Aluminum bronze alloy and sliding member using same
By adjusting the constituent elements and organizational structure of the aluminum bronze alloy to form appropriate Fe-Si intermetallic compounds and κ phase distribution, the deficiencies of the aluminum bronze alloy in terms of high load resistance and wear resistance are solved, and the application in seawater is achieved. Corrosion resistance and manufacturing stability in the environment, suitable for high load and wear-resistant sliding parts.
Patent Information
- Application Number
- CN202380023333.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-01
- Filing Date
- 2023-02-28
- Publication Date
- 2024-10-11
AI Technical Summary
Existing aluminum bronze alloys have deficiencies in high load resistance and wear resistance. In particular, it is difficult to balance corrosion resistance and wear resistance in seawater environments, and casting defects are prone to occur in the manufacture of large-diameter components.
By adjusting the constituent elements of the aluminum bronze alloy to ensure the content range of Al, Ni, Fe, and Si, a structure composed of α phase, coarse Fe-Si intermetallic compounds, and fine κ phase is formed to suppress the precipitation of β phase and improve the metal corrosion resistance and hardness, and avoid adding Sn during the manufacturing process to reduce casting defects.
It achieves the high load resistance, wear resistance and corrosion resistance of aluminum bronze alloy, ensures the long-term stable performance and manufacturing stability of sliding parts in seawater environment, and reduces the occurrence of casting defects.
Smart Images

Figure CN118765336A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an aluminum bronze alloy and to a sliding part using the alloy. Background Art
[0002] Practical aluminum bronze alloys are classified into four types, CAC701 to CAC704, in the Japanese Industrial Standards (JIS), and are composed of 7 to 10% by weight of aluminum (Al), 0.5 to 4.5% by weight of nickel (Ni), 0.5 to 5% by weight of iron (Fe), 0.1 to 2% by weight of manganese (Mn), and the balance of copper (Cu) and inevitable impurities relative to the total weight of the aluminum bronze alloy. From the perspective of chemical properties and mechanical properties such as corrosion resistance, seawater resistance, and wear resistance, the aluminum bronze alloy is often used for industrial purposes such as chemical industry parts, ship parts, and mechanical parts. In particular, aluminum bronze alloys represented by CAC703, which is composed of 8.5 to 10.5% by weight of Al, 3 to 6% by weight of Ni, 3 to 6% by weight of Fe, 0.1 to 1.5% by weight of Mn, and the balance of Cu and inevitable impurities, have excellent corrosion resistance and are used as seawater bearings.
[0003] Patent Document 1 discloses an aluminum bronze alloy having excellent acid corrosion resistance. The aluminum bronze alloy disclosed in Patent Document 1 is composed of 3 to 12 weight % of Al, 4 to 7 weight % of Ni, 3 to 6 weight % of Fe, 0.3 to 5.0 weight % of silicon (Si), and the balance of copper (Cu) and inevitable impurities. The aluminum bronze alloy disclosed in Patent Document 1 is mainly used for parts of acid cleaning devices because of its excellent acid corrosion resistance.
[0004] Patent Document 2 discloses an aluminum bronze alloy for synchronizer locking rings having excellent wear resistance. The aluminum bronze alloy disclosed in Patent Document 2 is composed of 7.5 to 9.5 weight % of Al, 7 to 11 weight % of Ni, 7.0 to 9.5 weight % of Fe, 1 to 4 weight % of Si, and the balance of copper (Cu) and inevitable impurities. The aluminum bronze alloy disclosed in Patent Document 2 has excellent wear resistance and a large friction coefficient, and is therefore suitable for synchronizer locking ring components.
[0005] In addition, it is known that the sliding property can be improved by adding tin (Sn) to the existing aluminum bronze alloy. The aluminum bronze alloy to which Sn is added has excellent corrosion resistance and is therefore used for bearing bushings, sliding seats, worm gears, or bearings for turbochargers (for example, see Patent Document 3).
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 51-47519
[0009] Patent Document 2: European Patent Application Publication No. 1279749
[0010] Patent Document 3: Japanese Patent Application No. 2017-515974 Summary of the invention
[0011] Problems to be solved by the invention
[0012] However, conventional aluminum bronze alloys (especially CAC703, which has excellent corrosion resistance) have the following problems: they cannot have both high load resistance and wear resistance in seawater areas. When the aluminum bronze alloy described in Patent Document 1 is used, there is a problem with wear resistance, making it difficult to use it as a sliding part. In addition, when the aluminum bronze alloy described in Patent Document 2 is used, there is a problem with corrosion resistance, making it difficult to use it in seawater or chemically active environments.
[0013] In order to improve the high load resistance and wear resistance, it is possible to consider making the structure of aluminum bronze alloy harder. There is a β phase in the structure that is harder than other phases. If the β phase is precipitated in the structure, the aluminum bronze alloy will generally become harder. However, if the β phase in the aluminum bronze alloy increases, metal corrosion is likely to occur. Metal corrosion will occur significantly in water, especially seawater, and the functions of aluminum bronze alloy will be damaged over time.
[0014] In addition, the aluminum bronze alloy to which Sn is added described in Patent Document 3 has excellent sliding performance and wear resistance. However, the aluminum bronze alloy to which Sn is added has the problem of being easily damaged during metal processing, and in particular, casting defects may occur during centrifugal and sand casting of large-diameter parts, making stable production difficult.
[0015] Therefore, from the viewpoint of suppressing the precipitation of the β phase and making the structure (parent phase) of the aluminum bronze alloy harder, it is necessary to make a part of the structure harder by constituting a phase different from the β phase. In order to make a part of the structure harder, it is necessary to adjust the constituent elements of the aluminum bronze alloy and the amount of each constituent element. In addition, from the viewpoint of improving the stability during manufacturing, it is necessary to adjust the amount of Al and / or Ni without adding Sn.
[0016] In order to solve the above problems, the present invention aims to provide an aluminum bronze alloy which has excellent corrosion resistance (suppressing β phase precipitation) and wear resistance (ensuring that the metal has a certain hardness or more) and can be stably manufactured. In addition, the present invention aims to provide a sliding part using the aluminum bronze alloy which has corrosion resistance, wear resistance and stability during manufacturing.
[0017] Means for solving problems (1)
[0019] The aluminum bronze alloy of the present invention is composed of copper (Cu), aluminum (Al), nickel (Ni), iron (Fe), silicon (Si) and inevitable impurities, and is characterized in that:
[0020] The content of Al is 9.5 wt% or more and 10.5 wt% or less relative to the total weight,
[0021] The content of Ni is 6.0 wt% or more and 8.0 wt% or less relative to the total weight,
[0022] The content of Fe is 4.0 wt% or more and 6.0 wt% or less relative to the total weight,
[0023] The content of Si is 1.0 wt% or more and 2.0 wt% or less relative to the total weight,
[0024] The balance is Cu and unavoidable impurities.
[0025] The aluminum bronze alloy has a structure consisting of an α phase, a coarse Fe-Si intermetallic compound having a length of 1 μm or more in the short-side direction, a fine κ phase having a length of less than 1 μm in the short-side direction different from the Fe-Si intermetallic compound, and a trace amount of inevitable phases.
[0026] The area ratio of the metal cross section of the coarse Fe-Si intermetallic compound to the entire structure is 4% or more and 14% or less,
[0027] The fine κ phase is dispersed in the entire structure in the form of dots and / or lines.
[0028] According to the aluminum bronze alloy having this structure, the precipitation of the β phase is suppressed, so the corrosion resistance of the metal can be improved. In addition, the coarse Fe-Si intermetallic compounds are precipitated in a certain proportion in the structure, and the fine κ phase different from the Fe-Si intermetallic compounds is dispersed in the entire structure in a dot-like and / or linear shape, so that the hardness of the metal can be ensured. Therefore, the high load resistance and wear resistance when used as a sliding part can be improved. In addition, since Sn is not added, defects during manufacturing can be reduced and stable manufacturing can be performed. (2)
[0030] In addition, in the aluminum bronze alloy of the present invention, it is preferred that
[0031] The content of Al is 9.5 wt% or more and 10.5 wt% or less relative to the total weight,
[0032] The content of Ni relative to the total weight is more than 7.0 wt % and less than 8.0 wt %,
[0033] The content of Fe is 4.0 wt% or more and 6.0 wt% or less relative to the total weight,
[0034] The content of Si is 1.0 wt% or more and 2.0 wt% or less relative to the total weight,
[0035] The balance is Cu and inevitable impurities.
[0036] According to the aluminum bronze alloy having this structure, the precipitation of the β phase is further suppressed compared with the aluminum bronze alloy described in (1), so the corrosion resistance of the metal is further improved. In addition, compared with the aluminum bronze alloy described in (1), the fine κ phase other than the coarse Fe-Si system intermetallic compound in the structure increases, and the hardness of the structure is improved. Therefore, when used as a sliding part, the high load resistance and wear resistance of the sliding part can be improved. (3)
[0038] In addition, in the aluminum bronze alloy of the present invention, it is preferable that the Rockwell hardness is HRC17 or higher.
[0039] The aluminum bronze alloy having this structure has a Rockwell hardness of HRC17 or more, showing excellent wear resistance, so that the function of the parts using the alloy can be maintained for a long time. In addition, when used as a sliding part, the high load resistance and wear resistance of the sliding part are improved. (4)
[0041] In the aluminum bronze alloy of the present invention, it is preferred that the maximum dealumination corrosion depth based on the corrosion test method in accordance with ISO6509-1981 is 120 μm or less.
[0042] According to the aluminum bronze alloy having such a structure, the maximum dealumination corrosion depth is 120 μm or less, so the metal is not easily corroded, and the corrosion resistance is improved. Therefore, even in an environment such as seawater that is chemically active for metals, the aluminum bronze alloy having such a structure can maintain the performance of the aluminum bronze alloy for a long time. (5)
[0044] The sliding surface of the sliding part of the present invention is a sliding part formed of the aluminum bronze alloy described in any one of (1) to (4).
[0045] According to the sliding component having such a configuration, since the sliding surface is formed of the aluminum bronze alloy having excellent corrosion resistance and wear resistance, the sliding performance of the sliding component can be maintained for a long period of time. (6)
[0047] In the sliding component of the present invention, it is preferable that a plurality of holes, grooves or recessed portions are formed on the sliding surface, and a solid lubricant is embedded and fixed in the holes, grooves or recessed portions.
[0048] According to the sliding component having such a configuration, since the solid lubricant is embedded and fixed in a part of the sliding surface, the wear resistance of the sliding component is further improved by utilizing the excellent corrosion resistance and wear resistance of the aluminum bronze alloy and the low friction of the solid lubricant. (7)
[0050] Furthermore, in the sliding component of the present invention, it is preferable that a part or the entirety of the sliding component is used in seawater.
[0051] According to the sliding component having such a configuration, since the sliding surface is formed of an aluminum bronze alloy having excellent corrosion resistance and wear resistance, wear and corrosion can be suppressed for a long period of time and the sliding performance of the sliding component can be maintained even when the sliding component is used in seawater.
[0052] Brief description of the attached figure
[0053] Figure 1 This is a schematic diagram showing a sliding member according to the present invention.
[0054] Figure 2 This is an optical microscope photograph showing the microstructure of the aluminum bronze alloy corresponding to Example 2 of the present invention.
[0055] Figure 3 This is an optical microscope photograph showing the microstructure of an aluminum bronze alloy corresponding to Comparative Example 1 which is different from the example of the present invention.
[0056] Figure 4 This is an optical microscope photograph showing the microstructure of an aluminum bronze alloy corresponding to Comparative Example 4 which is different from the examples of the present invention.
[0057] Figure 5 This is a graph showing the relationship between the area ratio of the Fe—Si based intermetallic compound in the aluminum bronze alloy of the present invention and the bearing wear amount and friction coefficient.
[0058] Figure 6 This is a graph showing the relationship between the Rockwell hardness of the aluminum bronze alloy of the present invention, the bearing wear amount, and the friction coefficient. DETAILED DESCRIPTION
[0059] The following is a description of embodiments of the present invention, which will be described with reference to the accompanying drawings.
[0060] The sliding component as one embodiment of the present invention is any sliding component such as a bearing, a shaft, a slider, a slider bracket, a gear or a washer, or a combination of these sliding components. Figure 1As shown in the figure, as a sliding member of one embodiment of the present invention, a sliding bearing 11 formed in a substantially cylindrical shape is described. A substantially cylindrical shaft 12 having a diameter substantially the same as the inner diameter thereof is coaxially inserted inside the sliding bearing 11. The shaft 12 and / or the sliding bearing 11 perform horizontal motion in the axial direction, rotational motion around the axial direction, or swinging motion.
[0061] As described later, at least a portion of the inner side surface (sliding surface of the sliding part) of the sliding bearing 11 is formed by an aluminum bronze alloy as one embodiment of the present invention by a prescribed method. The entire inner side surface of the sliding bearing 11 may be formed by an aluminum bronze alloy, or the inner side surface of the sliding bearing 11 in the circumferential direction and / or the axial direction may be partially formed with an aluminum bronze alloy. The entire sliding bearing 11 may be formed by an aluminum bronze alloy, or an aluminum bronze alloy layer may be formed on the inner side of a cylindrical part formed by a metal material or a non-metallic material. In addition, solid lubricants such as graphite, resin, and lead and / or lubricants such as lubricating oil or grease may be added according to the required sliding performance. In addition, the shaft 12 uses a prescribed metal material or non-metal material. In one embodiment of the present invention, SUS630 is used, but it is not limited to this. A prescribed metal material or non-metal material may also be used according to the required sliding performance and use conditions such as material strength and corrosion resistance.
[0062] In one embodiment of the present invention, the sliding bearing 11 is exemplified as a sliding component, but the present invention is not limited thereto. At least a portion of the outer side surface (sliding surface) of the shaft 12 is formed of an aluminum bronze alloy, and the shaft 12 can also constitute the sliding component of the present invention. In addition, at least a portion of the outer side surface of the shaft 12 and at least a portion of the inner side surface of the sliding bearing 11 can also be formed of an aluminum bronze alloy.
[0063] Although the sliding component of one embodiment of the present invention is illustrated in the shape of a sliding bearing, the sliding component of the present invention is not limited thereto. As described above, the sliding component of the present invention may be any sliding component such as a bearing, a shaft, a slider, a slider bracket, a gear or a washer, a part of or the entire sliding surface of which is formed by the aluminum bronze alloy described later, or a combination of these sliding components. For example, in the case where the sliding component is a washer, the entirety of the washer or a part or the entirety of the sliding surface (contact surface) of the washer is formed by the aluminum bronze alloy of the present invention. In addition, for example, in the case where the sliding component is a slider or a slider bracket, the sliding component is formed in a roughly plate-like shape. In this case, the roughly plate-like sliding component may be entirely made of an aluminum bronze alloy, or only one surface, i.e., the sliding surface, of the roughly plate-like sliding component may be formed of an aluminum bronze alloy.
[0064] A plurality of holes, grooves or recesses are formed on the sliding surface of the sliding bearing 11, which is a sliding component of one embodiment of the present invention, and a solid lubricant composed of graphite or wax is embedded and fixed in the holes, grooves or recesses. By having this structure, the sliding performance of the sliding component can be improved, but this structure can also be omitted according to the required sliding performance. A plurality of holes, grooves or recesses are formed by drilling or cutting using a drill or end mill, but the plurality of holes, grooves or recesses can also be formed by other means. At this time, the shape, size, area ratio of the plurality of holes, grooves or recesses relative to the entire sliding surface and the fixing position can be arbitrarily selected according to the required sliding performance or purpose. For example, the shape, size, area ratio and fixing position of the plurality of holes, grooves or recesses can be selected according to the method shown in Japanese Patent No. 5616032, or can be selected within a range that is obvious to those skilled in the art.
[0065] As described later, the sliding bearing 11 as a sliding component of one embodiment of the present invention has excellent corrosion resistance and can be used in various environments. In particular, the sliding component as one embodiment of the present invention can be used in seawater. However, the sliding component of the present invention is not limited to use in seawater, and can also be used in environments other than seawater. For example, the sliding component of the present invention can also be used in a high temperature environment.
[0066] The aluminum bronze alloy constituting at least a part of the sliding surface of the sliding part as one embodiment of the present invention is composed of Cu, Al, Ni, Fe, Si and inevitable impurities, wherein the content of Al is 9.5 wt% or more and 10.5 wt% or less relative to the total weight, the content of Ni is 6.0 wt% or more and 8.0 wt% or less relative to the total weight, the content of Fe is 4.0 wt% or more and 6.0 wt% or less relative to the total weight, the content of Si is 1.0 wt% or more and 2.0 wt% or less relative to the total weight, and the balance is Cu and inevitable impurities. In addition, the aluminum bronze alloy has a structure composed of an α phase, a coarse Fe-Si system intermetallic compound having a length of 1 μm or more in the short side direction, a fine κ phase having a length of less than 1 μm in the short side direction different from the Fe-Si system intermetallic compound, and a trace amount of inevitable phase, wherein the area ratio of the metal cross section of the coarse Fe-Si system intermetallic compound to the entire structure is 4% or more and 14% or less, and the fine κ phase is formed in a dot-like and / or linear shape and dispersed in the entire structure.
[0067] In the aluminum bronze alloy constituting at least a part of the sliding surface of the sliding part as one embodiment of the present invention, the above-mentioned range of Fe and Si is added to the alloy composition, and Ni and Al are adjusted in the above-mentioned range of amounts so that coarse Fe-Si intermetallic compounds are precipitated within the above-mentioned range, thereby achieving excellent wear resistance. At this time, it is preferred to have a Rockwell hardness of HRC17 or above, but it is not limited thereto, and the specified hardness can also be selected according to the sliding performance and use conditions. In addition, in the aluminum bronze alloy constituting at least a part of the sliding surface of the sliding part as one embodiment of the present invention, the above-mentioned range of Al and Ni is added to the alloy composition, further suppressing the precipitation of the β phase and improving the corrosion resistance of the metal. At this time, the maximum dealuminization corrosion depth based on the corrosion test method according to ISO6509-1981 is preferably 120μm or less.
[0068] The method for manufacturing the aluminum bronze alloy constituting at least a part of the sliding surface of the sliding component as one embodiment of the present invention is not particularly limited, but it is preferred that the master alloy of molten copper, Al Schottky, Fe50Al, Cu30Ni, and Cu15Si is measured in a manner to have a desired mass, melted in a high-frequency melting furnace, and cast by continuous casting, centrifugal casting, sand casting, etc.
[0069] In the aluminum bronze alloy constituting at least a part of the sliding surface of the sliding part as one embodiment of the present invention, the pure metal material and alloy material as the material are molten copper, Al Schottky, Fe50Al, Cu30Ni, Cu15Si, but not limited thereto. The prescribed pure metal material and alloy material are measured and used so that the content of Al relative to the total weight is 9.5 weight % or more and 10.5 weight % or less, Ni is 6.0 weight % or more and 8.0 weight % or less, Fe is 4.0 weight % or more and 6.0 weight % or less, Si is 1.0 weight % or more and 2.0 weight % or less, and the balance is composed of Cu and unavoidable impurities. For example, Fe, Ni, Si, Cu-50Fe, etc. can be used as the pure metal material and alloy material.
[0070] The manufacturing method of the aluminum bronze alloy constituting at least a part of the sliding surface of the sliding part as one embodiment of the present invention is a method of melting using a muffle furnace and casting using a predetermined mold, but is not limited thereto. A high-frequency melting furnace or the like can be used as a melting method. In addition, continuous casting, centrifugal casting, sand casting, etc. can be used as a casting method. In order to manufacture the required sliding parts, these methods are selected within a range that is obvious to those skilled in the art. The melting temperature is not particularly limited, and it is preferred to use a temperature that allows the pure metal material and the alloy material used to melt respectively.
[0071] When the aluminum bronze alloy constituting at least a part of the sliding surface of the sliding component as one embodiment of the present invention is processed into the above-mentioned sliding component, the sliding component can be formed using a mold or sand mold used to manufacture the sliding component during casting, but is not limited to this. It is also possible to use a metal mold or sand mold of any shape during casting to manufacture an aluminum bronze alloy of any shape, and then perform processing such as bending, grinding and / or grinding to form the sliding component.
[0072] It should be noted that the present invention is not limited to the above-mentioned embodiments, and a person skilled in the art having general knowledge in the art can make modifications or improvements within the technical concept of the present invention.
[0073] Example
[0074] The embodiments of the present invention are further described in detail below in conjunction with the test results.
[0075] In order to produce aluminum bronze alloys having the compositions shown in Table 1, nugget copper, Al Schottky, Fe50Al, Cu30Ni, and Cu15Si were weighed so as to form the composition ratios shown in Table 1, melted at 1200°C to 1250°C, and cast into a mold to prepare samples. When melting the aluminum bronze alloys of the present embodiment and the comparative example, flux was added to the molten metal, and the metal oxides were removed before casting in the mold. The weights of the samples were 300 g and 3500 g. The maximum dealumination corrosion depth of the 300 g sample was measured and the metal structure was observed. The Rockwell hardness (HRC) and sliding performance of the 3500 g sample were measured.
[0076] [Table 1]
[0077]
[0078] The description "(*)" on the edge of a numerical value means that it is out of the numerical range of the present invention.
[0079] Table 2 is a table showing the area ratio of the Fe-Si intermetallic compound relative to the whole in the cross-sectional view of the microstructure of the aluminum bronze alloy of the present embodiment and the comparative example. The area ratio of the Fe-Si intermetallic compound in the cross-sectional view is calculated as follows. Using a scanning electron microscope (SEM), the contrast is adjusted in such a way that the Fe-Si intermetallic compound is clearly displayed, and a portion of the whole cross section of the reflected electron image (COMP image) of each aluminum bronze alloy is photographed at a magnification of 500 times. At this time, any five parts are selected as the photographing parts relative to the whole cross section. Using image analysis software (WinROOF: manufactured by Mitani Shoji Co., Ltd.), the area ratio of the Fe-Si intermetallic compound in the five reflected electron images (cross-sectional views) of each aluminum bronze alloy is measured. The arithmetic mean of the five area ratios is shown in Table 2.
[0080] [Table 2]
[0081]
[0082] The "(*)" beside a numerical value means that it is out of the numerical range of the present invention.
[0083] Table 3 is a table showing the results of the maximum dealumination corrosion depth. Corrosion resistance can be compared based on the results of the maximum dealumination corrosion depth. Here, the maximum dealumination corrosion depth is measured based on the corrosion test method based on IS06509-1981.
[0084] [Table 3]
[0085]
[0086] The description of the numerical value edge (*)" means that it is out of the numerical range of the present invention.
[0087] As can be seen from the results in Table 3, the maximum dealumination corrosion depth and the average dealumination corrosion depth of the aluminum bronze alloys of the present embodiment (Examples 1 to 5) are respectively smaller than the maximum dealumination corrosion depth and the average dealumination corrosion depth of the aluminum bronze alloys of the comparative examples (Comparative Examples 4 to 7). Therefore, the aluminum bronze alloys of the present embodiment (Examples 1 to 5) have excellent corrosion resistance.
[0088] Figure 2 to Figure 4 The optical microscope photographs respectively show the microstructures of the aluminum bronze alloys corresponding to Example 2, Comparative Example 1 and Comparative Example 4. It should be noted that the contrast of the photographs was adjusted for easier identification. Figure 2 As shown representatively, in each figure, the brighter area is the α phase in the aluminum bronze alloy. The α phase is usually a soft structure. When there is a lot of α phase, the wear resistance and high load resistance of the metal will be impaired. In addition, in each figure, the darker and roughly circular or elliptical area with a short side length of more than 1μm is a coarse Fe-Si intermetallic compound, and the darker and linear or dotted area with a short side length of less than 1μm is a fine κ phase different from the Fe-Si intermetallic compound.
[0089] like Figure 2As shown, in the aluminum bronze alloy obtained in Example 2, coarse Fe-Si intermetallic compounds are uniformly and dispersedly precipitated. In addition, fine κ phases different from Fe-Si intermetallic compounds are dispersed in the entire structure and constitute the parent phase together with the α phase. It can be assumed that there is a β phase in addition to the α phase in the parent phase, but since the dealuminization corrosion depth is small (the maximum dealuminization corrosion depth is less than 120μm), it can be seen that the β phase is not formed at all inside the α phase or the β phase exists only to a degree that does not impair the corrosion resistance. The hardness of the parent phase is maintained by precipitating fine κ phases and coarse Fe-Si intermetallic compounds in the parent phase, and coarse and hard areas are precipitated in the parent phase. As a result, the coarse intermetallic compounds are not easy to fall off during sliding, and excellent sliding performance is shown as described later. Although not shown in the figure, the same situation as Example 2 is also shown in Examples 1 and 3 to 5.
[0090] On the other hand, Figure 3 As shown in the figure, it can be seen that the coarse Fe-Si intermetallic compounds of 1 μm or more in the aluminum bronze alloy of Comparative Example 1 are larger than Figure 2 The amount of coarse Fe-Si intermetallic compounds is less in Example 5 shown. Although not shown in the figure, in Comparative Example 1 and Comparative Examples 2 to 3, the amount of coarse Fe-Si intermetallic compounds is also less. Since the amount of coarse Fe-Si intermetallic compounds is less and the α phase ratio is larger, the aluminum bronze alloys of Comparative Examples 1 to 3 are shown in Table 4 described later, and the harder intermetallic compounds are easily detached during sliding, so the sliding performance is greatly impaired. In addition, the hardness (Rockwell hardness) is also lower than that of Examples 1 to 5, and the wear resistance and high load resistance when used as sliding parts are reduced.
[0091] In addition, if Figure 4 As shown in Table 2, the coarse Fe-Si intermetallic compounds in the aluminum bronze alloy of Comparative Example 4 are uniformly and dispersedly precipitated. Although not shown in the figure, the same morphology is confirmed in Comparative Examples 5 to 7. On the other hand, the aluminum bronze alloys of Comparative Examples 3 to 6 have a large dealumination corrosion depth (more than 120 μm), so it can be assumed that β phase is formed in the parent phase. Due to the significant formation of β phase, as shown in Table 2, the dealumination corrosion depth of the aluminum bronze alloys of Comparative Examples 4 to 7 is larger than that of Examples 1 to 5, the corrosion resistance is reduced, and the durability is reduced.
[0092] In order to measure the sliding performance of the sliding parts composed of the aluminum bronze alloy of this embodiment, a seawater journal test was carried out under the conditions shown in Table 4 below, and the friction coefficient, bearing wear and shaft wear at this time were measured. In addition, for comparison, the same test was carried out on Comparative Example 1 and Comparative Example 2. The sliding parts composed of the compositions of Examples 1 to 5 and Comparative Examples 1 and 2 respectively adopt the form of a sliding bearing 11 as described in one embodiment of the present invention. The sliding bearing 11 is formed into a roughly cylindrical shape. The sliding bearing 11 of this embodiment has an inner diameter of 60 mm, an outer diameter of 75 mm and a length of 30 mm. In addition, a solid lubricant is embedded in a part of the sliding surface of the sliding bearing 11 of this embodiment. As a solid lubricant, a PTFE-based solid lubricant SL464 (manufactured by Oiles Industries, Ltd.) is used.
[0093] [Table 4]
[0094]
[0095] like Figure 1 As shown in Table 4, the seawater journal test is as follows: in seawater, the shaft 12 is inserted into the sliding bearing 11, and a load in a direction perpendicular to the axis of the shaft 12 is applied to the sliding bearing 11 in such a way that the inner peripheral surface (sliding surface) of the sliding bearing 11 presses the outer peripheral surface of the shaft 12 at the surface pressure shown in Table 4, while the sliding bearing 11 is oscillated with the shaft 12 as the axis at the speed shown in Table 4. Based on the seawater journal test, the friction coefficient, bearing wear amount, and shaft wear amount of the sliding bearing 11 are measured.
[0096] Table 5 is a table showing the test results of the friction coefficient, bearing wear and mating shaft wear of the sliding bearing 11 made of aluminum bronze alloy in each embodiment and comparative example when the seawater journal test was performed under the conditions shown in Table 4. Furthermore, in order to investigate the load resistance as a sliding part, the Rockwell hardness (HRC) is shown in Table 5. The friction coefficient is the friction coefficient at the end of the seawater journal test, and the wear amount of the shaft 12 and the wear amount of the sliding bearing 11 are also the values at the end of the seawater journal test. In addition, at this time, in Example 3, in order to confirm the sliding performance under different lubrication conditions, the situation was distinguished according to the presence or absence of lubricant, and the sliding performance was confirmed. Grease was used as a lubricant.
[0097] [Table 5]
[0098]
[0099] The description "(*)" beside a numerical value means that it is out of the numerical range of the present invention.
[0100] The sliding bearing 11 composed of the aluminum bronze alloy of Examples 1 to 5 used in this embodiment has a friction coefficient of 0.13 or less at the end of the test, and is preferably used as a sliding part. In addition, the sliding bearing 11 composed of the aluminum bronze alloy of Examples 1 to 5 has a wear amount of 0.04 mm or less, and a Rockwell hardness of HRC17 or more, so it is excellent in high load resistance and wear resistance as a sliding part. On the other hand, according to Comparative Examples 1 to 3, as shown in Table 5, the friction coefficient at the end of the test is 0.16 or more, which is larger than that of Examples 1 to 5, and there are problems in sliding performance compared with Examples 1 to 5. In addition, according to Comparative Examples 1 to 3, the wear amount of the sliding bearing 11 at the end of the test exceeds 0.08 mm, and the Rockwell hardness is less than HRC17. The wear amount of the sliding bearing 11 is more than twice the wear amount measured in Examples 1 to 5, so Comparative Examples 1 to 3 have problems in high load resistance and wear resistance, and are difficult to be used as sliding parts. In Example 3, the sliding performance was confirmed under the condition of grease or not (see Table 5). The friction coefficient (0.13) of the sliding bearing 11 when the sliding bearing 11 was not coated with grease was less changed than the friction coefficient (0.11 or 0.12) of the sliding bearing 11 when the sliding bearing 11 was coated with grease. On the other hand, the wear amount (0.028 mm) of the sliding bearing 11 when the sliding bearing 11 was not coated with grease was larger than the wear amount (0.015 mm or 0.019 mm) of the sliding bearing 11 when the sliding bearing 11 was coated with grease, but was significantly smaller than the wear amount (0.124 mm and 0.087 mm) of the bearings of Comparative Examples 1 to 3. Therefore, the sliding parts made of the aluminum bronze alloy of the present invention have excellent sliding performance regardless of whether the lubricant is coated or not, and are therefore suitable for sliding parts in an environment where a large amount of lubricant cannot be used.
[0101] exist Figure 5The area ratio of Fe-Si intermetallic compounds to the whole structure is calculated by optical microscope photographs showing the microstructure of aluminum bronze alloys of Examples 1 to 5 and Comparative Examples 1 to 3, and the relationship between the area ratio and the friction coefficient and bearing wear obtained in Table 5 is shown. Here, the horizontal axis represents the area ratio of Fe-Si intermetallic compounds to the whole, the vertical axis on the left represents the bearing wear, and the vertical axis on the right represents the friction coefficient. In addition, the numbers surrounded by white circles represent the friction coefficient of the embodiment to which the numbers relate, the numbers surrounded by black circles represent the bearing wear of the embodiment to which the numbers relate, the numbers surrounded by white quadrilaterals represent the friction coefficient of the comparative example to which the numbers relate, and the numbers surrounded by black quadrilaterals represent the bearing wear of the comparative example to which the numbers relate. Generally, under high surface pressure, the real contact area increases and it is difficult to maintain the lubricating film, so the friction coefficient and bearing wear tend to increase. In order to prevent this influence, it is necessary to increase the area ratio of Fe-Si intermetallic compounds and reduce the real contact area. In particular, referring to Figure 5 , the area ratio of Fe-Si intermetallic compounds to the whole is 4% or more, so the effect of reducing the friction coefficient and the bearing wear is significant. When the area ratio of Fe-Si intermetallic compounds to the whole is less than 4%, the friction coefficient becomes high and the bearing wear also increases. On the other hand, when the Fe-Si intermetallic compounds exceed 14%, the wear of the mating shaft becomes significant and the sliding performance cannot be maintained for a long time. Moreover, the degree of freedom during processing is limited by the hardness. Therefore, in the aluminum bronze alloy of the present invention, the area ratio of Fe-Si intermetallic compounds is preferably in the range of 4% to 14%, and more preferably in the range of 4.7% to 13.2%.
[0102] Figure 6 It is a graph showing the relationship between the Rockwell hardness of the sliding bearing 11 composed of the aluminum bronze alloy of Examples 1 to 5 and Comparative Examples 1 to 3 (refer to Table 5) and the friction coefficient and bearing wear amount obtained in Table 5. Here, the horizontal axis represents the Rockwell hardness of the sliding bearing 11, the vertical axis on the left side represents the bearing wear amount, and the vertical axis on the right side represents the friction coefficient. In addition, the numbers surrounded by white circles represent the friction coefficient of the embodiments to which the numbers relate, the numbers surrounded by black circles represent the bearing wear amount of the embodiments to which the numbers relate, the numbers surrounded by white quadrilaterals represent the friction coefficient of the comparative examples to which the numbers relate, and the numbers surrounded by black quadrilaterals represent the bearing wear amount of the comparative examples to which the numbers relate. Generally, under high surface pressure, the actual contact area increases and it is difficult to maintain the lubricating film, so the friction coefficient and the bearing wear amount tend to increase. In order to prevent this influence, it is necessary to increase the area ratio of the Fe-Si system intermetallic compounds and reduce the actual contact area, and in order to prevent the Fe-Si system intermetallic compounds from falling off, it is necessary to increase the parent phase hardness. Refer to Figure 6 By making the Rockwell hardness HRC17 or more, the effect of reducing the friction coefficient and the bearing wear amount is significant. In particular, in Comparative Examples 1 to 3, the Rockwell hardness is less than HRC17, so the friction coefficient is maintained at a high level of 0.16, and the bearing wear amount is also 0.08 mm or more. Therefore, from the viewpoint of maintaining sliding performance, the Rockwell hardness of the aluminum bronze alloy of the present invention is preferably HRC17 or more, and more preferably HRC17.5 or more.
[0103] The present invention has been described above based on the embodiments. The aluminum bronze alloy according to the present invention has a smaller dealuminization corrosion depth than other aluminum bronze alloys, and therefore can maintain the properties of an aluminum bronze alloy and even the properties of a sliding part even in seawater or in a chemically active environment. In addition, the aluminum bronze alloy of the present invention has sufficient hardness and shows sufficient sliding performance in a seawater journal test. Therefore, the aluminum bronze alloy of the present invention is a preferred material for a sliding part having high load resistance and wear resistance.
[0104] Explanation of symbols
[0105] Sliding bearing 11; shaft 12.
Claims
1. An aluminum bronze alloy, characterized in that: It is composed of copper (Cu), aluminum (Al), nickel (Ni), iron (Fe), silicon (Si) and inevitable impurities. The content of Al relative to the total weight is 9.5 wt% or more and 10.5 wt% or less, The content of Ni is 6.0 wt% or more and 8.0 wt% or less relative to the total weight, The content of Fe is 4.0 wt% or more and 6.0 wt% or less relative to the total weight, The content of Si is 1.0 wt% or more and 2.0 wt% or less relative to the total weight, The balance is Cu and unavoidable impurities. The aluminum bronze alloy has a structure consisting of an α phase, a coarse Fe-Si intermetallic compound having a length of 1 μm or more in the short-side direction, a fine κ phase having a length of less than 1 μm in the short-side direction different from the Fe-Si intermetallic compound, and a trace amount of inevitable phases. The area ratio of the metal cross section of the coarse Fe-Si intermetallic compound to the entire structure is 4% or more and 14% or less, The fine κ phase is formed in a dot-like and / or line-like shape and is dispersed throughout the entire structure.
2. The aluminum bronze alloy according to claim 1, characterized in that The content of Al is 9.5 wt% or more and 10.5 wt% or less relative to the total weight, The content of Ni relative to the total weight is more than 7.0 wt% and less than 8.0 wt%, The content of Fe is 4.0 wt% or more and 6.0 wt% or less relative to the total weight, The content of Si is 1.0 wt% or more and 2.0 wt% or less relative to the total weight, The balance is Cu and inevitable impurities.
3. The aluminum bronze alloy according to claim 1 or 2, characterized in that: Rockwell hardness is HRC17 or above.
4. The aluminum bronze alloy according to any one of claims 1 to 3, characterized in that The maximum dealumination corrosion depth based on the corrosion test method in accordance with ISO6509-1981 is 120 μm or less.
5. A sliding component, characterized in that: The sliding surface is formed of the aluminum bronze alloy according to any one of claims 1 to 4.
6. The sliding component according to claim 5, characterized in that: A plurality of holes, grooves or recessed portions are formed on the sliding surface, and a solid lubricant is embedded and fixed in these holes, grooves or recessed portions.
7. The sliding component according to claim 5 or 6, characterized in that: A part or the whole of the sliding member is used in seawater.
Citation Information
Patent Citations
Aluminum bronze with high wear resistance
EP1279749A1
Aluminum-bronze alloys, methods of production, and products made from aluminum-bronze
JP2017515974A