Composite resin molded article and method for producing same
By using natural fibers and composite resin moldings coated with resin to support microorganisms and enzymes in biodegradable plastics, the problems of slow decomposition and insufficient mechanical strength of biodegradable plastics in humid environments have been solved, and a high elastic modulus has been achieved. and rapid biodegradation, suitable for industrial and daily necessities.
Patent Information
- Application Number
- CN202280092495.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-02
- Filing Date
- 2022-09-21
- Publication Date
- 2024-10-11
AI Technical Summary
Biodegradable plastics decompose slowly in humid environments and have insufficient mechanical strength, which limits their application in mechanical products and industrial products such as automobiles. Existing technologies such as microbial products and microencapsulation methods have problems with reduced rigidity and thermal damage.
A composite resin molded body is used, which contains the main agent biodegradable resin, natural fiber and coating resin. The surface of the natural fiber is loaded with microorganisms and enzymes, and the fiber contact points and water absorption are increased through melting and mixing to form a highly water-absorbent composite resin. Promote biodegradation in humid environments.
It maintains high rigidity and high elastic modulus during use, and rapidly biodegrades in the ocean and soil after being discarded, reducing environmental load and replacing traditional petroleum-based plastics.
Smart Images

Figure CN118765308A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a composite resin molded body having excellent mechanical properties and a controlled biodegradation rate in a high-humidity environment, and a method for producing the same. Background Art
[0002] So-called "general-purpose plastics" such as polyethylene (PE), polypropylene (PP), polystyrene (PS), and polyvinyl chloride (PVC) are not only very cheap, but also easy to shape and lightweight, with a weight only a fraction of that of metals or ceramics. Therefore, general-purpose plastics are used as materials for a variety of daily necessities such as bags, various packages, various containers, and sheets, as well as for industrial parts such as automobile parts and electrical parts, and as materials for daily necessities and sundry goods.
[0003] Due to such circumstances, the amount of plastic waste after use is increasing year by year. Plastic waste is a substance with the characteristic of being difficult to decompose and accumulates in the natural environment, thus causing public nuisance problems such as damage and pollution of the natural environment. In recent years, as one of the strategies to solve these problems, biodegradable plastics that can be decomposed into water and carbon dioxide in the natural environment have been proposed, and it is expected that they will replace general-purpose plastics using petroleum-based raw materials and expand their applications.
[0004] However, biodegradable plastics have disadvantages such as insufficient mechanical strength compared to general-purpose plastics. Therefore, the current situation is that biodegradable plastics do not have sufficient properties required for materials used in various industrial products such as mechanical products such as automobiles and electrical / electronic / information products, and their application range is limited.
[0005] On the other hand, the environment has a great influence on the biodegradation rate of discarded biodegradable plastics. In an environment with few microorganisms such as the ocean, it takes a long time to achieve complete decomposition, and the biodegradability cannot be fully utilized. In order to solve this problem, various methods have been proposed to accelerate the decomposition of discarded biodegradable plastics.
[0006] In order to solve such problems, products in which microorganisms having enzyme activity to decompose biodegradable plastics are compounded (for example, see Patent Document 1) and methods in which pre-encapsulated microorganisms are contained in biodegradable plastics (for example, see Patent Document 2) are disclosed.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2013-209587
[0010] Patent Document 2: Japanese Patent Application No. 2020-520794 Summary of the invention
[0011] A composite resin molded body according to one embodiment of the present invention is a composite resin molded body comprising: a main resin, a plurality of natural fibers dispersed in the main resin, and at least one of a microorganism and an enzyme carried by each of the plurality of natural fibers, at least one of the plurality of natural fibers having a portion exposed on the surface of the composite resin molded body, and at least a portion of the surface of each of the plurality of natural fibers being coated with a coating resin.
[0012] A method for manufacturing a composite resin molded body according to one embodiment of the present invention comprises: a step of preparing at least one of a microorganism and an enzyme, a natural fiber, a water-soluble coating resin, and a main resin; a step of causing at least one of the microorganism and the enzyme to be carried on the natural fiber; a step of dispersing the natural fiber carrying at least one of the microorganism and the enzyme, and the coating resin in water, drying and crushing the natural fiber to obtain a coated natural fiber in which at least a portion of the surface of the natural fiber is coated with the coating resin; a step of melt-kneading the coated natural fiber and the main resin to defibrate the coated natural fiber from the end portion in the fiber length direction to obtain a composite resin material with an enlarged surface area of the defibrated portion at the end portion; and a step of molding the composite resin material to obtain a composite resin molded body. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a schematic diagram showing a cross-sectional structure of a composite resin molded body according to an embodiment.
[0014] Figure 2 It is a schematic diagram showing the cross-sectional structure of natural fibers which are a constituent material of the composite resin molded body according to the embodiment.
[0015] Figure 3 It is a schematic diagram showing the cross-sectional structure of a composite resin molded body containing natural fibers having a defibrated portion according to an embodiment.
[0016] Figure 4 It is a schematic diagram of a production process of a composite resin molded body according to an embodiment.
[0017] Figure 5 The figures show the structures and measurement results of composite resin molded bodies of Examples and Comparative Examples of the embodiment. DETAILED DESCRIPTION
[0018] In the method described in Patent Document 1, since microorganisms are directly kneaded into biodegradable plastics, the material is limited to biodegradable plastics that can be molded at a temperature at which the microorganisms can survive.
[0019] On the other hand, the method described in Patent Document 2 has the problem that the molded body needs to be physically destroyed in order to release the microorganisms from the microcapsules, and also has the problem that the rigidity of the molded body decreases as the content of the microcapsules increases.
[0020] An object of one embodiment of the present disclosure is to solve the above-mentioned conventional problems and to provide a composite resin molded body that maintains high rigidity during use and promotes biodegradation in a humid environment such as the ocean or soil after disposal.
[0021] The first type of composite resin molded body is a composite resin molded body having a main resin, a plurality of natural fibers dispersed in the main resin, and at least one of microorganisms and enzymes carried by each of the plurality of natural fibers, at least one of the plurality of natural fibers having a portion exposed on the surface of the composite resin molded body, and at least a portion of the surface of each of the plurality of natural fibers is coated with a coating resin.
[0022] In the above-mentioned first aspect, the moisture content of the natural fibers of the composite resin molded body of the second aspect may be 5% or more according to the method specified in JIS L0105:2020.
[0023] In the first or second aspect described above, the main resin of the composite resin molded body of the third aspect may be a biodegradable resin containing any one selected from the group consisting of polyhydroxy acids, polyhydroxyalkanoates, polyalkylene dicarboxylates, and modified starches.
[0024] In any one of the first to third aspects described above, the coating resin of the composite resin molded body of the fourth aspect may be any water-soluble resin selected from the group consisting of polyvinyl alcohol, polyethylene oxide, carboxymethyl cellulose, and starch-based resins.
[0025] In any of the above-mentioned methods 1 to 4, for the composite resin molded body of the 5th method, when the composite resin molded body is set to 100 volume %, if the volume % of the main resin is set to A, the volume % of the natural fiber 2 carrying at least one of the microorganism and the enzyme is set to B, and the volume % of the coating resin 3 is set to C, then A+B+C=100, and 0.01B≤C≤0.5B, and 10≤B+C≤99, and C≤A can also be established.
[0026] In any one of the first to fifth aspects described above, each of the plurality of natural fibers in the composite resin molded body of the sixth aspect may carry at least one of a microorganism and an enzyme on the fiber surface.
[0027] In any one of the first to sixth aspects described above, the plurality of natural fibers in the composite resin molded body of the seventh aspect may each be cellulose.
[0028] In any one of the first to seventh aspects described above, the plurality of natural fibers of the composite resin molded body of the eighth aspect may each have a defibrated portion at an end portion in the fiber length direction.
[0029] The manufacturing method of the composite resin molded body of the 9th mode includes: the step of preparing at least one of a microorganism and an enzyme, a natural fiber, a water-soluble coating resin, and a main resin; the step of causing at least one of the microorganism and the enzyme to be carried on the natural fiber; the step of dispersing the natural fiber carrying at least one of the microorganism and the enzyme, and the coating resin in water, drying and crushing them, and obtaining coated natural fibers in which at least a portion of the surface of the natural fiber is coated with the coating resin; the step of melt-kneading the coated natural fiber and the main resin together to defibrate the coated natural fiber from the end portion in the fiber length direction, and obtaining a composite resin material with an enlarged surface area of the defibrated portion at the end portion; and the step of molding the composite resin material to obtain a composite resin molded body.
[0030] Hereinafter, a composite resin molded body and a method for producing the same according to an embodiment will be described with reference to the drawings. In the following description, the same components are denoted by the same reference numerals, and the description thereof will be appropriately omitted.
[0031] (Implementation Method)
[0032] Figure 1 It is a schematic diagram showing a cross-sectional structure of a composite resin molded body 10 according to the embodiment. Figure 2 Schematic diagram showing a cross-sectional structure of natural fibers as a constituent material of the composite resin molded body 10 according to the embodiment.
[0033] The composite resin molded body 10 of the embodiment includes a melt-kneaded product of a main resin 1 and a natural fiber 2 supported with a microorganism and / or an enzyme 4 (at least one of the microorganism and the enzyme) and coated with a coating resin 3. Figure 1 As shown in the schematic diagram showing the cross-sectional structure of FIG. 1 , the natural fiber 2 carrying the microorganism and / or enzyme 4 and covered with the covering resin 3 is dispersed in the main component resin 1 of the composite resin molded body 10 .
[0034] Furthermore, if Figure 3 As shown in the schematic diagram of the cross-sectional structure of the composite resin molded body 10 containing the natural fiber 2 having the defibration site according to the embodiment, by having the defibration site at the end of the natural fiber 2, the specific surface area of the defibration site increases, and the contact points between the natural fibers 2 increase. As a result, water can be absorbed into the interior of the composite resin molded body 10 through the contact points between the natural fibers 2 in a humid environment.
[0035] According to the composite resin molded body 10, at least one natural fiber 2 is exposed on the surface of the composite resin molded body. Since the natural fibers 2 have contact points with each other, they have high water absorption in addition to high elastic modulus. In a humid environment, when the water absorption of the natural fiber 2 causes the coating resin 3 to be dissolved, the microorganisms and / or enzymes 4 carried by the natural fiber 2 are released, and the decomposition of the main resin 1 is promoted. Therefore, it is possible to realize a composite resin molded body 10 that maintains high rigidity during use and has excellent biodegradability in a humid environment such as the ocean and soil after disposal.
[0036] Hereinafter, each material constituting the composite resin molded body will be described.
[0037] <Main resin>
[0038] In this embodiment, the main resin 1 is preferably a biodegradable plastic selected from polyhydroxy acid, polyhydroxyalkanoate, polyalkylene dicarboxylate, and modified starch. In addition, in order to ensure good formability, it is preferably a thermoplastic resin, and the above resins can be used alone or in combination of two or more. It should be noted that the main resin 1 is not limited to the above materials as long as it is biodegradable.
[0039] In the present embodiment, "biodegradable plastic" refers to "a resin that has the same function as existing petroleum-derived resins when used, and is ultimately decomposed into water and carbon dioxide by microorganisms in the soil and ocean in nature after use". Specifically, it includes polyhydroxyalkanoates such as polyhydroxybutyrate and polyhydroxyvalerate, polyhydroxy acids such as polylactic acid, polyglycolic acid, and polycaprolactone, polyester resins such as polyalkylene dicarboxylates such as polybutylene adipate terephthalate, polyethylene succinate, and polybutylene succinate, polyamides, modified starch, and the like. In addition to homopolymers of the monomers of the above-mentioned resins, biodegradable plastics may also include copolymers of the monomers of the above-mentioned resins such as poly(3-hydroxybutyrate-co-3-hydroxyvalerate), and copolymers of the monomers of the above-mentioned resins with other copolymerizable monomers.
[0040] <Natural Fiber>
[0041] Next, the natural fiber 2 is described. The first main purpose of adding the natural fiber 2 (hereinafter, sometimes simply referred to as "fiber") contained in the composite resin molded body 10 of the present embodiment is that when the composite resin molded body 10 is discarded after use, it does not impose a load on the environment, and absorbs water in the soil or the ocean, so that the coating resin 3 comes into contact with water and dissolves. For this purpose, the natural fiber 2 preferably has high water absorption, and the moisture content of the natural fiber 2 is preferably 5% or more according to the method specified in JIS L0105: 2020. Specifically, pulp, cellulose, cellulose nanofiber, wood cellulose, wood cellulose nanofiber, cotton, silk or hemp is preferred.
[0042] The second purpose of adding natural fiber 2 is to improve dimensional stability by improving mechanical properties and reducing linear expansion coefficient. For this purpose, natural fiber 2 preferably has a higher elastic modulus than main resin 1. Specifically, pulp, cellulose, cellulose nanofiber, lignocellulose, lignocellulose nanofiber, cotton, silk, wool or hemp can be cited. In addition, among these, cellulose is particularly preferred from the viewpoint of availability, high elastic modulus and low linear expansion coefficient. It should be noted that natural fiber 2 is not limited to the above-mentioned materials as long as it can improve mechanical properties and has water absorption.
[0043] The natural fiber 2 carries the microorganism and / or enzyme 4, and after at least a part of the natural fiber is coated with the coating resin 3, the content of the natural fiber 2 carrying the microorganism and / or enzyme 4 and the coating resin 3 in the composite resin molded body 10 is preferably 10% by volume or more and 99% by volume or less when the composite resin molded body 10 is set to 100% by volume. When the content of the natural fiber 2 carrying the microorganism and / or enzyme 4 and the coating resin 3 is less than 10% by volume, it is difficult for the natural fibers 2 to have contact points with each other inside the composite resin molded body 10, and the natural fibers 2 do not have sufficient water absorption. On the other hand, when the content of the natural fiber 2 carrying the microorganism and / or enzyme 4 and the coating resin 3 is greater than 99% by volume, the proportion of the main resin 1 becomes small, so that the effect of bonding the natural fibers 2 to each other disappears, and the moldability deteriorates.
[0044] The morphology of the natural fiber 2 in the composite resin molded body 10 is described. Since the larger the bonding interface between the natural fiber 2 and the coating resin 3, the more the dissolution of the coating resin 3 is promoted when the natural fiber 2 absorbs water, the higher the specific surface area of the natural fiber 2 is preferably. On the other hand, in order to improve the water absorbency of the composite resin molded body 10, the natural fiber 2 is preferably exposed on the surface of the composite resin molded body 10. As the natural fiber 2 is exposed on the surface of the composite resin molded body 10, water is absorbed by the exposed portion of the natural fiber 2, and the water is absorbed into the interior of the composite resin molded body 10 by the capillary phenomenon of the fibers constituting the natural fiber. The smaller the specific surface area of the exposed portion of the natural fiber 2 exposed on the surface of the composite resin molded body 10, the higher the water absorbency. This is because when the specific surface area of the exposed portion of the natural fiber 2 exposed on the surface is large, the effect of fine concavo-convexity leads to improved waterproofness. Furthermore, as Figure 3 As shown, by having the defibrated portion at the end of the natural fiber 2, the specific surface area of the defibrated portion increases, and the contact points between the natural fibers 2 increase, thereby increasing the water absorption rate through the contact points of the natural fibers 2 in a humid environment.
[0045] The central portion of the natural fiber 2 having a small specific surface area and not defibrated is less entangled with the main resin 1 and is easily exposed on the surface of the composite resin molded body according to the molding conditions. On the contrary, the front end portion of the defibrated natural fiber 2 is more entangled with the main resin 1 and enters the interior together with the main resin 1. Thus, a composite resin molded body 10 can be obtained in which the central portion of the natural fiber 2, excluding the two end portions, is exposed on the surface.
[0046] The total length of the front end defibrated portions present at both ends of the natural fiber 2 is preferably 5% or more and 50% or less of the fiber length L of the entire natural fiber 2. When the defibrated portions are less than 5% of the overall fiber length L, the elastic modulus cannot be improved due to the small specific surface area, and when the defibrated portions are longer than 50% of the overall fiber length L, the defibrated portions with a large aspect ratio are exposed on the surface of the composite resin molded body, and the water absorption becomes poor.
[0047] Next, the characteristics of natural fiber 2 are described. About the types of main agent resin 1 and natural fiber 2, as mentioned above, if natural fiber 2 is too soft relative to main agent resin 1, that is, the elastic modulus of natural fiber 2 is small, then the elastic modulus of composite resin molded body 10 as a whole becomes small, and the strength is reduced as a result. On the other hand, if natural fiber 2 is too hard relative to main agent resin 1, that is, the elastic modulus of natural fiber 2 is large, then the shock wave generated during impact cannot be propagated, and is absorbed at the interface between main agent resin 1 and natural fiber 2, so cracks and cracks are easily generated near the interface, and the impact resistance is reduced as a result. Therefore, the relationship between the elastic modulus of main agent resin 1 and the elastic modulus of natural fiber 2 is preferably: the elastic modulus of natural fiber 2 is higher than the elastic modulus of main agent resin 1, and the smaller their difference, the better. As the most suitable relationship, it can be calculated according to the simulation results, and the elastic modulus difference between main agent resin 1 and natural fiber 2 is preferably within 20GPa.
[0048] In addition, these natural fibers 2 are sometimes surface-treated for the purpose of improving their adhesion to the main resin 1 and the coating resin 3 or improving their dispersibility in the composite resin molded body 10. However, when the water absorption of the natural fibers 2 is impaired due to the surface treatment, it is preferably not to perform surface treatment in advance.
[0049] <Additives>
[0050] Additives may be used as needed for purposes such as improving the affinity between the main resin 1 and the natural fiber 2. It should be noted that commonly used additives may be used.
[0051] <Coating resin>
[0052] Next, the coating resin 3 is described. The coating resin 3 in this embodiment protects the microorganisms and / or enzymes 4 carried by the natural fibers 2 during the manufacture of the composite resin molded body 10, and inhibits the microorganisms and / or enzymes 4 from being thermally damaged by the molten main resin 1. In addition, in the use of the composite resin molded body 10, it is used for the purpose of protecting the microorganisms and / or enzymes 4 carried by the natural fibers 2 and preventing them from contacting the main resin 1. After the composite resin molded body 10 is discarded, in order to promote its biodegradation in a humid environment, it is necessary to dissolve the coating resin 3 and release the microorganisms and / or enzymes 4 carried by the natural fibers 2. Therefore, the coating resin 3 is preferably a water-soluble resin that is soluble in water at a temperature of 20°C. Specifically, polyvinyl alcohol, polyethylene oxide, carboxymethyl cellulose, and modified starches can be cited. The above resins can be used alone or in combination of two or more. It should be noted that the coating resin 3 is not limited to the above materials as long as it is water-soluble.
[0053] In addition, in the composite resin molded body 10, in order to maintain the state in which the coating resin 3 is coated on at least a part of the surface of the natural fiber 2, when the composite resin molded body 10 is set to 100 volume %, if the volume % of the main resin 1 is A, the volume % of the natural fiber 2 carrying the microorganism and / or enzyme 4 is B, and the volume % of the coating resin 3 is C, it is preferred that A+B+C=100, 0.01B≤C≤0.5B, and C≤A hold. When 0.5B<C, the volume % of the coating resin 3 relative to the natural fiber 2 is too large, and it is difficult to maintain the contact points between the natural fibers 2. When C<0.01B, the volume % of the coating resin 3 relative to the natural fiber 2 is too small, and it is difficult to protect the microorganism and / or enzyme 4 carried by the natural fiber 2. When A<C, the volume % of the coating resin 3 is too large, and the water-soluble coating resin 3 exposed on the surface of the composite resin molded body 10 becomes easy to deteriorate, so it is difficult to maintain durability.
[0054] The present state of the coating resin 3 in the composite resin molded body 10 will be described. The coating resin 3 can control the decomposition rate by controlling the volume % of the natural fiber 2 to delay the release of the microorganisms and / or enzymes 4 carried by the natural fiber 2.
[0055] <Microorganisms and / or enzymes>
[0056] Next, the microorganism and / or enzyme 4 is described. The microorganism and / or enzyme 4 in the present embodiment is used for the purpose of accelerating the decomposition of the composite resin molded body 10 in a humid environment. The microorganism and / or enzyme 4 in the present embodiment varies according to the main resin 1. Specifically, microorganisms of the genus Amycolatopsis as polylactic acid decomposition substances and polybutylene succinate decomposition substances can be cited. In addition, as poly 3-hydroxybutyric acid decomposition substances, there can be cited: microorganisms of the genus Streptomyces; microorganisms of the genus Pseudomonas, such as Pseudomonas reuteri; microorganisms of the genus Alcaligenes, Alcaligenes arguably, etc. Furthermore, as decomposition substances of polyethers such as polyvinyl alcohol, there can be cited: microorganisms of the genus Pseudomonas, such as Pseudomonas stutzeri, Pseudomonas aeruginosa, Pseudomonas vesicularis; microorganisms of the genus Alcaligenes; microorganisms of the genus Acinetobacter; microorganisms of the genus Xanthomonas, etc.
[0057] As the enzyme in the present embodiment, for example, various enzymes extracted from the above-mentioned microorganism can be cited. Specifically, as the enzyme used for the decomposition of polylactic acid, proteinase K, polyvinyl alcohol dehydrogenase, polyvinyl alcohol oxidase, secondary alcohol oxidase, etc. can be cited, as the enzyme used for the decomposition of polylactic acid, PHB depolymerase can be cited, as the enzyme used for the decomposition of poly 3-hydroxybutyric acid, cholesterol esterase, chitosan cholesterol esterase (Japanese: キトパールコレステロールエステラーゼ), urease, etc. can be cited. The above-mentioned microorganism and / or enzyme can be used alone, or two or more can be used in combination. It should be noted that as long as the microorganism and / or enzyme have decomposability for the main agent resin 1, they are not limited to the above-mentioned materials.
[0058] <Method for producing composite resin molded body>
[0059] Next, a method for producing the composite resin molded body 10 will be described. Figure 4 1 is a flowchart illustrating a process for producing the composite resin molded body 10 according to the present embodiment.
[0060] (1) The microorganism and / or enzyme 4 is supported on the surface of the natural fiber 2 in advance. The method of supporting the microorganism and / or enzyme 4 includes: physical adsorption based on dry mixing, impregnation of natural fibers with a dispersion solvent, crosslinking, and wrapping. The supporting method is not limited to the above method as long as it can maintain the microorganism and / or enzyme 4 on the surface of the natural fiber 2.
[0061] (2) After the natural fiber 2 carrying the microorganism and / or enzyme 4 and the water-soluble coating resin 3 are dispersed in water and dried, they are crushed by a cutter or a pulverizer, thereby obtaining the natural fiber 2 of the present embodiment in which at least a portion of the surface is coated with the coating resin 3. As specific methods, a granulator, a ball mill, a roller mill, a hammer mill, a Wonder crusher, a jet mill, and combinations thereof can be cited. As long as it is a method that can maintain the state in which at least a portion of the natural fiber 2 is coated with the coating resin 3, it may also be a cutting or pulverizing method other than the above.
[0062] (3) The main resin 1 and the natural fiber 2 coated with the coating resin 3 are dry-mixed and then placed in a melt-kneading treatment device for melt-kneading. At this time, since the natural fiber is coated with the coating resin 3, thermal damage to the microorganisms and / or enzymes carried by the natural fiber can be suppressed. Thus, the shearing action of the device promotes the defibration of the agglomerated mass of the natural fiber 2, and the coated natural fiber 2 can be finely dispersed in the main resin 1. At this time, by adjusting the shearing conditions, the ends of the natural fiber 2 can also be dispersed as shown in FIG. Figure 3 The fiber is defibrated as shown to obtain a defibrated portion.
[0063] In the past, when fibers were compounded into resins, materials obtained by defibration of fibers in advance through pretreatments such as wet dispersion were used. However, when natural fibers were defibrated in the solvent used for wet dispersion, the fibers swelled due to the solvent. Therefore, in order to allow the natural fibers to fully absorb water and swell in the composite resin forming material, the solvent in the natural fibers needed to be dried before being mixed with the main resin. In addition, compared with defibration in molten main resin, the fibers are more easily defibrated by wet dispersion, so it is difficult to defibrate only the ends, resulting in a state where the natural fibers are defibrated as a whole. In addition, due to the incorporation of pretreatments, there are problems of increased processes and poor productivity.
[0064] In contrast, in the manufacturing process of the composite resin molded body 10 of the present embodiment, a pretreatment based on wet dispersion for the purpose of defibration of the natural fiber 2 is not performed, but a melt-kneading treatment (complete dry process) is performed together with the main resin 1. In this process, by not performing a wet dispersion treatment of the natural fiber 2, the swelling of the natural fiber 2 in the manufacturing process can be suppressed, and the water absorption rate of the natural fiber 2 in the composite resin molded body 10 can be increased. By drying the natural fiber 2 in advance or during kneading, the water absorption rate of the composite resin molded body 10 in a humid environment can be further increased. In addition, since the natural fiber 2 has a defibration site as described above, there are more contact points between the fibers inside the composite resin molded body 10, and the water absorption rate of the composite resin molded body 10 can be increased through the contact points between the fibers.
[0065] When utilizing the full dry process to make the natural fiber 2 of the present embodiment, preferably high shear stress is applied during mixing. As specific mixing method, single shaft mixer, double shaft mixer, roller mixer, Banbury mixer and their combination etc. can be enumerated. From the viewpoint that high shear is easily applied and mass production is also high, particularly preferably continuous double shaft mixer, continuous roller mixer. As long as the method that high shear stress can be applied, then the mixing method other than the above-mentioned can also be used.
[0066] (4) By subjecting the composite resin composition extruded from the melt-kneading device to injection molding, a composite resin molded body 10 as an injection molded product can be produced.
[0067] Hereinafter, each Example and each Comparative Example in the experiment performed by the inventors will be described.
[0068] (Example 1)
[0069] In Example 1, a cellulose composite poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (PHBV) resin molded body was produced by the following production method.
[0070] As the starting material of natural fiber, conifer pulp (trade name: NBKP Celgar, manufactured by Mitsubishi Paper Co., Ltd.) was used. As the PHBV degrading enzyme, PHB depolymerase extracted from the culture solution of a microorganism of the genus Streptomyces was used. Conifer pulp and PHB depolymerase were dry-mixed to a volume ratio of 90:10, and pulverized by a roll mill to obtain a cellulose filler loaded with the enzyme.
[0071] The polyvinyl alcohol (PVA) (trade name: PVA-217 manufactured by Kuraray) as the coating resin and the above-mentioned cellulose filler loaded with the enzyme were weighed so that the volume ratio was 10:90, dispersed in pure water, and formed into sheets using a stretching machine (IMC-1124 manufactured by Imoto Seisakusho) and dried. The obtained cellulose PVA sheet was crushed using a Wonder crusher (WC-3 manufactured by Osaka Chemical) to obtain a cellulose filler coated with a PVA resin. The crushing condition was set to a rotation speed of 15,000 rpm.
[0072] The cellulose filler coated with PVA resin and PHBV (trade name: Y1000P manufactured by TianAn Biopolymer) as the main resin were weighed to a volume ratio of 90:10 and dry-mixed. Then, melt-mixed was performed using a twin-shaft mixer (KRC kneader manufactured by Kurimoto Iron Works). The screw was of medium shear type. The melt-mixed conditions were set to a material temperature of 180°C and a rotation speed of 50 min. -1 The composite resin composition discharged from the twin-screw kneading machine was thermally cut to produce cellulose composite PHBV resin pellets having a volume ratio of 10:81:9 among the main resin, the enzyme-loaded natural fiber, and the coating resin.
[0073] Then, a test piece of cellulose composite PHBV resin molded body was made by injection molding machine (180AD manufactured by Nippon Steel Works). The test piece production conditions were set as the temperature of the main resin 200°C, the metal mold temperature 50°C, the injection speed 100mm / s, and the holding pressure 100Pa. At this time, the total heating time of the above-mentioned melt kneading and injection molding was set within 5 minutes. The shape of the test piece was changed according to the evaluation items described below.
[0074] (Evaluation of water absorption of fibers)
[0075] The water absorption of the fiber is evaluated by measuring the moisture content of the fiber according to the method specified in JIS L0105:2020. Specifically, the weight of the fiber dried at 80°C for 24 hours is measured and used as the base weight. Then, the weight of the fiber maintained at a temperature of 20°C and a humidity of 65% for 24 hours is measured. The increased weight from the base weight is taken as the moisture content, and the moisture content is calculated. A moisture content of less than 5% is recorded as B, and a moisture content of more than 5% is recorded as A. For the composite resin molded body of Example 1, the moisture content of coniferous pulp is 6.5%, which is evaluated as A.
[0076] (Fiber end defibrillation)
[0077] The obtained cellulose composite PHBV resin molded body was immersed in chloroform and pure water to dissolve PHBV and PVA, and the remaining cellulose fibers were observed for their shape using SEM. In the composite resin molded body of Example 1, the ends of the fibers were in a defibrillated state.
[0078] (Evaluation of Elastic Modulus of Composite Resin Molded Article)
[0079] The obtained dumbbell-shaped test piece of JIS K7139 type A12 size was used to perform a three-point bending test. As a method for evaluating the elastic modulus, a value less than 200 MPa was recorded as B, and a value greater than 200 MPa was recorded as A. In the composite resin molded body of Example 1, the elastic modulus of the test piece was 605 MPa, and the evaluation was A.
[0080] (Deterioration Test of Composite Resin Molded Body)
[0081] A degradation test was carried out using the obtained JIS K7139 type A12 dumbbell-shaped test piece. The test piece was kept at a temperature of 60°C and a humidity of 40% for 48 hours. An environment of 60°C is an accelerated test about 50 times that of a normal atmosphere at room temperature. A three-point bending test was carried out using the test piece after the degradation test. As a degradation evaluation method, a reduction rate of the elastic modulus before the accelerated test of less than 10% is recorded as A, and a reduction rate of more than 10% is recorded as B. In the composite resin molded body of Example 1, the reduction rate of the elastic modulus of the test piece is 5%, and it is evaluated as A.
[0082] (Evaluation of Biodegradability of Composite Resin Molded Articles)
[0083] A biodegradation test was conducted using a rod-shaped test piece made of the obtained cellulose composite resin molded body. 50 g of a composting inoculum source (YK-11 manufactured by Yawata Bussan) was placed in a plastic container, and a rod-shaped test piece with a height of 20 mm, a width of 10 mm, and a thickness of 3 mm, which had been weighed in advance, was buried in the inoculum source. The weight reduction after being kept at a temperature of 58°C and a humidity of 50% for 2 months was evaluated. As a method for evaluating the biodegradability, a weight reduction value of 50% or more was recorded as AA, a weight reduction value of 40% or more and less than 50% was recorded as A, and a weight reduction value of less than 40% was recorded as B. In the composite resin molded body of Example 1, the biodegradability of the test piece was 41%, and it was evaluated as A.
[0084] (Example 2)
[0085] In Example 2, the volume ratio of the main resin, the enzyme-supported natural fiber, and the coating resin was changed to 40:40:20, and the material conditions and process conditions other than this were the same as those in Example 1 to produce a cellulose composite PHBV resin molded body. The same evaluation as in Example 1 was also performed.
[0086] (Comparative Example 1)
[0087] In Comparative Example 1, no coating resin was used and the volume ratio of the main resin to the enzyme-supported cellulose filler was changed to 19:81. The material conditions and process conditions other than these were the same as those in Example 1 to produce a cellulose composite PHBV resin molded body. The same evaluation as in Example 1 was also performed.
[0088] (Comparative Example 2)
[0089] In Comparative Example 2, no natural fiber was used and the volume ratio of the main resin, enzyme, and coating resin was changed to 82.9:8.1:9. The material conditions and process conditions other than these were the same as those in Example 1 to produce a PHBV composite resin molded body. The same evaluation as in Example 1 was also performed.
[0090] (Comparative Example 3)
[0091] In Comparative Example 3, the volume ratio of the main resin, the enzyme-supported natural fiber, and the coating resin was changed to 10:40:50, and the other material conditions and process conditions were the same as those in Example 1 to produce a cellulose composite PHBV resin molded body. The same evaluation as in Example 1 was also performed.
[0092] (Comparative Example 4)
[0093] In Comparative Example 4, PET fibers with a fiber diameter of 20 μm and a fiber length of 100 μm were used instead of softwood pulp to produce enzyme-supported PET fibers. The other material conditions and process conditions were the same as those in Example 1 to produce a PHBV composite resin molded body. The same evaluation as in Example 1 was performed.
[0094] The compositions and measurement results of the composite resin molded bodies of Examples 1 and 2 and Comparative Examples 1 to 4 are as follows: Figure 5 shown.
[0095] like Figure 5 As explained, in Examples 1 and 2, in which the enzyme carried by the natural fiber was protected by the coating resin, the elastic modulus was as high as 200 MPa or more, and Example 1, in which the ratio of the natural fiber was larger than that of Example 2, showed a higher elastic modulus. In a low humidity environment of 40%, the decrease in elastic modulus was suppressed compared with Comparative Example 3. The biodegradation rate was accelerated compared with the Comparative Example.
[0096] As described above, it has been confirmed that if natural fibers with enzymes loaded on their surfaces are compounded, at least a portion of the fiber surface of the natural fibers is covered with a water-soluble resin, the fibers are exposed on the surface of the composite resin molded body, and the natural fibers have a high water absorption rate, a composite resin with high elastic modulus, high durability, and high biodegradability can be obtained.
[0097] Comparative Example 1, which was prepared without using a coating resin, had an improved elastic modulus compared to Comparative Example 2 due to the compounding of natural fibers. However, since the enzyme was not protected by the coating resin during molding, the enzyme was severely thermally damaged during mixing and molding. Therefore, the biodegradation rate was lower than that of Example 1 and was evaluated as B.
[0098] In Comparative Example 2 produced without using natural fibers, since water absorption into the composite resin molded body was not performed by the natural fibers, dissolution of PVA did not proceed, and the biodegradation rate was lower than that of Example 1, and was evaluated as B.
[0099] In Comparative Example 3 in which the volume ratio of the coating resin to the main resin was high, the water-soluble coating resin dissolved in the degradation test, the elastic modulus decreased, and the elastic modulus reduction rate was evaluated as B.
[0100] Comparative Example 4, which was prepared using PET fiber instead of softwood pulp, did not dissolve PVA in the biodegradability evaluation because PET fiber had a low moisture content and no water absorption. The biodegradation rate was lower than that of Example 1 and was evaluated as B.
[0101] According to the above evaluation, it is confirmed that as long as a water-absorbent natural fiber and a biodegradable plastic are used, an enzyme is carried on the surface of the natural fiber, at least a part of the surface of the fiber is coated with a water-soluble coating resin, and the fiber is exposed on the surface of the composite resin molded body, a composite resin molded body with high elastic modulus, high durability and high biodegradability can be obtained. In addition, since the microorganisms and / or enzymes carried by the natural fiber are coated with the coating resin, the microorganisms and / or enzymes carried by the natural fiber can be protected from thermal damage due to the molten main agent resin during the melt kneading performed when manufacturing the composite resin molded body.
[0102] It should be noted that the present disclosure includes solutions obtained by appropriately combining any of the various embodiments and / or examples described above, which can achieve the effects of each embodiment and / or example.
[0103] The composite resin molded article of one embodiment of the present disclosure can realize a composite resin molded article that has not only a high elastic modulus compared to a resin alone but also a controlled biodegradation rate in a high-humidity environment and is accelerated.
[0104] Industrial Applicability
[0105] According to a composite resin molded body of one embodiment of the present invention, a molded body capable of controlling mechanical strength and biodegradation rate compared to conventional biodegradable plastics can be provided. According to a composite resin molded body of one embodiment of the present invention, since the properties of the main resin can be improved, it can be used as a substitute for general-purpose plastics derived from petroleum. As a result, the environmental load of various industrial products or daily necessities made of general-purpose plastics derived from petroleum can be greatly reduced. Furthermore, it can be used for packaging materials, daily necessities, home appliance housings, building materials, etc.
[0106] Description of Reference Numerals
[0107] 1 Main resin
[0108] 2 Natural Fibers
[0109] 3 Coating resin
[0110] 4 Microorganisms and / or enzymes
[0111] 10 Composite resin molded body
Claims
1. A composite resin molded body comprising a main resin, a plurality of natural fibers dispersed in the main resin, and at least one of a microorganism and an enzyme carried by each of the plurality of natural fibers, At least one of the plurality of natural fibers has a portion exposed on the surface of the composite resin molded body, At least a portion of the surface of each of the plurality of natural fibers is coated with a coating resin.
2. The composite resin molded article according to claim 1, wherein The plurality of natural fibers obtained by the method specified in JIS L0105:2020 each have a moisture content of 5% or more.
3. The composite resin molded article according to claim 1 or 2, wherein The main resin in the composite resin molded body is a biodegradable resin containing any one selected from the group consisting of polyhydroxy acids, polyhydroxyalkanoates, polyalkylene dicarboxylates, and modified starches.
4. The composite resin molded article according to any one of claims 1 to 3, wherein The coating resin is any water-soluble resin selected from polyvinyl alcohol, polyethylene oxide, carboxymethyl cellulose, and starch-based resins.
5. The composite resin molded article according to any one of claims 1 to 4, wherein When the composite resin molded body is set to 100 volume %, if the volume % of the main resin is set to A, the volume % of the natural fiber carrying at least one of the microorganism and the enzyme is set to B, and the volume % of the coating resin is set to C, then A+B+C=100, and 0.01B≤C≤0.5B, and 10≤B+C≤99, and C≤A hold.
6. The composite resin molded article according to any one of claims 1 to 5, wherein Each of the plurality of natural fibers in the composite resin formed body carries at least one of the microorganism and the enzyme on the fiber surface.
7. The composite resin molded article according to any one of claims 1 to 6, wherein Each of the plurality of natural fibers is cellulosic.
8. The composite resin molded article according to any one of claims 1 to 7, wherein Each of the plurality of natural fibers has a defibrated portion at an end portion in the fiber length direction.
9. A method for producing a composite resin molded body, comprising: A step of preparing at least one of a microorganism and an enzyme, natural fibers, a water-soluble coating resin, and a main resin; A step of allowing at least one of the microorganism and the enzyme to be supported on the natural fiber; The step of dispersing the natural fiber carrying at least one of the microorganism and the enzyme and the coating resin in water, drying and pulverizing the fibers, and obtaining coated natural fibers in which at least a portion of the surface of the natural fiber is coated with the coating resin; The step of melt-kneading the coated natural fibers together with the main resin to defiberize the coated natural fibers from the ends in the fiber length direction to obtain a composite resin material having an enlarged surface area of the defiberized portion at the ends; The step of molding the composite resin material to obtain a composite resin molded body.