost layer 36 as the main component. It should be noted that not only oxygen plasma but also oxygen radicals and oxygen ions may be generated to perform oxidation.
[0124] Target T contains Zr. The content of Zr in target T relative to the entire target T is preferably 50 atomic % or more and 100 atomic % or less, more preferably 60 atomic % or more and 100 atomic % or less, 70 atomic % or more and 100 atomic % or less, or 80 atomic % or more and 100 atomic % or less. By setting the content of Zr in target T within this range, the volume expansion rate of the film in the oxidation process can be increased, and a high-hardness outermost layer 36 can be formed due to the increased film density, and scratch resistance can be improved. It should be noted that target T may contain ZrO as a component other than Zr. 2 .
[0125] In the oxidation step, oxygen plasma can be generated by any method. For example, an electrode can be provided in the second space SP2, and a voltage can be applied to the electrode, thereby plasmatizing the oxygen O in the second space SP2, thereby generating oxygen plasma. In this case, the power applied to the electrode is preferably 2 kW or more and 4 kW or less, and more preferably 3 kW or more and 4 kW or less. By setting the applied power within the above range, Zr can be appropriately oxidized to form the outermost layer 36 with high hardness, and the scratch resistance can be improved.
[0126] In the present embodiment, the outermost layer 36 may be formed so as to gradually become thicker by repeating the processes of step S10 to step S16 .
[0127] It should be noted that, in the present embodiment, the first space SP1 and the second space SP2 are different isolated spaces (chambers), and the above-mentioned stacking step and oxidation step are performed while the substrate 30 is moved from the first space SP1 to the second space SP2 or from the second space SP2 to the first space SP1, thereby forming the outermost layer 36. The method of moving the substrate 30 between the first space SP1 and the second space SP2 can be arbitrary, for example, the substrate 30 can be mounted on the surface of a rotatable drum to form the first space SP1 and the second space SP2 in a manner arranged in the rotation direction of the drum. In this case, the substrate 30 moves from the first space SP1 to the second space SP2 (or from the second space SP2 to the first space SP1) by the rotation of the drum.
[0128] In addition, the first space SP1 and the second space SP2 may be the same space (chamber). In this case, a vacuum may be formed with the substrate 30 disposed in the space, and then a voltage may be applied to the target T while the inert gas G is introduced to perform sputtering, and then oxygen plasma may be supplied into the space to oxidize the stack 36A to form the outermost layer 36.
[0129] In the present embodiment, the outermost layer 36 is preferably formed on the surface of the substrate 30 by sputtering under the conditions of a specified pressure and a specified temperature. The specified pressure here is preferably 0.5 Pa or less, more preferably 0.1 Pa or more and 0.3 Pa or less, and further preferably 0.15 Pa or more and 0.25 Pa or less. By setting the sputtering conditions in this way, the refractive index of the outermost layer 36 can be increased, the indentation hardness can be increased, the arithmetic mean roughness can be reduced, and the scratch resistance can be more appropriately improved. It should be noted that the specified pressure can also be applied when forming layers other than the outermost layer 36.
[0130] (Effect)
[0131] As described above, the far-infrared ray transmitting member 20 of this embodiment includes a substrate 30 that allows far-infrared rays to be transmitted and a first functional film 32 (functional film) formed on the substrate 30. The far-infrared ray transmitting member 20 has an average transmittance of light of a wavelength of 8 μm to 12 μm of 50% or more. The outermost layer 36 of the first functional film 32 is made of ZrO 2 The layer as the main component has ZrO in the entire outermost layer 36. 2 The content of is 50 mass % or more and 100 mass % or less, and the refractive index of the outermost layer 36 of the first functional film 32 with respect to light of a wavelength of 550 nm is 2.05 or more.
[0132] Here, the far-infrared ray transmitting member is required to appropriately transmit far-infrared rays and improve scratch resistance. 2 The outermost layer 36 as the main component can appropriately transmit far infrared rays and improve scratch resistance. Further, for example, diamond-like carbon (DLC) can also improve scratch resistance, but the film forming process of DLC is limited and the elastic modulus needs to be controlled, so the load in the film forming process becomes high. In contrast, by using ZrO as in this embodiment, 2 The outermost layer 36 as a main component can reduce the load in the film forming process and improve the scratch resistance.
[0133] The extinction coefficient of the outermost layer 36 for light having a wavelength of 10 μm is preferably 0.10 or less. When the extinction coefficient of the outermost layer 36 is within this range, far infrared rays can be appropriately transmitted.
[0134] The thickness D2 of the outermost layer 36 is preferably 20 nm or more. When the thickness D2 of the outermost layer 36 is within this range, far infrared rays can be appropriately transmitted and scratch resistance can be improved.
[0135] The arithmetic mean roughness Ra of the surface 36a of the outermost layer 36 is preferably 7.0 nm or less. When the surface roughness is within this range, the dynamic friction coefficient and the change in surface roughness before and after scratching can be reduced, and the scratch resistance can be more appropriately improved.
[0136] The refractive index of the outermost layer 36 for light with a wavelength of 550 nm is preferably 2.05 or more. When the refractive index is within this range, the density of the film of the outermost layer 36 can be improved, and the scratch resistance can be more appropriately improved. In order to make the refractive index of the outermost layer 36 for light with a wavelength of 550 nm be 2.05 or more, it is effective to increase the film forming energy. Specifically, sputtering within a pressure range of 0.5 Pa or less, close-range sputtering with the distance between the target and the substrate 30 set to 100 mm or less, film forming in a high temperature region of 200° C. or more, ion beam treatment during film forming, etc. can be cited.
[0137] Δa of the far-infrared ray transmitting member 20 * b * It is preferably 5 or less. * b * In this range, the visible light reflected from the far-infrared transmissive member 20 becomes a neutral color, and an appearance with secured design properties can be achieved.
[0138] The ratio of the thickness D2 of the outermost layer 36 to the thickness D1 of the substrate 30 is preferably 0.002% or more and 0.030% or less. When the thickness D2 is within such a range, far infrared rays can be appropriately transmitted and scratch resistance can be improved.
[0139] The first functional film 32 preferably further includes an intermediate layer 34 provided between the outermost layer 36 and the substrate 30. By providing the intermediate layer 34, far infrared rays can be appropriately transmitted.
[0140] The intermediate layer 34 preferably includes an anti-reflection layer. The anti-reflection layer is made of NiO X As the main component of the layer, NiO X The content of NiO is preferably 50% by mass or more and 100% by mass or less. X The antireflection layer as a main component can appropriately transmit far infrared rays.
[0141] The far infrared ray transmitting member 20 is preferably mounted on a vehicle. The far infrared ray transmitting member 20 is particularly suitable for vehicle use.
[0142] The far infrared ray transmitting member 20 is preferably disposed on a window member of a vehicle. The far infrared ray transmitting member 20 is particularly suitable for a window member of a vehicle.
[0143] The far-infrared ray transmitting member 20 is preferably disposed on a vehicle pillar exterior member. The far-infrared ray transmitting member 20 is particularly suitable for a vehicle pillar exterior member.
[0144] The far-infrared ray transmitting member 20 is preferably disposed in a light shielding region of a vehicle exterior member. The far-infrared ray transmitting member 20 is particularly suitable for a vehicle exterior member.
[0145] The manufacturing method of this embodiment is a manufacturing method of a far-infrared transmitting member 20 in which a first functional film 32 (functional film) is formed on a substrate 30 that allows far-infrared transmission, and includes a step of manufacturing the far-infrared transmitting member 20 by forming an outermost layer 36 of the first functional film 32 on the substrate 30 by sputtering. The far-infrared transmitting member 20 has an average transmittance of 50% or more for light with a wavelength of 8 μm to 12 μm, and the outermost layer 36 is made of ZrO 2 The layer as the main component has ZrO in the entire outermost layer 36. 2 The content of is 50 mass % or more and 100 mass % or less, and the refractive index of the outermost layer 36 for light of wavelength 550 nm is 2.05 or more. According to this manufacturing method, a far-infrared transmitting member 20 capable of appropriately transmitting far-infrared rays and improving scratch resistance can be manufactured.
[0146] In the step of forming the outermost layer 36 , sputtering is preferably performed at a pressure of 0.30 Pa or less. By performing sputtering at such a low pressure, the outermost layer 36 having excellent scratch resistance can be formed.
[0147] The sputtering is preferably a post-oxidation sputtering method. By performing post-oxidation sputtering, the outermost layer 36 having excellent scratch resistance can be formed.
[0148] (Example)
[0149] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited thereto. Tables 1 and 2 are tables showing the far-infrared transmitting members of the respective Examples.
[0150]
[0151]
[0152] (Example 1)
[0153] As shown in Table 1, in Example 1, NiO as an intermediate layer was sequentially formed on a substrate made of Si (FZ grade) by post-oxidation sputtering using a load-lock sputtering apparatus (RAS-1100BII, manufactured by Syncron). X Film, ZrO 2 Membrane and NiO XThe outermost ZrO film is formed on the surface farthest from the substrate. 2 Film. Substrate, NiO X Film, ZrO 2 The film thickness is shown in Table 1. The substrate thickness was measured using a digital vernier caliper (CD-15CX, manufactured by Mitutoyo Co., Ltd.) and the functional film thickness was evaluated using a probe profilometer (Dektak XT-S, manufactured by BRUKER).
[0154] NiO X Film, ZrO 2 The film forming conditions are as follows: Table 1 shows a part of the film forming conditions (sputtering method and film forming pressure).
[0155] (NiO X film forming conditions)
[0156] Target: NiO (70 mass%) + Ni (30 mass%) mixed target
[0157] Sputtering gas: Ar gas (flow rate: 150 sccm)
[0158] Input power: 6kW
[0159] Reactive gas: Ar (flow rate 70sccm) + O 2 (Flow rate: 10sccm)
[0160] RF power: 2kW
[0161] Substrate temperature: normal temperature
[0162] Film forming pressure: 0.20Pa
[0163] (ZrO 2 film forming conditions)
[0164] Target: Zr target
[0165] Sputtering gas: Ar gas (flow rate: 150 sccm)
[0166] Input power: 6kW
[0167] Reactive gas: O 2 (Flow rate: 100sccm)
[0168] RF power: 4kW
[0169] Substrate temperature: room temperature
[0170] Film forming pressure: 0.21Pa
[0171] (Example 2)
[0172] As shown in Table 1, in Example 2, NiO as an intermediate layer was sequentially formed on a substrate made of Si (FZ grade) by reactive sputtering using a rotating disk sputtering device. X film and the outermost ZrO 2 In addition to setting the substrate, NiO X Film, ZrO 2 A far-infrared transmitting member was obtained by the same method as in Example 1 except for the film thickness.
[0173] NiO X Film, ZrO 2 The film formation conditions are as follows: The film formation pressure is adjusted by the APC valve opening of the turbomolecular pump.
[0174] (NiO X film forming conditions)
[0175] Target: NiO (70 mass%) + Ni (30 mass%) mixed target
[0176] Sputtering gas: Ar gas (flow rate: 120 sccm)
[0177] Reactive gas: O 2 (Flow rate: 30sccm)
[0178] Input power: 3000W
[0179] Substrate temperature: room temperature
[0180] Film forming pressure: 0.30Pa
[0181] (ZrO 2 film forming conditions)
[0182] Target: Zr target
[0183] Sputtering gas: Ar gas (flow rate: 100 sccm)
[0184] Reactive gas: O 2 (Flow rate: 50sccm)
[0185] Input power: 3kW
[0186] Substrate temperature: room temperature
[0187] Film forming pressure: 0.24Pa
[0188] (Example 3~Example 12)
[0189] In Examples 3 to 12, far-infrared transmitting members were obtained by the same method as in Example 2 except that the material and thickness of the film in Example 2 were changed as shown in Tables 1 and 2.2 Film, Al 2 O 3 The film formation conditions of the Si film and the Si film are as follows.
[0190] (ZnO film formation conditions)
[0191] Target: Zn target
[0192] Sputtering gas: Ar gas (flow rate: 100 sccm)
[0193] Reactive gas: O 2 (Flow rate: 100sccm)
[0194] Input power: 3000W
[0195] Substrate temperature: room temperature
[0196] Film forming pressure: 0.24Pa
[0197] (SiO 2 film forming conditions)
[0198] Target: Si target
[0199] Sputtering gas: Ar gas (flow rate: 100 sccm)
[0200] Reactive gas: O 2 (Flow rate: 100sccm)
[0201] Input power: 3000W
[0202] Substrate temperature: room temperature
[0203] Film forming pressure: 0.28Pa
[0204] (Al 2 O 3 film forming conditions)
[0205] Target: Al target
[0206] Sputtering gas: Ar gas (flow rate: 100 sccm)
[0207] Reactive gas: O 2 (Flow rate: 100sccm)
[0208] Input power: 3000W
[0209] Substrate temperature: room temperature
[0210] Film forming pressure: 0.24Pa
[0211] (Si film formation conditions)
[0212] Target: Si target
[0213] Sputtering gas: Ar gas (flow rate: 200 sccm)
[0214] Reactive gas: None
[0215] Input power: 3000W
[0216] Substrate temperature: room temperature
[0217] Film forming pressure: 0.27Pa
[0218] (Example 13)
[0219] In Example 13, in addition to changing the NiO in Example 2 as shown in Table 2, X Film thickness, ZrO 2 A far-infrared transmitting member was obtained by the same method as in Example 2 except for the film forming conditions. ZrO 2 The film forming conditions are as follows.
[0220] (ZrO 2 film forming conditions)
[0221] Target: Zr target
[0222] Sputtering gas: Ar gas (flow rate: 100 sccm)
[0223] Reactive gas: O 2 (Flow rate: 50sccm)
[0224] Input power: 3000W
[0225] Substrate temperature: room temperature
[0226] Film forming pressure: 0.84Pa
[0227] (Example 14)
[0228] In Example 14, except that the configuration of the intermediate layer in Example 1 was changed as shown in Table 2, the same method as in Example 1 was carried out to obtain a far-infrared transmissive member.
[0229] (Outermost layer refractive index)
[0230] The physical property values of the far-infrared transmissive member of each example were measured.
[0231] As a physical property value, the refractive index of the film on the side (outermost) farthest from the substrate of the far-infrared ray transmitting member for light of wavelength 550nm was evaluated. The refractive index was determined by fitting an optical model using polarization information obtained using a spectroscopic ellipsometer (manufactured by JA Woollam, M-2000) and spectral transmittance measured based on JIS R3106.
[0232] It should be noted that the film on the side farthest from the substrate (outermost) is referred to as the outermost layer, for example, in Example 1, it is referred to as the film 4, and in Example 2, it is referred to as the film 2.
[0233] (Arithmetic mean roughness Ra)
[0234] As a physical property value, the arithmetic mean roughness Ra of the surface on the side farthest from the substrate (outermost) of the far-infrared ray transmitting member was measured based on JIS B 0601. It should be noted that the surface on the side farthest from the substrate (outermost) refers to the surface of the film 4 in Example 1 and the surface of the film 2 in Example 2.
[0235] (Indentation hardness)
[0236] As physical property values, the indentation hardness of the first functional film in the film thickness direction (depth direction) was measured by the nanoindentation method using an iMicro nanoindenter (manufactured by KLA Corporation). The measurement conditions are as follows.
[0237] ・Indenter: Bosch Indenter
[0238] ・Actuator: IF50
[0239] ・Measurement method: Continuous stiffness measurement method
[0240] ・Maximum indentation load: 50mN
[0241] ・Strain rate: 0.2% / sec
[0242] ・Poisson's ratio of sample: 0.25
[0243] ・Number of measurement points: 15 to 20 points per substrate
[0244] The average value of the indentation hardness at an indentation depth of 108 nm is used as a representative value. In order to minimize the influence of the substrate, it is recommended to evaluate at an indentation depth of 1 / 10 or less of the evaluation film thickness.
[0245] (Average transmittance of light with a wavelength of 8μm to 12μm)
[0246] As a physical property value, the average transmittance (FIR-T) of light with a wavelength of 8 μm to 12 μm was measured. As a measurement method, a Fourier transform infrared spectrometer (manufactured by ThermoScientific, trade name: Nicolet iS10) was used to measure the transmittance of light of each wavelength of 8 μm to 12 μm, and the average transmittance was calculated from the measured transmittance.
[0247] (Δa * b * )
[0248] As the physical property value, Δa was measured. * b * The reflectance spectrum in the visible light region was measured using U4100 (manufactured by Hitachi Ltd.) based on JIS R3106, and the chromaticity coordinates L of the reflected light in the CIE-Lab colorimetric system when the standard light source D65 was used for the illumination light were calculated based on JIS Z 8781-4. * a * b * , Δa is calculated based on the above formula (3) * b * .
[0249] Tables 1 and 2 show the measurement results of the physical property values of each example.
[0250] (evaluate)
[0251] The far-infrared transmission components of each example were evaluated. As an evaluation, a wiper test was performed, and the number of scratches formed in the wiper test was measured. Specifically, the wiper test was performed on the surface on the side farthest from the substrate (the outermost side) under the following conditions, and then the sliding part of the wiper was observed in a dark field at a magnification of 350 times using an optical microscope DSX500 (manufactured by OLYMPUS). In the dark field observation, the number of scratches in the 1.8 mm area perpendicular to the sliding direction was measured.
[0252] In the wiper test, the surface on the side farthest from the substrate (outermost side) is worn by using a traverse wear tester under the test conditions shown below. A wiper rubber (genuine Toyota product, model 85214-47170) is mounted on the traverse wear tester, and a dust solution is dripped between the wiper and the sample, and reciprocating friction is performed while applying a contact load to the wiper. The wiper width is set to 20 mm, the stroke width is set to 40 mm, the number of strokes is set to 2500 reciprocations, and the load is set to the equivalent of 50 g. The dust solution is prepared by mixing 8 types of JIS test powders 1 and pure water in a mass ratio of 3:100, and 2 ml of the dust solution is dripped onto the sliding part. The substrate is cleaned every 500 reciprocations, and the dust solution is dripped again, thereby performing a total of 2500 reciprocating reciprocating frictions.
[0253] The number of scratches in the wiper test was evaluated as 5 or less, and the number of scratches was evaluated as unqualified. As shown in Table 1, the outermost layer is made of ZrO 2The film as the main component has an outermost layer with a refractive index of 2.05 or more for light of a wavelength of 550nm. In Examples 1 to 4, 11, 12, and 14 corresponding to the embodiments, the wiper test was qualified, and it can be seen that the far-infrared rays can be appropriately transmitted and the scratch resistance can be improved. On the other hand, in Examples 5 to 10 and 13 corresponding to the comparative examples, the wiper test was unqualified due to the low mechanical strength. It is speculated that the far-infrared rays cannot be appropriately transmitted and the scratch resistance cannot be improved. In Examples 5, 7, and 9 corresponding to the comparative examples, although the indentation hardness is as high as 8.0GPa or more, it can be seen that the wiper scratch resistance is low. It is speculated that this is because the film type is a film type with low resistance to adhesive wear and chemical wear in a mixed system of water and dust. Based on the above results, it can be said that ZrO with high chemical stability and high indentation hardness. 2 The film is suitable as the outermost layer. Example 13 corresponding to the comparative example has ZrO 2 The film forming pressure is high and ZrO 2 The film had a sparse film quality with a refractive index of less than 2.05 for light of a wavelength of 550 nm, and therefore failed the wiper test. It is presumed that the film could not improve the scratch resistance while appropriately transmitting far infrared rays.
[0254] (optional evaluation)
[0255] As optional evaluations, evaluation of color change and boiling tests were performed.
[0256] In the evaluation of color change, the surface on the side farthest from the substrate after the wiper test is visually observed to confirm whether the color of the entire worn area changes. In the case of color change, it can be considered that slight film wear and surface roughness change have occurred, so it is more preferable that no color change occurs. As shown in Table 2, by comparing Example 11 with Examples 2, 12, and 14, it can be seen that when the arithmetic mean roughness Ra of the surface is small, no color change occurs, and the scratch resistance can be more appropriately improved.
[0257] In addition, the boiling test was conducted according to JIS R3212 by keeping the samples of each example in pure water at 100°C ± 2°C for 2 hours. After the boiling test, samples in which film peeling occurred or the average transmittance of 8μm to 12μm changed by 5% or more were evaluated as unqualified. As shown in Examples 1, 2, 11 to 14 corresponding to the embodiment, by making the outermost layer of ZrO 2 The film as the main component passed the boiling test and the water resistance was improved, which can be said to be more satisfactory.
[0258] Above, the embodiments of the present invention have been described, but the embodiments are not limited to the contents of the embodiments. In addition, the above-mentioned constituent elements include elements that can be easily thought of by those skilled in the art, substantially the same elements, and elements of so-called equivalent scopes. In addition, the above-mentioned constituent elements can be appropriately combined. In addition, various omissions, substitutions or changes of constituent elements can be performed within the scope of the gist of the above-mentioned embodiments.
[0259] Description of symbols
[0260] 1. Glass for vehicles
[0261] 10, 12, 14 glass substrate
[0262] 20 Far infrared transmission components
[0263] 30 base material
[0264] 32First functional film (functional film)
[0265] 34 Middle layer
[0266] 36 Outermost layer
[0267] 38 Second functional film
Claims
1. A far infrared ray transmitting member, wherein: The far infrared ray transmitting member includes a substrate that allows far infrared ray transmission and a functional film formed on the substrate. The far-infrared ray transmitting member has an average transmittance of light with a wavelength of 8 μm to 12 μm of 50% or more, The outermost layer of the functional film is a layer with ZrO2 as the main component, and the content of ZrO2 relative to the entire outermost layer is greater than 50 mass% and less than 100 mass%. The refractive index of the outermost layer of the functional film for light with a wavelength of 550nm is greater than 2.
05.
2. The far-infrared ray transmitting member according to claim 1, wherein The extinction coefficient of the outermost layer for light with a wavelength of 10 μm is 0.10 or less.
3. The far-infrared ray transmitting member according to claim 1 or claim 2, wherein: The thickness of the outermost layer is greater than 20 nm.
4. The far-infrared transmitting member according to any one of claims 1 to 3, wherein The arithmetic mean roughness Ra of the surface of the outermost layer is 7.0 nm or less.
5. The far-infrared transmitting member according to any one of claims 1 to 4, wherein Δa is defined by the following formula (3): * b * The value of is less than 5, Δa * b * =(a *2 +b *2 ) 0.5 ・・・(3) a* and b* are chromaticity coordinates of reflected light in the CIE-Lab colorimetric system when standard light source D65 is used as illumination light, and are calculated based on JIS Z 8781-4 using spectral reflectance measured based on JIS R3106.
6. The far-infrared transmitting member according to any one of claims 1 to 5, wherein A ratio of the thickness of the outermost layer of the far-infrared transmissive member to the thickness of the substrate is 0.002% or more and 0.030% or less.
7. The far-infrared transmitting member according to any one of claims 1 to 6, wherein The functional film further includes an intermediate layer disposed between the outermost layer and the substrate.
8. The far-infrared ray transmitting member according to claim 7, wherein The intermediate layer comprises NiO X The anti-reflection layer as the main component has NiO as the main component relative to the entire anti-reflection layer. X The content rate is 50 mass % or more and 100 mass % or less.
9. The far-infrared transmitting member according to any one of claims 1 to 8, wherein The far-infrared ray transmitting member is mounted on a vehicle.
10. The far-infrared ray transmitting member according to claim 9, wherein The far-infrared ray transmitting member is disposed on a window member of a vehicle.
11. The far-infrared ray transmitting member according to claim 9 or claim 10, wherein: The far-infrared ray transmitting member is disposed on a pillar outer member of a vehicle.
12. The far-infrared transmitting member according to any one of claims 9 to 11, wherein The far-infrared ray transmitting member is disposed in a light shielding region of the vehicle exterior member.
13. A method for manufacturing a far-infrared transmitting member, the method comprising forming a functional film on a substrate that allows far-infrared transmission, wherein: The method for manufacturing the far-infrared ray transmitting member comprises the steps of: forming the outermost layer of the functional film on the substrate by sputtering; The far-infrared ray transmitting member has an average transmittance of light with a wavelength of 8 μm to 12 μm of 50% or more, The outermost layer is a layer containing ZrO 2 as a main component, the content of ZrO 2 relative to the entire outermost layer is greater than or equal to 50 mass % and less than or equal to 100 mass %, and the refractive index of the outermost layer for light of a wavelength of 550 nm is greater than or equal to 2.
05.
14. The method for manufacturing a far-infrared transmissive member according to claim 13, wherein: In the step of forming the outermost layer, the sputtering is performed at a pressure of 0.30 Pa or less.