Polyolefin resin foam and molded article
By adding metal oxide and hydroxide fillers to the polyolefin resin foam, the coefficient of variation of the bubble shape is controlled, which solves the problem of difficulty in reducing odor in the polyolefin resin foam and achieves a more uniform resin distribution. and significant reduction in odor.
Patent Information
- Application Number
- CN202380023891.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-09-08
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-11
AI Technical Summary
It is difficult to fully reduce the odor in polyolefin-based resin foams with the existing technology. Although there are existing methods using alkaline magnesium, deodorizing and deodorizing agents, activated carbon, carbon black, zeolite, and burned alum, the effects are not satisfactory enough.
By adding metal oxide and metal hydroxide fillers to the polyolefin resin foam, the coefficient of variation of bubble diameter, flattening ratio and area is controlled within a certain range to improve the uniformity of bubble shape and reduce odor generation.
It effectively reduces the generation of odor in polyolefin resin foams and molded bodies, improves the uniformity of resin distribution and the decomposition of foaming agent residues, and significantly reduces the intensity of odor.
Smart Images

Figure BDA0005012382990000191 
Figure BDA0005012382990000251
Abstract
Description
Technical Field
[0001] The present invention relates to a polyolefin resin foam and a molded product. Background Art
[0002] The polyolefin resin foam has excellent moldability due to the characteristics of the resin used, and the molded foam is used for cushioning materials for vehicle interior parts and the like.
[0003] On the other hand, sometimes, odors caused by the materials used and byproducts generated during the production process remain in the polyolefin resin foam, which becomes a problem as interior odor after being installed in the vehicle. For example, it is known that many users feel uncomfortable with the interior odor of the car in a dissatisfaction survey when purchasing a new car.
[0004] As a method for reducing the odor of polyolefin resin foam, for example, a method using basic magnesium is known (Patent Document 1). In addition, a method using a deodorant (Patent Document 2), a method using activated carbon or the like (Patent Document 3), a method using carbon black or the like (Patent Document 4), a method using zeolite (Patent Document 5), a method using burnt alum and zeolite (Patent Document 6), etc. are also known.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2021-169549
[0008] Patent Document 2: Japanese Patent Application Publication No. 2021-172676
[0009] Patent Document 3: Japanese Patent Application Laid-Open No. 11-60774
[0010] Patent Document 4: Japanese Patent Application Laid-Open No. 11-263863
[0011] Patent Document 5: Japanese Patent No. 6832112
[0012] Patent Document 6: Japanese Patent Application Publication No. 2002-12690 Summary of the invention
[0013] Problems to be solved by the invention
[0014] However, even when the above-mentioned conventional technology is applied to an automobile interior provided with an automobile interior part composed of a molded article of a polyolefin-based resin foam, it is sometimes difficult to reduce odor to a degree that fully satisfies the requirements of users.
[0015] Therefore, an object of the present invention is to provide a polyolefin resin foam capable of reducing the generation of odor compared with the related art, and a molded product obtained by molding the polyolefin resin foam.
[0016] Means for solving problems
[0017] The present inventors conducted intensive research and found that the above-mentioned problems can be solved by making the coefficient of variation of the bubble diameter in the width direction (TD), the bubble diameter in the thickness direction (ZD), the bubble flatness, and the bubble area below a certain level, and by containing a certain amount or more of at least one filler selected from metal oxides and metal hydroxides, thereby completing the present invention.
[0018] That is, the present invention is as follows [1] to [9].
[0019] [1] A polyolefin resin foam, wherein the coefficient of variation of the bubble diameter in the width direction (TD) and the coefficient of variation of the bubble diameter in the thickness direction (ZD) for every 50 bubbles contained in the foam are respectively less than 0.38, the coefficient of variation of the bubble flatness is less than 0.45, and the coefficient of variation of the bubble area is less than 0.65, the polyolefin resin foam comprising a polyolefin resin and at least one filler selected from metal oxides and metal hydroxides, and the content of the filler is not less than 0.3% by mass relative to the total amount of the polyolefin resin foam.
[0020] [2] The polyolefin resin foam according to [1] above, wherein the coefficient of variation of the cell diameter in the width direction (TD) is 0.35 or less.
[0021] [3] The polyolefin resin foam according to [1] or [2], wherein the coefficient of variation of the cell diameter in the thickness direction (ZD) is 0.33 or less.
[0022] [4] The polyolefin resin foam according to any one of [1] to [3] above, wherein the coefficient of variation of the cell flatness is 0.40 or less.
[0023] [5] The polyolefin resin foam according to any one of [1] to [4] above, wherein the coefficient of variation of the cell area is 0.60 or less.
[0024] [6] The polyolefin-based resin foam according to any one of [1] to [5] above, wherein the content of the filler is 0.5% by mass or more based on the total amount of the polyolefin-based resin foam.
[0025] [7] The polyolefin resin foam according to any one of [1] to [6] above, wherein the filler is a metal oxide.
[0026] [8] The polyolefin resin foam according to any one of [1] to [7] above, wherein the polyolefin resin contains a polypropylene resin.
[0027] [9] A polyolefin resin foam, wherein the coefficient of variation of the cell diameter in the width direction (TD) and the coefficient of variation of the cell diameter in the thickness direction (ZD) per 50 cells contained in the foam are respectively 0.38 or less, the coefficient of variation of the cell flattening ratio is 0.45 or less, and the coefficient of variation of the cell area is 0.65 or less,
[0028] The polyolefin resin foam contains a polyolefin resin and at least one filler selected from metal oxides and metal hydroxides, and the content of the filler is 0.4 parts by mass or more based on 100 parts by mass of the polyolefin resin.
[0029]
[10] The polyolefin resin foam according to [9] above, wherein the coefficient of variation of the cell diameter in the width direction (TD) is 0.35 or less.
[0030]
[11] The polyolefin resin foam according to [9] or
[10] above, wherein the coefficient of variation of the cell diameter in the thickness direction (ZD) is 0.33 or less.
[0031]
[12] The polyolefin resin foam according to any one of [9] to
[11] above, wherein the coefficient of variation of the cell flatness is 0.40 or less.
[0032]
[13] The polyolefin resin foam according to any one of [9] to
[12] above, wherein the coefficient of variation of the cell area is 0.60 or less.
[0033]
[14] The polyolefin resin foam according to any one of [9] to
[13] above, wherein the content of the filler is 0.6 parts by mass or more relative to 100 parts by mass of the polyolefin resin.
[0034]
[15] The polyolefin resin foam according to any one of [9] to
[14] above, wherein the filler is a metal oxide.
[0035]
[16] The polyolefin resin foam according to any one of [9] to
[15] above, wherein the polyolefin resin contains a polypropylene resin.
[0036]
[17] A molded product obtained by molding the polyolefin resin foam according to any one of [1] to
[16] above.
[0037]
[18] The molded article according to
[17] above, wherein a skin material is laminated on at least one surface of the polyolefin-based resin foam.
[0038] Effects of the Invention
[0039] According to the present invention, a polyolefin resin foam capable of reducing the generation of odor and a molded product obtained by molding the polyolefin resin foam can be provided. DETAILED DESCRIPTION
[0040] The polyolefin resin foam of the present invention has a coefficient of variation of the bubble diameter in the width direction (TD) and the coefficient of variation of the bubble diameter in the thickness direction (ZD) of each 50 bubbles, a coefficient of variation of the bubble flatness of 0.45 or less, and a coefficient of variation of the bubble area of 0.65 or less. In addition, the polyolefin resin foam contains a polyolefin resin and at least one filler selected from metal oxides and metal hydroxides, and the content of the filler is 0.3% by mass or more relative to the total amount of the polyolefin resin foam.
[0041] The polyolefin resin foam may contain a polyolefin resin and at least one filler selected from metal oxides and metal hydroxides, wherein the content of the filler is 0.4 parts by mass or more based on 100 parts by mass of the polyolefin resin.
[0042] The polyolefin resin foam of the present invention (hereinafter, sometimes simply referred to as the foam) has a sheet-like shape. In the present invention, "TD" refers to the transverse direction, which is a direction perpendicular to the extrusion direction of the foam (MD: Machine Direction), and refers to the width direction of the foam. Furthermore, "ZD" refers to the thickness direction, which is a direction perpendicular to both MD and TD, and is the thickness direction of the foam.
[0043] The polyolefin resin foam of the present invention can reduce the generation of odor. The reason is not clear, but it is presumed as follows.
[0044] As described above, the coefficient of variation of the bubble diameter of TD and ZD, the coefficient of variation of the bubble flatness, and the coefficient of variation of the bubble area of the polyolefin resin foam of the present invention are below a certain value. This means that the uniformity of the shapes of the multiple bubbles (cells) present in the foam is high. It is believed that if the uniformity of the shapes of the multiple bubbles is high, the distribution of the resin constituting the foam is also improved in uniformity, and the odor is reduced. For example, in the case where there are places with more resin and places with less resin in the foam (that is, in the case where the distribution of the resin is uneven), since it is easy to generate odor from the place with more resin, it is inferred that the odor is difficult to be reduced.
[0045] Furthermore, the polyolefin resin foam of the present invention contains a certain amount or more of at least one filler selected from metal oxides and metal hydroxides. As a result, the decomposition of the blowing agent (for example, a thermal decomposition type blowing agent such as azodicarbonamide) used in the production of the polyolefin resin foam is promoted, and the residue of the blowing agent that causes the odor is reduced.
[0046] As described above, it is considered that the polyolefin-based resin foam of the present invention effectively reduces odor due to two factors: the uniformity of the shapes of the plurality of cells is high, and the polyolefin-based resin foam contains a certain amount or more of a specific filler.
[0047] <Coefficient of variation (TD)>
[0048] The coefficient of variation of the bubble diameter in the width direction (TD) of every 50 bubbles contained in the polyolefin resin foam of the present invention is 0.38 or less. If the coefficient of variation of the bubble diameter in TD exceeds 0.38, it is difficult to reduce the odor. From the viewpoint of further reducing the odor, the coefficient of variation of the bubble diameter in TD in the foam is preferably 0.35 or less, more preferably 0.30 or less, and further preferably 0.25 or less. From the viewpoint of practicality in manufacturing, the coefficient of variation of the bubble diameter in TD is preferably 0.1 or more.
[0049] It should be noted that the coefficient of variation of the bubble diameter of TD is measured as follows. The polyolefin resin foam is cut in the thickness direction along the TD direction, and the obtained cross section is photographed with a 200-fold magnification photo using a digital microscope, and the bubble diameter of TD is measured for 50 bubbles. Based on the result, the standard deviation of the bubble diameter of TD and the average bubble diameter of TD are obtained. Furthermore, as shown in the following formula, the value obtained by dividing the standard deviation of the bubble diameter of TD by the average bubble diameter of TD becomes the coefficient of variation of the bubble diameter of TD.
[0050] Coefficient of variation of bubble diameter of TD = standard deviation of bubble diameter of TD / average bubble diameter of TD
[0051] <Coefficient of variation (ZD)>
[0052] The coefficient of variation of the bubble diameter in the thickness direction (ZD) of every 50 bubbles contained in the polyolefin resin foam of the present invention is 0.38 or less. If the coefficient of variation of the bubble diameter of ZD exceeds 0.38, it is difficult to reduce the odor. From the viewpoint of further reducing the odor, the coefficient of variation of the bubble diameter of ZD in the foam is preferably 0.33 or less, more preferably 0.28 or less, and further preferably 0.23 or less. From the practical viewpoint of manufacturing, the coefficient of variation of the bubble diameter of ZD is preferably 0.1 or more.
[0053] It should be noted that the coefficient of variation of the bubble diameter of ZD is measured as follows. The polyolefin resin foam is cut in the thickness direction along the TD direction, and the obtained cross section is photographed with a 200-fold magnification using a digital microscope. The bubble diameter of ZD is measured for 50 bubbles, and based on the result, the standard deviation of the bubble diameter of ZD and the average bubble diameter of ZD are obtained. Furthermore, as shown in the following formula, the value obtained by dividing the standard deviation of the bubble diameter of ZD by the average bubble diameter of ZD becomes the coefficient of variation of the bubble diameter of ZD.
[0054] Coefficient of variation of ZD cell diameter = standard deviation of ZD cell diameter / average cell diameter of ZD
[0055] <Coefficient of variation (cell flattening rate)>
[0056] The coefficient of variation of the flattening rate of bubbles per 50 bubbles contained in the polyolefin resin foam of the present invention is 0.45 or less. If the coefficient of variation of the flattening rate of bubbles exceeds 0.45, it is difficult to reduce the odor. From the viewpoint of further reducing the odor, the coefficient of variation of the flattening rate of bubbles in the foam is preferably 0.40 or less, more preferably 0.35 or less, and further preferably 0.30 or less. From the viewpoint of practicality in manufacturing, the coefficient of variation of the flattening rate of bubbles is preferably 0.2 or more.
[0057] It should be noted that the coefficient of variation of the cell flatness is determined as follows: a polyolefin resin foam is cut in the thickness direction along the TD direction, a 200-fold magnified photograph of the obtained cross section is taken using a digital microscope, and the cell diameters of TD and ZD are measured for 50 cells, respectively, and the 50 cell flatnesses are calculated based on the following formula.
[0058] Cell flatness = 1-[(cell diameter at ZD / 2) / (cell diameter at TD / 2)]
[0059] Furthermore, based on the 50 cell flatnesses thus obtained, the average cell flatness and the standard deviation of the cell flatness were obtained. Furthermore, as shown in the following formula, the value obtained by dividing the standard deviation of the cell flatness by the average cell flatness is the coefficient of variation of the cell flatness.
[0060] Coefficient of variation of bubble flatness = standard deviation of bubble flatness / average bubble flatness
[0061] <Coefficient of variation (bubble area)>
[0062] The coefficient of variation of the bubble area of every 50 bubbles contained in the polyolefin resin foam of the present invention is 0.65 or less. If the coefficient of variation of the bubble area exceeds 0.65, it is difficult to reduce the odor. From the viewpoint of further reducing the odor, the coefficient of variation of the bubble area in the foam is preferably 0.60 or less, more preferably 0.55 or less, and further preferably 0.50 or less. From the viewpoint of practicality in manufacturing, the coefficient of variation of the bubble area is preferably 0.25 or more.
[0063] It should be noted that the coefficient of variation of the bubble area is measured as follows: a polyolefin resin foam is cut in the thickness direction along the TD direction, a 200-fold magnified photograph of the obtained cross section is taken with a digital microscope, and the bubble diameters of TD and ZD are measured for 50 bubbles, respectively, and the 50 bubble areas are calculated based on the following formula.
[0064] Bubble area = (circumference) × (bubble diameter of TD / 2) × (bubble diameter of ZD / 2)
[0065] Furthermore, based on the 50 bubble areas thus obtained, the average bubble area and the standard deviation of the bubble area are obtained. Furthermore, as shown in the following formula, the value obtained by dividing the standard deviation of the bubble area by the average bubble area is the coefficient of variation of the bubble area.
[0066] Coefficient of variation of bubble area = standard deviation of bubble area / average bubble area
[0067] The method for making each coefficient of variation equal to or less than a certain value as described above is not particularly limited, and an example thereof includes a method of applying the method for producing a foam described later.
[0068] <Packing>
[0069] The polyolefin resin foam of the present invention contains 0.3% by mass or more of at least one filler selected from metal oxides and metal hydroxides based on the total amount of the polyolefin resin foam, thereby reducing odor generated from the foam.
[0070] The filler is at least one selected from metal oxides and metal hydroxides, and is preferably a metal oxide from the viewpoint of easiness in reducing odor.
[0071] Examples of the metal oxide include magnesium oxide, titanium oxide, silicon oxide, zinc oxide, and aluminum oxide. Among them, magnesium oxide is preferred from the viewpoint of reducing odor.
[0072] Examples of the metal hydroxide include magnesium hydroxide, aluminum hydroxide, and iron hydroxide, and magnesium hydroxide is preferred.
[0073] Among these fillers, magnesium oxide is particularly preferred from the viewpoint of reducing odor.
[0074] The filler may be used alone or in combination of two or more.
[0075] The content of the filler in the polyolefin resin foam is 0.3% by mass or more relative to the total amount of the polyolefin resin foam. If the content of the filler is less than 0.3% by mass, the residue of the foaming agent such as azodicarbonamide is likely to remain in the foam, and odor is likely to be generated.
[0076] From the viewpoint of suppressing odor, the filler content is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, and further preferably 0.9% by mass or more, relative to the total amount of the polyolefin resin foam. Furthermore, from the viewpoint of practicality in manufacturing, it is preferably 10% by mass or less, more preferably 5% by mass or less, further preferably 2% by mass or less, and further preferably 1% by mass or less.
[0077] The content of the filler in the polyolefin resin foam may be 0.4 parts by mass or more relative to 100 parts by mass of the polyolefin resin. If the content of the filler is 0.4 parts by mass or more, the residue of the blowing agent such as azodicarbonamide is unlikely to remain in the foam, and odor is unlikely to be generated.
[0078] From the viewpoint of suppressing odor, the content of the filler is preferably 0.6 parts by mass or more, more preferably 1.0 parts by mass or more, based on 100 parts by mass of the polyolefin resin, and is preferably 10 parts by mass or less from the viewpoint of practicality in production.
[0079] <Polyolefin resin>
[0080] The polyolefin resin foam of the present invention contains a polyolefin resin. As the polyolefin resin, for example, polypropylene resin, polyethylene resin, olefin thermoplastic elastomer (TPO), ethylene-α-olefin copolymer rubber, etc. can be cited. Among these polyolefin resins, from the viewpoint of ensuring a certain mechanical strength of the foam and also ensuring good formability at high temperatures, it is preferred to contain at least a polypropylene resin. From the viewpoint of ensuring flexibility, the polyolefin resin preferably includes at least one selected from polyethylene resin, olefin thermoplastic elastomer, and ethylene-α-olefin copolymer rubber in addition to the polypropylene resin.
[0081] (Polypropylene resin)
[0082] The polypropylene resin is not particularly limited, and examples thereof include propylene homopolymers (homopolypropylene) and copolymers of propylene and other olefins. The copolymers of propylene and other olefins may be any of block copolymers, random copolymers, and random block copolymers, but are preferably random copolymers (random polypropylene).
[0083] As other olefins copolymerized with propylene, for example, α-olefins such as ethylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, and 1-decene can be mentioned, among which ethylene is preferred. Therefore, as random polypropylene, ethylene-propylene random copolymer is more preferred.
[0084] Among the polypropylene resins, propylene homopolymers (homopolypropylene) or random polypropylene are preferred, and random polypropylene is more preferred from the viewpoint of moldability, etc. The polypropylene resins may be used alone or in combination of two or more.
[0085] The polypropylene resin preferably has a melt flow rate (hereinafter also referred to as "MFR") at 230°C of 0.1 to 20 g / 10 minutes. If the MFR of the polypropylene resin is within the above range, the fluidity of the resin becomes good, and on the other hand, the fluidity of the resin is prevented from becoming too high, and the processability when the foamable composition described later is processed into a foam becomes good. From these viewpoints, the MFR of the polypropylene resin is more preferably 0.3 to 15 g / 10 minutes.
[0086] The content of polypropylene resin is preferably 15 to 90% by mass relative to the total amount of resin constituting the foam. By making the content of polypropylene resin more than 10% by mass, it is easy to ensure mechanical strength and moldability at high temperature. In addition, by being less than 90% by mass, a certain amount of other resins such as olefin-based thermoplastic elastomers can be mixed to ensure flexibility. From the above viewpoint, the content of polypropylene resin is more preferably 30 to 85% by mass, and further preferably 50 to 80% by mass.
[0087] (Polyethylene resin)
[0088] The polyolefin resin in the present invention preferably contains a polyethylene resin in addition to the polypropylene resin, because the flexibility of the foam can be further improved.
[0089] As polyethylene resin, there is no particular limitation, and examples thereof include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, etc., wherein linear low-density polyethylene is preferred. As linear low-density polyethylene, ethylene / 1-butene copolymer, ethylene / 1-hexene copolymer, ethylene / 4-methyl-1-pentene copolymer, ethylene / 1-octene copolymer, etc. can be mentioned.
[0090] The linear low-density polyethylene has a density of 0.880 to 0.940 g / cm 3 The polyethylene preferably has a density of 0.900 to 0.930 g / cm 3 It should be noted that the density is measured in accordance with JIS K7112.
[0091] Furthermore, from the viewpoint of processability and flexibility, the melt flow rate (MFR) of the polyethylene resin at 190°C is preferably 0.5 to 20 g / 10 min, more preferably 1 to 15 g / 10 min, and further preferably 1.5 to 12 g / 10 min.
[0092] The content of polyethylene resin is preferably 10 to 50% by mass relative to the total amount of resin components constituting the foam. By making the content of polyethylene resin 10% by mass or more, it is easy to ensure flexibility. In addition, by being below 50% by mass, it is easy to ensure the mechanical strength of the foam sheet, etc. by mixing other resins such as a considerable amount of polypropylene resin. From these viewpoints, the content of polyethylene resin is more preferably 15 to 45% by mass.
[0093] (Olefin thermoplastic elastomer (TPO))
[0094] The polyolefin resin in the present invention preferably contains an olefin thermoplastic elastomer (TPO) in addition to the polypropylene resin. This can further improve the flexibility of the foam.
[0095] As TPO, there can be mentioned a blended elastomer or a dynamically cross-linked elastomer. The blended elastomer is made by blending a polyolefin resin with a rubber component. The rubber component can be partially cross-linked before blending with the polyolefin resin. In addition, the dynamically cross-linked elastomer is made by cross-linking the rubber component when mixing the polyolefin resin with the rubber component. Among the rubber components blended with the polyolefin resin, for example, ethylene-propylene copolymer (EPR), ethylene-propylene-diene copolymer (EPDM), nitrile rubber (NBR), natural rubber (NR), isobutylene-isoprene rubber (IIR), etc. can be mentioned.
[0096] The content of TPO is preferably 10 to 60% by mass relative to the total amount of resin constituting the foam. By making the content of TPO 10% by mass or more, the flexibility of the foam can be further improved. In addition, by being 60% by mass or less, the mechanical strength of the foam can be improved. From the above viewpoints, the content of TPO is more preferably 15 to 45% by mass.
[0097] (Ethylene-α-olefin copolymer rubber)
[0098] The polyolefin resin in the present invention preferably contains an ethylene-α-olefin copolymer rubber in addition to the polypropylene resin, thereby further improving the flexibility of the foam.
[0099] The ethylene-α-olefin copolymer rubber is preferably an amorphous or low-crystalline rubbery material obtained by substantially randomly copolymerizing two or more olefin monomers.
[0100] Examples of the α-olefin used in the ethylene-α-olefin copolymer rubber include one or more α-olefins having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, such as propylene, 1-butene, 2-methylpropylene, 3-methyl-1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene and 1-octene.
[0101] The ethylene-α-olefin copolymer rubber may have other monomer units in addition to the ethylene unit and the α-olefin unit.
[0102] Examples of the monomer forming the other monomer unit include conjugated dienes having 4 to 8 carbon atoms, non-conjugated dienes having 5 to 15 carbon atoms, vinyl ester compounds, unsaturated carboxylic acid esters, and unsaturated carboxylic acids.
[0103] Examples of the conjugated diene having 4 to 8 carbon atoms include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene.
[0104] Examples of the non-conjugated diene having 5 to 15 carbon atoms include dicyclopentadiene, 5-ethylidene-2-norbornene, 1,4-hexadiene, 1,5-dicyclooctadiene, 7-methyl-1,6-octadiene, and 5-vinyl-2-norbornene.
[0105] Examples of the vinyl ester compound include vinyl acetate and the like.
[0106] Examples of the unsaturated carboxylic acid ester include methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, and ethyl methacrylate.
[0107] Examples of the unsaturated carboxylic acid include acrylic acid and methacrylic acid.
[0108] These monomers may be used alone or in combination of two or more. Among the above, non-conjugated dienes having 5 to 15 carbon atoms are preferred, and from the viewpoint of availability, 5-ethylidene-2-norbornene, 1,4-hexadiene, and dicyclopentadiene (DCPD) are more preferred.
[0109] Among the ethylene-α-olefin copolymer rubbers, ethylene-propylene copolymers (EPR) and ethylene-propylene-diene copolymers (EPDM) are preferred, and among them, EPDM is more preferred.
[0110] The content of ethylene-α-olefin copolymer rubber is preferably 3 to 30% by mass relative to the total amount of resin constituting the foam. By making the content of ethylene-α-olefin copolymer rubber more than 3% by mass, the flexibility of the foam can be further improved. In addition, by being less than 30% by mass, the mechanical strength of the foam can be improved. From the above viewpoint, the content of ethylene-α-olefin copolymer rubber is more preferably 5 to 15% by mass.
[0111] As the polyolefin resin, resin components other than those mentioned above may be used, and specific examples thereof include ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-alkyl (meth)acrylate copolymers, and modified copolymers obtained by copolymerizing maleic anhydride.
[0112] In addition, as long as the effect of the present invention is not impaired, the foam may contain resins other than polyolefin resins such as styrene-based thermoplastic elastomers. The content of the resins other than the polyolefin resins is, for example, 25% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less, and further preferably 0% by mass, relative to the total amount of the resin components.
[0113] <Foamable composition>
[0114] The foam of the present invention is obtained by foaming, preferably crosslinking and foaming, a foamable composition containing the above-mentioned polyolefin resin and filler. The foamable composition usually contains a foaming agent as an additive, and preferably contains a crosslinking aid, an antioxidant, and the like.
[0115] (foaming agent)
[0116] As the foaming agent, a thermal decomposition type foaming agent is used, and for example, an organic or inorganic chemical foaming agent having a decomposition temperature of about 160 to 270° C. can be used.
[0117] Examples of the organic foaming agent include azodicarbonamide, azodicarboxylic acid metal salts (barium azodicarboxylate and the like), azo compounds such as azobisisobutyronitrile, nitroso compounds such as N,N'-dinitrosopentamethylenetetramine, biurea, hydrazine derivatives such as 4,4'-oxybis(benzenesulfonylhydrazide) and toluenesulfonylhydrazide, and semicarbazide compounds such as toluenesulfonylsemicarbazide.
[0118] Examples of the inorganic foaming agent include ammonium carbonate, sodium carbonate, ammonium hydrogen carbonate, sodium hydrogen carbonate, ammonium nitrite, sodium borohydride, and anhydrous monosodium citrate.
[0119] Among them, from the viewpoint of obtaining fine bubbles, and from the viewpoint of economic efficiency and safety, azo compounds and nitroso compounds are preferred, azodicarbonamide, azobisisobutyronitrile, and N,N′-dinitrosopentamethylenetetramine are more preferred, and azodicarbonamide is particularly preferred.
[0120] In order to properly foam the foam without breaking the cells of the foam, the content of the thermally decomposable foaming agent in the foamable composition is preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, and even more preferably 5 to 10 parts by mass based on 100 parts by mass of the polyolefin resin.
[0121] (Crosslinking aid)
[0122] As a crosslinking aid, a multifunctional monomer can be used. For example, trimethylolpropane trimethacrylate, trimethylolpropane triacrylate and other trifunctional (meth)acrylate compounds, trimellitic acid triallyl ester, 1,2,4-benzenetricarboxylic acid triallyl ester, isocyanuric acid triallyl ester and other compounds having three functional groups in one molecule, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, 1,10-decanediol dimethacrylate, neopentyl glycol dimethacrylate and other bifunctional (meth)acrylate compounds, divinylbenzene, diallyl phthalate, diallyl terephthalate, diallyl isophthalate and other compounds having two functional groups in one molecule, ethylvinylbenzene, lauryl methacrylate, stearyl methacrylate and the like.
[0123] The crosslinking aid may be used alone or in combination of two or more. Among the above, (meth)acrylate compounds are preferred.
[0124] By adding a crosslinking aid to the foamable composition, the foamable composition can be crosslinked with a small ionizing radiation dose, thereby preventing the breakage and degradation of each resin molecule accompanying irradiation with ionizing radiation.
[0125] The content of the crosslinking aid in the foamable composition is preferably 0.2 to 20 parts by mass relative to 100 parts by mass of the polyolefin resin. If the content is 0.2 parts by mass or more, it is easy to adjust the desired crosslinking degree when the foamable composition is foamed. In addition, if it is 20 parts by mass or less, it is easy to control the crosslinking degree given to the foamable composition. The content of the crosslinking aid is more preferably 0.5 to 10 parts by mass, and more preferably 1 to 8 parts by mass relative to 100 parts by mass of the polyolefin resin.
[0126] (Antioxidant)
[0127] As antioxidants, phenolic antioxidants, sulfur-based antioxidants, phosphorus-based antioxidants, amine-based antioxidants, etc. can be mentioned, but among them, phenolic antioxidants and phosphorus-based antioxidants are preferred, and phenolic antioxidants and phosphorus-based antioxidants are more preferably used in combination. Antioxidants can be used alone or in combination of two or more.
[0128] The content of the antioxidant in the foamable composition is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 5 parts by mass, based on 100 parts by mass of the polyolefin-based resin.
[0129] Furthermore, the foam composition may contain additives other than those listed above, such as a foaming aid, a flame retardant, a metal damage preventing agent, an antistatic agent, a stabilizer, and a pigment, as required.
[0130] <Foaming ratio>
[0131] From the viewpoint of improving flexibility, the expansion ratio of the polyolefin resin foam of the present invention is preferably 8 cm 3 / g or more, more preferably 10cm 3 / g or more, more preferably 15cm 3 In addition, from the viewpoint of ensuring a certain mechanical strength, the expansion ratio of the foam is preferably 30 cm 3 / g or less, more preferably 28cm 3 / g or less, more preferably 25cm 3 / g or less.
[0132] In addition, the expansion ratio in the present invention refers to the reciprocal of the density of the foamed sheet measured in accordance with JIS K7222.
[0133] <Apparent density>
[0134] From the viewpoint of ensuring a certain mechanical strength, the apparent density of the polyolefin resin foam of the present invention is preferably 0.03 g / cm 3 More preferably, 0.04 g / cm 3 In addition, from the viewpoint of improving flexibility, the apparent density of the foam is preferably 0.13 g / cm 3 Below, more preferably 0.10 g / cm 3 the following.
[0135] <Degree of cross-linking>
[0136] The polyolefin resin foam of the present invention is preferably a crosslinked body. In the case of a crosslinked body, the crosslinking degree (%) indicating the crosslinking degree of the foam is preferably 30 to 60%. If the crosslinking degree is within the above range, the mechanical strength of the foam is well maintained while the flexibility is excellent. From these viewpoints, the crosslinking degree (%) of the foam sheet is more preferably 35 to 55%.
[0137] The degree of crosslinking was calculated by the following formula by taking out the insoluble component of the solvent and determining the weight A of the test piece and the weight B of the insoluble component by the method described in the Examples.
[0138] Degree of crosslinking (weight %) = (B / A) × 100
[0139] <Thickness>
[0140] The thickness of the polyolefin resin foam of the present invention is preferably 0.5 to 5 mm, more preferably 1 to 4 mm. When the thickness is within these ranges, a molded article molded from the foam can be suitably used for a vehicle interior part.
[0141] <Tensile Strength>
[0142] From the viewpoint of uniformly molding the foam, etc., the tensile strength of the polyolefin resin foam of the present invention in MD at 120°C is preferably 0.15 MPa or more, more preferably 0.25 MPa or more, and further preferably 3 MPa or less, more preferably 1 MPa or less.
[0143] From the viewpoint of uniformly molding the foam, etc., the tensile strength of the polyolefin resin foam of the present invention in TD at 120°C is preferably 0.07 MPa or more, more preferably 0.10 MPa or more, and further preferably 2 MPa or less, more preferably 1 MPa or less.
[0144] <Tensile elongation>
[0145] From the viewpoint of preventing the material from breaking during vacuum forming or the like, the tensile elongation in MD at 120° C. of the polyolefin resin foam of the present invention is preferably 250% or more, more preferably 300% or more, and even more preferably 400% or more. From the viewpoint of practicality in production, the tensile elongation in MD at 120° C. of the polyolefin resin foam is preferably 1000% or less.
[0146] From the viewpoint of preventing the material from breaking during vacuum forming or the like, the tensile elongation in TD at 120° C. of the polyolefin resin foam of the present invention is preferably 160% or more, more preferably 200% or more, and still more preferably 300% or more. From the viewpoint of practicality in production, the tensile elongation in TD at 120° C. of the polyolefin resin foam is preferably 1000% or less.
[0147] The tensile strength and tensile elongation of the foam at 120° C. can be adjusted to the above-specified ranges by adjusting the type of the resin component, etc. In addition, they can also be adjusted by the expansion ratio, the degree of crosslinking, etc.
[0148] <Dimensional change rate after heating>
[0149] From the viewpoint of improving the moldability in vacuum molding or the like, the dimensional change rate of the polyolefin resin foam of the present invention in MD at 120°C is preferably -8 to 8%, more preferably -7 to 7%, and even more preferably -5 to 5%.
[0150] From the viewpoint of improving the moldability in vacuum molding or the like, the dimensional change rate of heating in TD at 120° C. of the polyolefin resin foam of the present invention is preferably −7 to 7%, more preferably −6 to 6%, and even more preferably −4 to 4%.
[0151] [Method for producing polyolefin resin foam]
[0152] The foamable composition containing a polyolefin resin, a filler, and a foaming agent is foamed, and preferably foamed after crosslinking.
[0153] The polyolefin resin foam of the present invention is not particularly limited and can be produced by heating a foamable sheet formed of a foamable composition comprising a polyolefin resin, a filler, and a foaming agent to foam the foaming agent. In addition, the foamable sheet is preferably cross-linked and the cross-linked foamable sheet is heated to foam. The foamable composition may contain a cross-linking aid, an antioxidant, and other additives as required.
[0154] The foamable composition is preferably produced by using at least a polyolefin-based resin, a filler masterbatch, and a foaming agent as raw materials and melt-kneading these components.
[0155] The filler masterbatch is produced by melt-kneading the filler of the present invention and a polyolefin-based resin, and preferably has a pellet shape.
[0156] It is believed that by using this filler masterbatch, the filler can be easily dispersed uniformly in the foamable composition, thereby making it easy to obtain a foamed body in which the coefficient of variation of the cell diameter of MD, the cell diameter of ZD, the cell flatness, and the cell area is below a certain level as described above, and the odor is reduced.
[0157] From the viewpoint of easily obtaining a foam having each coefficient of variation being equal to or less than a certain value, the content of the filler in the filler masterbatch is preferably 10 to 50% by mass, more preferably 20 to 30% by mass.
[0158] In addition, as raw materials for producing the foamable composition, in addition to the above, a cross-linking auxiliary agent, an antioxidant, and other additives may be used as necessary.
[0159] Specifically, it is industrially advantageous to produce the polyolefin-based resin foam of the present invention by a method having the following steps (1) to (3).
[0160] Step (1): A step of supplying the raw materials of the foamable composition to a kneading device and kneading them to obtain a sheet-like foamable composition.
[0161] Step (2): a step of irradiating the foamable composition obtained in step (1) with ionizing radiation to perform crosslinking
[0162] Step (3): A step of heating the foamable composition crosslinked in step (2) to a temperature higher than the decomposition temperature of the foaming agent to foam the composition, thereby obtaining a sheet-like foam.
[0163] In step (1), the foamable composition can be produced in a sheet form by kneading the raw materials of the foamable composition using a kneading machine such as a Banbury mixer or a pressure kneader and then continuously extruding the mixture using an extruder, a calender, a conveyor casting machine or the like.
[0164] As described above, it is preferred to use at least a polyolefin resin, a filler masterbatch, and a foaming agent as the raw materials of the foamable composition.
[0165] In addition, the ionizing radiation used in step (2) includes α-rays, β-rays, γ-rays, electron beams, etc., but electron beams are preferred. The irradiation dose of the ionizing radiation may be any dose as long as the desired degree of crosslinking can be obtained, but is preferably 0.1 to 10 Mrad, more preferably 0.2 to 5 Mrad, and even more preferably 0.5 to 3 Mrad.
[0166] In the step (3), the temperature at which the foamable composition is heated to foam depends on the decomposition temperature of the thermally decomposable foaming agent used as the foaming agent, but is usually 140 to 300°C, preferably 150 to 280°C.
[0167] In step (3), the foam is preferably stretched in either or both of MD and TD after foaming or while foaming. In addition, step (3) may be performed after step (1) without going through step (2). That is, the sheet-like foamable composition may be foamed without crosslinking.
[0168] <Molding body>
[0169] The molded article of the present invention is formed by molding the polyolefin resin foam of the present invention. For example, the molded article of the present invention can be obtained by molding the polyolefin resin foam of the present invention by a known method. When manufacturing the molded article, other raw materials such as a substrate and a skin material can be laminated with the polyolefin resin foam to manufacture. The molded article of the present invention is preferably laminated with a skin material on at least one surface of the polyolefin resin foam.
[0170] Examples of the surface material include polyvinyl chloride sheets, sheets formed of mixed resins of polyvinyl chloride and ABS resin, thermoplastic elastomer sheets, fabrics, knitted fabrics, nonwoven fabrics, leathers such as artificial leather and synthetic leather, and metals, etc. In addition, a molded body having a surface design of pores, wood grain patterns, etc., may be used using a silicone stamp with concavoconvex patterns transferred from genuine leather, stone, wood, etc.
[0171] By laminating the skin material and the polyolefin-based resin foam and molding them, a molded body in which the skin material is laminated on the polyolefin-based resin foam can be obtained.
[0172] As methods for bonding the surface materials, for example, there can be cited extrusion lamination, adhesive lamination after applying an adhesive, thermal lamination (thermal fusion), hot melt, high-frequency welding, non-electrolytic plating for metals, electrolytic plating and vapor deposition, etc. Any method is acceptable as long as the two are bonded.
[0173] As the molding method of the molded body of the present invention, stamping molding, vacuum molding, compression molding, injection molding, etc. can be mentioned. Among them, stamping molding and vacuum molding are preferred. As the vacuum molding method, both the male mold vacuum molding method and the female mold vacuum molding method can be adopted, but the male mold vacuum molding method is more preferred.
[0174] The molded body formed by molding the polyolefin resin foam of the present invention can be used as a heat insulating member, a cushioning member, etc. The molded body formed by molding the polyolefin resin foam of the present invention is not easy to generate odor even in the hot summer period, so it can be suitably used as a car interior decoration member such as a ceiling member, a door, and an instrument panel, especially in the automotive field.
[0175] Example
[0176] Hereinafter, the present invention will be described by way of examples, but the present invention is not limited to these examples at all.
[0177] In addition, the measuring method of each physical property and the evaluation method of the foam sheet are as follows.
[0178] <Coefficient of variation>
[0179] The polyolefin resin foam was cut in the thickness direction along the TD direction, and the obtained cross section was photographed at 200 times magnification using a digital microscope (manufactured by Keyence Corporation, product name VHX-900), and 50 bubbles (cells) were observed. Furthermore, each coefficient of variation was determined as follows.
[0180] (Coefficient of variation of TD)
[0181] The cell diameters of 50 TDs were measured, and based on the results, the standard deviation of the cell diameters of TD and the average cell diameter of TD were calculated. Furthermore, as shown in the following formula, the value obtained by dividing the standard deviation of the cell diameters of TD by the average cell diameter of TD was defined as the coefficient of variation of the cell diameters of TD.
[0182] Coefficient of variation of bubble diameter of TD = standard deviation of bubble diameter of TD / average bubble diameter of TD
[0183] (Coefficient of variation of ZD)
[0184] The cell diameters of 50 ZDs were measured, and based on the results, the standard deviation of the cell diameters of ZDs and the average cell diameter of ZDs were calculated. Furthermore, as shown in the following formula, the value obtained by dividing the standard deviation of the cell diameters of ZDs by the average cell diameter of ZDs was defined as the coefficient of variation of the cell diameters of ZDs.
[0185] Coefficient of variation of ZD cell diameter = standard deviation of ZD cell diameter / average cell diameter of ZD
[0186] (Coefficient of variation of bubble flatness)
[0187] The cell diameters of 50 TD and ZD were measured, and the flattening ratios of 50 cells were calculated based on the following formula.
[0188] Cell flatness = 1-[(cell diameter at ZD / 2) / (cell diameter at TD / 2)]
[0189] Based on the 50 cell flatnesses thus obtained, the average cell flatness and the standard deviation of the cell flatness were obtained. Furthermore, as shown in the following formula, the value obtained by dividing the standard deviation of the cell flatness by the average cell flatness was defined as the coefficient of variation of the cell flatness.
[0190] Coefficient of variation of bubble flatness = standard deviation of bubble flatness / average bubble flatness
[0191] (Coefficient of variation of bubble area)
[0192] The cell diameters of 50 TD and ZD were measured, and the areas of 50 cells were calculated based on the following formula.
[0193] Bubble area = (circumference) × (bubble diameter of TD / 2) × (bubble diameter of ZD / 2)
[0194] Based on the 50 bubble areas thus obtained, the average bubble area and the standard deviation of the bubble area were obtained. Furthermore, as shown in the following formula, the value obtained by dividing the standard deviation of the bubble area by the average bubble area was defined as the coefficient of variation of the bubble area.
[0195] Coefficient of variation of bubble area = standard deviation of bubble area / average bubble area
[0196] In addition, the following general calculation formula was used to calculate the standard deviations (the standard deviation of the cell diameter in TD, the standard deviation of the cell diameter in ZD, the standard deviation of the cell flatness, and the standard deviation of the cell area).
[0197] It should be noted that σ is the standard deviation, X is the measurement data, and n is the number of measurements.
[0198] [Number 1]
[0199]
[0200] <Foaming ratio>
[0201] The apparent density of the foam was measured in accordance with JIS K 7222, and the reciprocal thereof was defined as the expansion ratio.
[0202] <Degree of cross-linking (gel fraction)>
[0203] A test piece of about 100 mg was taken from the foam, and the mass A (mg) of the test piece was accurately weighed. Next, the test piece was placed in xylene at 115°C for 30 cm 3 After being immersed in the solution and left for 24 hours, the insoluble matter on the metal mesh was filtered through a 200-mesh metal mesh, vacuum dried, and the mass B (mg) of the insoluble matter was accurately weighed. The crosslinking degree (mass %) was calculated from the obtained value by the following formula.
[0204] Gel fraction (mass %) = 100 × (B / A)
[0205] <Tensile strength, tensile elongation>
[0206] The foam was cut into a dumbbell No. 1 shape specified in JIS K6251 4.1. This was used as a sample, and the tensile strength and tensile elongation in MD and TD were measured at a measurement temperature of 120° C. in accordance with JIS K6767.
[0207] <Dimensional change rate after heating>
[0208] The heating dimensional change rates of the foam in MD and TD at 120° C. were measured in accordance with JIS K 6767.
[0209] <Odor Evaluation>
[0210] 25cm 3 2 test pieces (50cm in total) 3) was added to a 1 L glass bottle, covered with a lid, and cured in an oven adjusted to 105°C for 2 hours. Then, the glass bottle was taken out and cooled to 23°C.
[0211] The cap of the glass bottle kept at 23°C was opened, and the odor was smelled with the nose at a position 1 cm away from the mouth of the glass bottle.
[0212] The odor rating was determined by comparing the intensity of the odor perceived to which level the following n-butanol dilution in water corresponds.
[0213] Odor level 10: n-butanol concentration 0ml / L (pure water alone)
[0214] Odor level 9.0: n-butanol concentration 1.2ml / L
[0215] Odor level 8.0: n-butanol concentration 1.4ml / L
[0216] Odor level 7.0: n-butanol concentration 2.0ml / L
[0217] Odor level 6.0: n-butanol concentration 3.6ml / L
[0218] Odor level 5.5: n-butanol concentration 6.0ml / L
[0219] Odor level 5.0: n-butanol concentration 9.0ml / L
[0220] Odor level 4.5: n-butanol concentration 18.0ml / L
[0221] Odor level 4.0: n-butanol concentration 22.7ml / L
[0222] Odor level 3.0: n-butanol concentration 30.0ml / L
[0223] Odor level 2.0: n-butanol concentration 57.0ml / L
[0224] Odor level 1.0: n-butanol only
[0225] The odor was evaluated by three persons, and the average value of the odor levels of the three persons was evaluated according to the following criteria.
[0226] A: The average odor level is 6.0 or above
[0227] B: The average odor level is more than 5.5 and less than 6.0
[0228] C: The average odor level is 5.5 or less
[0229] <Amount of filler in polyolefin resin foam>
[0230] The amount of the filler relative to the total amount of the polyolefin-based resin foam was measured by the following method.
[0231] The polyolefin resin foam Xg (e.g. 5g) was added to a calcining dish (heat resistant temperature 1900°C, 150mm×150mm×5mm) and allowed to stand in an electric heating muffle furnace (width 100mm, depth 180mm, height 100mm, Yamato Science FM-27). The temperature was raised from room temperature (25°C) to 200°C at 50°C / min in an air atmosphere and maintained for 30 minutes. After maintaining, the temperature was raised to 600°C at 50°C / min, and after reaching 600°C, it was maintained for 2 hours. Then, the temperature was lowered to room temperature (25°C), the calcining dish was taken out, and the mass of the combustion residue was measured by an electronic balance.
[0232] The amount of the filler in the polyolefin-based resin foam was determined by the following formula.
[0233] Amount of filler in polyolefin resin foam (mass %) = [mass of combustion residue (g) / mass of foam X (g)] × 100
[0234] It should be noted that the elemental analysis of the combustion residue can be performed by an ICP emission spectrometry mass spectrometer (SELFA SSGW-7602). For example, 0.05 g of the combustion residue is weighed, added to 10 mL of 1% nitric acid, heated at 60°C for 2 hours, and then the total amount is diluted to 100 mL. The combustion residue can be qualitatively and quantitatively analyzed by an ICP emission spectrometry mass spectrometer (SELFA SSGW-7602).
[0235] The materials used in Examples and Comparative Examples are as follows.
[0236] <Polyolefin resin>
[0237] Homopolypropylene: J106G (manufactured by Polymer Co., Ltd.), MFR=15g / 10 minutes (230℃)
[0238] Random polypropylene: AD571 (manufactured by Sumitomo Chemical Co., Ltd.), density 0.90 g / cm 3 , MFR = 0.5g / 10min (230℃)
[0239] Linear low-density polyethylene (LLDPE): Ultezex 1020L, density 0.91 g / cm 3 , MFR = 2.0g / 10min (190℃)
[0240] TPO: Softell CA 02A (Basell)
[0241] EPDM: 3045 (Mitsui Chemicals), MFR = 0.6 g / 10 min (230°C)
[0242] <Metal oxide>
[0243] Magnesium oxide: RF-50C-SC (manufactured by Ube Materia Co., Ltd.)
[0244] <Metal hydroxide>
[0245] Magnesium hydroxide: Magnesium hydroxide S (manufactured by Kamishima Chemical Industry Co., Ltd.)
[0246] <Crosslinking aid>
[0247] 1,9-Nonanediol dimethacrylate: Light Ester 1.9ND (manufactured by Kyoeisha Chemical Co., Ltd.) Viscosity 8 mPa·s (25°C)
[0248] <Thermal decomposition type foaming agent>
[0249] Azodicarbonamide: SOL (manufactured by Otsuka Chemical Co., Ltd.), decomposition temperature: 197°C, average particle size: 3.2 μm
[0250] <Antioxidants>
[0251] The following phenolic antioxidants and phosphorus antioxidants were used in combination.
[0252] Phenolic antioxidants: Ilganox 1010 (manufactured by BASF Japan), tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane
[0253] Phosphorus antioxidants: ADEKASTAB PEP-8 (ADEKA), 3,9-bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane
[0254] [Example 1]
[0255] The linear low-density polyethylene and magnesium oxide were fed into an extruder, mixed, and cut into pellets to obtain a filler masterbatch having a magnesium oxide content of 20% by mass.
[0256] The filler masterbatch, polyolefin resins of the type listed in Table 1, a thermally decomposable foaming agent, an antioxidant, and a crosslinking aid were fed into an extruder and melt-kneaded to obtain a foamable composition in the form of a sheet having a thickness of 1.42 mm. The composition of the foamable composition is shown in Table 1.
[0257] The obtained sheet-shaped foamable composition was cross-linked by irradiating both surfaces with electron beams at an accelerating voltage of 1000 kV and 2.0 Mrad. The cross-linked foamable composition was heated to 270° C. to obtain a density of 0.05 g / cm 3 (foaming ratio 20cm 3 / g), a foam with a thickness of 2.5 mm.
[0258] [Example 2]
[0259] A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 0.65 mm. The density of the obtained foam was 0.10 g / cm 3 (foaming ratio 10cm 3 / g), thickness is 1.0mm.
[0260] [Example 3]
[0261] A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 1.35 mm. The density of the obtained foam was 0.04 g / cm 3 (foaming ratio 25cm 3 / g), with a thickness of 2.5mm.
[0262] [Example 4]
[0263] A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 1.30 mm. The density of the obtained foam was 0.04 g / cm 3 (foaming ratio 25cm 3 / g), with a thickness of 2.5mm.
[0264] [Example 5]
[0265] Random polypropylene and magnesium oxide were fed into an extruder, mixed, and cut into pellets to obtain a filler masterbatch having a magnesium oxide content of 25% by mass.
[0266] The filler masterbatch, polyolefin resins of the type listed in Table 1, a thermally decomposable foaming agent, an antioxidant, and a crosslinking aid were fed into an extruder and melt-kneaded to obtain a foamable composition in the form of a sheet having a thickness of 1.85 mm. The composition of the foamable composition is shown in Table 1.
[0267] The obtained sheet-shaped foamable composition was cross-linked by irradiating both surfaces with electron beams at an accelerating voltage of 1000 kV and 2.0 Mrad. The cross-linked foamable composition was heated to 270° C. to obtain a density of 0.05 g / cm 3 (foaming ratio 20cm 3 / g), a foam with a thickness of 3.6 mm.
[0268] [Example 6]
[0269] A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 1.45 mm. The density of the obtained foam was 0.07 g / cm 3 (foaming ratio 15cm 3 / g), and the thickness is 2.0mm.
[0270] [Example 7]
[0271] A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 0.85 mm. The density of the obtained foam was 0.05 g / cm 3 (foaming ratio 20cm 3 / g), thickness is 1.5mm.
[0272] [Example 8]
[0273] A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1. The density of the obtained foam was 0.05 g / cm 3 (foaming ratio 20cm 3 / g), with a thickness of 2.5mm.
[0274] [Example 9]
[0275] A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1 and the thickness of the sheet-like foamable composition was changed to 1.45 mm. The density of the obtained foam was 0.07 g / cm 3 (foaming ratio 15cm 3 / g), and the thickness is 2.0mm.
[0276] [Comparative Example 1]
[0277] The polyolefin resins, thermally decomposable foaming agents, magnesium oxide, antioxidants, and crosslinking aids of the types listed in Table 1 were fed into an extruder and melt-kneaded to obtain a foamable composition in the form of a sheet having a thickness of 1.8 mm. The composition of the foamable composition is as shown in Table 1.
[0278] The obtained sheet-shaped foamable composition was cross-linked by irradiating both surfaces with electron beams at an accelerating voltage of 1000 kV and 2.0 Mrad. The cross-linked foamable composition was heated to 270° C. to obtain a density of 0.067 g / cm 3 (foaming ratio 15cm 3 / g), a foam with a thickness of 3.0 mm.
[0279] [Comparative Example 2]
[0280] A foam was obtained in the same manner as in Example 1 except that the composition was changed as shown in Table 1. The density of the obtained foam was 0.05 g / cm 3 (foaming ratio 20cm 3 / g), with a thickness of 2.5mm.
[0281] [Comparative Example 3]
[0282] A foam was obtained in the same manner as in Comparative Example 1 except that the composition was changed as shown in Table 1 and the thickness of the foamable composition in sheet form was changed to 0.65 mm. The density of the obtained foam was 0.10 g / cm 3 (foaming ratio 10cm 3 / g), thickness is 1.0mm.
[0283] [Comparative Example 4]
[0284] A foam was obtained in the same manner as in Comparative Example 1 except that the composition was changed as shown in Table 1 and the thickness of the foamable composition in sheet form was changed to 1.30 mm. The density of the obtained foam was 0.04 g / cm 3 (foaming ratio 25cm 3 / g), and the thickness is 2.0mm.
[0285] [Table 1]
[0286]
[0287] It is found that the foam of the present invention having a metal oxide content of at least a certain value and each coefficient of variation of the TD cell diameter, the ZD cell diameter, the cell flatness, and the cell area being at or below a certain value can reduce the generation of odor.
[0288] On the other hand, it is found that the foam of Comparative Example 1 having large coefficients of variation and the foams of Comparative Examples 2 to 4 in which a small amount of metal oxide is mixed or no metal oxide is mixed generate a large amount of odor.
Claims
1. A polyolefin resin foam, wherein the coefficient of variation of the cell diameter in the width direction TD and the coefficient of variation of the cell diameter in the thickness direction ZD per 50 cells contained in the foam are respectively 0.38 or less, the coefficient of variation of the cell flatness is 0.45 or less, and the coefficient of variation of the cell area is 0.65 or less, The polyolefin resin foam contains a polyolefin resin and at least one filler selected from metal oxides and metal hydroxides, wherein the content of the filler is 0.3% by mass or more based on the total amount of the polyolefin resin foam. 2 . The polyolefin-based resin foam according to claim 1 , wherein a coefficient of variation of cell diameters in the width direction TD is 0.35 or less. The polyolefin resin foam according to claim 1 or 2, wherein a coefficient of variation of cell diameters in the thickness direction ZD is 0.33 or less. The polyolefin resin foam according to claim 1 or 2, wherein the coefficient of variation of the cell flatness is 0.40 or less. The polyolefin resin foam according to claim 1 or 2, wherein the coefficient of variation of the cell area is 0.60 or less. The polyolefin-based resin foam according to claim 1 or 2, wherein the content of the filler is 0.5% by mass or more based on the total amount of the polyolefin-based resin foam. The polyolefin resin foam according to claim 1 or 2, wherein the filler is a metal oxide. 8 . The polyolefin-based resin foam according to claim 1 , wherein the polyolefin-based resin contains a polypropylene-based resin.
9. A polyolefin resin foam, wherein the coefficient of variation of the cell diameter in the width direction TD and the coefficient of variation of the cell diameter in the thickness direction ZD per 50 cells contained in the foam are respectively 0.38 or less, the coefficient of variation of the cell flatness is 0.45 or less, and the coefficient of variation of the cell area is 0.65 or less, The polyolefin resin foam includes a polyolefin resin and at least one filler selected from metal oxides and metal hydroxides, wherein the content of the filler is 0.4 parts by mass or more relative to 100 parts by mass of the polyolefin resin. 10 . A molded product obtained by molding the polyolefin resin foam according to claim 1 or 2. 11 . The molded article according to claim 10 , wherein a skin material is laminated on at least one surface of the polyolefin-based resin foam.