Method for manufacturing protective film having metal silicide coating layer formed thereon, and protective film manufactured thereby
By using silicon precursors and metal precursors to form protective films of metal silicide coatings in the extreme ultraviolet (EUV) exposure process, the problems of insufficient transmittance and thermal emissivity of existing materials are solved, and efficient light source transmission and Improved heat resistance, suitable for high temperature environments.
Patent Information
- Application Number
- CN202380023938.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-14
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-11
AI Technical Summary
In the extreme ultraviolet (EUV) exposure process, the transmittance and thermal radiation rate of existing protective film materials are insufficient, resulting in serious light source loss and poor heat resistance, affecting the production efficiency and quality of semiconductor products.
Silicon precursors and metal precursors are used to form a metal silicide covering layer on the central layer, and the protective film is manufactured by atomic layer deposition (ALD) or chemical vapor deposition (CVD), combined with a protective layer to increase transmittance and thermal radiation rate. .
It achieves high transmittance and excellent thermal radiation rate of the protective film for extreme ultraviolet exposure, prolongs the service life of the film and improves the mechanical strength, and is suitable for high-temperature thermal shock environments.
Smart Images

Figure CN118765384A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a protective film for forming a metal silicide capping layer using a silicon precursor and a metal precursor, and a protective film for extreme ultraviolet (EUV) exposure manufactured based on the method. Background Art
[0002] In the exposure process, which is one of the main processes in semiconductor manufacturing, the wavelength of the light source is important in order to realize the mask circuit more finely and clearly. The smaller the wavelength, the higher the resolution, and the finer the circuit pattern can be drawn, and small semiconductor devices can be produced. In recent years, the light source used in the exposure process has developed to EUV (Extreme Ultraviolet) with a wavelength of 13.5nm.
[0003] In the exposure process using EUV light source, since the circuit of the mask is reduced and drawn on the wafer, if the mask is contaminated by impurities such as dust or foreign matter, the light is absorbed or reflected by such impurities, causing damage to the transferred pattern and significantly reducing the production yield of semiconductor products. In order to prevent impurities from adhering to the surface of the mask, a thin film called a pellicle is covered on the mask for protection. Such a pellicle is indispensable in terms of yield and also serves to extend the life of the mask, so its necessity is increasing.
[0004] In the EUV (Extreme Ultraviolet) process, the light source passes through the protective film twice. Therefore, in order to reduce the loss of the light source passing through the protective film, a protective film material with a transmittance of more than 90% is required, and a lot of research is currently underway. In addition, when the EUV light source passes through the protective film, it is instantly heated to 600-1200°C and then cooled to room temperature, so a material with sufficient thermal emissivity must be used to withstand such thermal shock. Therefore, it is necessary to study protective films with better transmittance and thermal emissivity. Summary of the invention
[0005] The object of the present invention is to provide a method for manufacturing a protective film for extreme ultraviolet (EUV) exposure, wherein the method uses a silicon precursor and a metal precursor to form a metal silicide capping layer on a central layer.
[0006] Another object of the present invention is to provide a protective film including a metal silicide cap layer manufactured by the above-mentioned manufacturing method and showing excellent transmittance and thermal emissivity.
[0007] The present invention provides a method for manufacturing a protective film, comprising the step of forming a metal silicide capping layer on a central layer using a silicon precursor and a metal precursor represented by the following chemical formula 1.
[0008] [Chemical formula 1]
[0009] S H n X 4-n
[0010] [In the above chemical formula 1,
[0011] X is a halogen;
[0012] n is an integer from 1 to 3.]
[0013] The above-mentioned core layer can be Si, SiN x 、SiC x or a mixed film thereof, which may be a layer of Si material and SiN x The material layer is a 2-layer membrane structure.
[0014] According to an embodiment of the present invention, the protective film may have one or more protective layers between the layer where the central layer and the cover layer are bonded, below the central layer, or at these locations simultaneously. The protective layer is selected from B x N, B, Zr, Zn, B x C. SiC x or SiN x It is composed of one or two or more substances.
[0015] In one embodiment, the metal of the metal precursor may be Mo, Ni, Ru, Pt, Cu, Ti, Zr, Nb, Hf, Ta, W or Cr, and the molar ratio of the metal:silicon of the silicon precursor and the metal precursor may be 1:0.2 to 6.
[0016] According to another embodiment, the formation of the metal silicide capping layer may be performed by atomic layer deposition (ALD) or chemical vapor deposition (CVD).
[0017] According to one embodiment of the present invention, the formation of the metal silicide capping layer is as follows:
[0018] The following steps may be included:
[0019] a) step of heating the core layer installed in the chamber;
[0020] b) a step of allowing a silicon precursor and a metal precursor to be adsorbed on the central layer; and
[0021] c) A step of injecting a reaction gas into the core layer on which the silicon precursor and the metal precursor are adsorbed to produce a metal silicide capping layer.
[0022] The above-mentioned reaction gas can be any one or more selected from oxygen (O2), ozone (O3), distilled water (H2O), hydrogen peroxide (H2O2), nitric oxide (NO), nitrous oxide (N2O), nitrogen dioxide (NO2), ammonia (NH3), nitrogen (N2), hydrazine (N2H4), amines, diamines, carbon monoxide (CO), carbon dioxide (CO2), C1 to C12 saturated or unsaturated hydrocarbons, hydrogen (H2), argon (Ar) and helium (He).
[0023] The present invention provides a protective film, comprising a core layer and a metal silicide capping layer, wherein the metal silicide capping layer is manufactured on the core layer using a silicon precursor and a metal precursor represented by the following chemical formula 1.
[0024] [Chemical formula 1]
[0025] S H n X 4-n
[0026] [In the above chemical formula 1,
[0027] X is a halogen;
[0028] n is an integer from 1 to 3.]
[0029] In one embodiment, the molar ratio of metal to silicon in the metal silicide capping layer may be 1:0.2-6.
[0030] The present invention provides a method for manufacturing a protective film for extreme ultraviolet (EUV) exposure that forms a metal silicide capping layer using a silicon precursor and a metal precursor, and a protective film manufactured by the above-mentioned manufacturing method, wherein the above-mentioned protective film exhibits excellent performance in transmittance and thermal emissivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A schematic diagram showing the structure and manufacturing process of the protective film of the present invention.
[0032] Figure 2 FIG. 4 is a graph showing the deposition rate of the metal silicide capping layer according to Example 1 of the present invention.
[0033] Figure 3 FIG. 4 is a graph showing the molar ratio of metal to silicon in the metal silicide capping layer according to Example 1 of the present invention. DETAILED DESCRIPTION
[0034] The present invention provides a method for manufacturing a protective film for extreme ultraviolet exposure including a metal silicide capping layer manufactured using a silicon precursor and a metal precursor, and a protective film manufactured based on the method.
[0035] The singular form used in the present invention is intended to include the plural form as well, unless otherwise indicated in the context.
[0036] In addition, the numerical range used in the present invention includes the lower limit value and the upper limit value and all values within the range, the increment theoretically induced from the form and amplitude of the defined range, all values defined therein, and all possible combinations of the upper and lower limits of the numerical range defined in different forms. In the specification of the present invention, unless otherwise specified, values outside the numerical range that may be generated due to experimental errors or rounding of numerical values are also included in the defined numerical range.
[0037] The term “comprising / including” described in the present invention is an open-ended term having an equivalent meaning to expressions such as “having”, “containing”, “having” or “characterized by” and does not exclude elements, materials or processes not further listed.
[0038] The "halogen" described in the present invention means fluorine, chlorine, bromine or iodine.
[0039] The present invention will be described in more detail below. At this time, the technical terms and scientific terms used, if not otherwise defined, have the meanings commonly understood by those skilled in the art to which the present invention belongs, and in the following description, the description of the known functions and structures that may unnecessarily confuse the gist of the present invention is omitted.
[0040] The present invention provides a method for manufacturing a protective film, comprising the step of forming a metal silicide capping layer on a central layer using a silicon precursor and a metal precursor represented by the following chemical formula 1.
[0041] [Chemical formula 1]
[0042] S H n X 4-n
[0043] [In the above chemical formula 1,
[0044] X is a halogen;
[0045] n is an integer from 1 to 3.]
[0046] The above-mentioned core layer can be Si, SiN x 、SiC x or a mixed film thereof, which may be a layer of Si material and SiN x The material layer is a 2-layer membrane structure.
[0047] like Figure 1As shown in the schematic diagram of FIG. 1 , the protective film may include a core layer, a cover layer, and a protective layer. The protective film has a transmittance of more than 85% with respect to the exposed ultraviolet light, and a reflectivity preferably within 0.04%.
[0048] The Si constituting the core layer may be formed of silicon in one or more states including single crystal, polycrystalline and amorphous. x Compared with Si material, the material has higher mechanical strength and chemical stability. x material, thereby ensuring the mechanical strength and chemical stability of the center layer.
[0049] The core layer preferably has a transmittance of 85% or more to the exposed ultraviolet light. In addition, the cover layer can be formed with various thicknesses in consideration of the mechanical strength and optical properties of the protective film. Preferably, the cover layer can be formed with a thickness that minimizes the reflectivity of the exposed ultraviolet light to the protective film.
[0050] Preferably, the silicon precursor forming the above-mentioned capping layer may be SiH2X2 or SiHX3, more specifically, may be SiH2X2. Specifically, X in the chemical formula 1 representing the above-mentioned silicon precursor may be chlorine, bromine or iodine, more specifically, X in the above-mentioned chemical formula 1 may be chlorine or iodine, but is not limited thereto.
[0051] The metal silicide covering layer manufactured by the above-mentioned manufacturing method according to one embodiment of the present invention is manufactured into a uniform thin film with a certain component ratio according to the purpose, which improves the thermal and mechanical durability. It is a material with excellent light transmittance and thermal emissivity, and is very suitable as a protective film for extreme ultraviolet exposure.
[0052] According to an embodiment of the present invention, the protective film may have one or more protective layers between the layers where the central layer and the cover layer meet, below the central layer, or at these locations simultaneously. The protective layer is selected from B x N, B, Zr, Zn, B x C. SiC x or SiN x It is composed of one or two or more substances.
[0053] The protective layer can play a protective function against chemical reactions occurring in the extreme ultraviolet lithography environment. In the environment where the protective film is used, there are a large number of hydrogen free radicals, which can react with the cover layer to reduce the function of the cover layer. Therefore, the protective layer can protect the cover layer from contact with hydrogen free radicals and can also enhance the mechanical strength of the protective film.
[0054] According to one embodiment of the present invention, the metal of the above-mentioned metal precursor may be Mo, Ni, Ru, Pt, Cu, Ti, Zr, Nb, Hf, Ta, W or Cr. Specifically, it may be Mo, Ni, Ti, Zr, Nb, Hf or W. More specifically, it may be Mo, Ti or W. The above-mentioned metal precursor may be a metal halide, but is not limited thereto.
[0055] According to an embodiment of the present invention, the molar ratio of metal:silicon in the silicon precursor and the metal precursor may be 1:0.2 to 6, preferably 1:0.5 to 5.0, and more preferably 1:1.0 to 3.0.
[0056] In one embodiment of the present invention, the method for forming the above-mentioned metal silicide covering layer can be a conventional method used in the present technical field, specifically, it can be atomic layer deposition (ALD), chemical vapor deposition (CVD), metal organic chemical vapor deposition (MOCVD), low pressure chemical vapor deposition (LPCVD), plasma enhanced chemical vapor deposition (PECVD) or plasma enhanced atomic layer deposition (PEALD). Preferably, it can be implemented by atomic layer deposition (ALD) or chemical vapor deposition (CVD), and more preferably, it can be atomic layer deposition (ALD).
[0057] According to one embodiment of the present invention, the method for forming the above-mentioned metal silicide covering layer may include the following steps: a) a step of heating a central layer installed in a chamber; b) a step of adsorbing a silicon precursor and a metal precursor on the above-mentioned central layer; and c) a step of injecting a reaction gas into the central layer adsorbing the above-mentioned silicon precursor and the metal precursor to manufacture the metal silicide covering layer.
[0058] According to another embodiment, the method for forming the metal silicide capping layer may further include a step of purifying with a conveying gas after step b) and step c), and the steps b) to c) may be repeated as a cycle.
[0059] In one embodiment, the conditions of the above-mentioned formation method can be adjusted according to the structure or thermal characteristics of the target covering layer, and examples thereof include the silicon precursor input flow rate, the metal precursor input flow rate, the reaction gas and the transport gas input flow rate, the pressure, the RF power, etc.
[0060] As a non-limiting example of such conditions, the input flow rate of the silicon precursor and the metal precursor may be adjusted within the range of 1 to 1000 sccm, the transport gas within the range of 1 to 5000 sccm, the flow rate of the reaction gas within the range of 10 to 5000 sccm, the pressure within the range of 0.1 to 10 torr, and the RF power within the range of 10 to 1000 W, but it is not limited to these.
[0061] In one embodiment, the temperature of heating the central layer installed in the chamber in the above step a) may be 200° C. to 700° C., specifically, 300° C. to 500° C., but is not limited thereto.
[0062] The above-mentioned reaction gas can be any one or more selected from oxygen (O2), ozone (O3), distilled water (H2O), hydrogen peroxide (H2O2), nitric oxide (NO), nitrous oxide (N2O), nitrogen dioxide (NO2), ammonia (NH3), nitrogen (N2), hydrazine (N2H4), amines, diamines, carbon monoxide (CO), carbon dioxide (CO2), C1 to C12 saturated or unsaturated hydrocarbons, hydrogen (H2), argon (Ar) and helium (He).
[0063] Specifically, the above-mentioned reaction gas can be any one or more selected from oxygen (O2), hydrogen peroxide (H2O2), nitrous oxide (N2O), ammonia (NH3), nitrogen (N2) and hydrogen (H2). More specifically, it can be any one or more selected from nitrous oxide (N2O), ammonia (NH3) or nitrogen (N2), but is not limited to this.
[0064] In one embodiment, the transport gas is an inert gas, which may be any one or more selected from argon (Ar), helium (He) and nitrogen (N2). Specifically, it may be argon (Ar), but is not limited thereto.
[0065] In one embodiment, after the transport gas and the silicon precursor are injected into the chamber, a purge step of removing the unabsorbed silicon precursor using the transport gas may be performed. Next, after the transport gas and the metal precursor are injected into the chamber, a purge step of removing the unabsorbed metal precursor using the transport gas may be performed.
[0066] In one embodiment, after the reaction gas is injected into the chamber, a purge step may be performed to remove reaction byproducts and residual reaction gas using the transport gas.
[0067] In one embodiment, the above-mentioned steps of injecting the silicon precursor, purging, injecting the metal precursor, purging, injecting the reaction gas, and purging may be repeated as one cycle.
[0068] According to one embodiment of the present invention, the growth thickness of the cover layer can be 1 to 100 mm / s per cycle of the above process. Specifically, it can be 1.3 to More specifically, it can be 1.6 to
[0069] The present invention provides a protective film, which includes a core layer and a metal silicide capping layer, wherein the metal silicide capping layer is manufactured on the core layer using a silicon precursor represented by the following chemical formula 1 and a metal precursor.
[0070] [Chemical formula 1]
[0071] S H n X 4-n
[0072] [In the above chemical formula 1,
[0073] X is a halogen;
[0074] n is an integer from 1 to 3.]
[0075] In one embodiment, the central layer may be a layer of Si material and SiN x The two-layer film structure of the material layer, the molar ratio of metal:silicon in the above-mentioned metal silicide covering layer can be 1:0.2 to 6, preferably, it can be 1:0.5 to 5.0, and more preferably, it can be 1:1.0 to 3.0.
[0076] According to an embodiment of the present invention, the pellicle including a metal silicide capping layer in the central layer using a silicon precursor and a metal precursor has significantly improved transmittance and thermal emissivity, and can be used as a more excellent pellicle for extreme ultraviolet exposure.
[0077] Next, the method for manufacturing a pellicle using a silicon precursor and a metal precursor to form a metal silicide capping layer according to the present invention and the pellicle for extreme ultraviolet exposure manufactured thereby will be described in more detail through specific examples.
[0078] However, the following embodiments are only a reference for describing the present invention in detail, and the present invention is not limited thereto and can be implemented in various forms. In addition, the terms used for explanation in the present invention are only used to effectively describe specific embodiments and are not intended to limit the present invention.
[0079] [Example 1]
[0080] A molybdenum silicide capping layer is formed by atomic layer deposition.
[0081] A silicon wafer formed of silicon nitride to be covered with a molybdenum silicide layer was transferred into a deposition chamber and maintained at 450° C. Diiodosilane (SiH2I2) filled in a stainless steel container and argon gas (50 sccm) as a delivery gas were transferred for 1 to 7 seconds for adsorption, and then unreacted compounds were removed for 3 seconds using 2000 sccm of argon gas.
[0082] Then, the molybdenum pentachloride (MoCl5) filled in the stainless steel container and the argon gas as the transport gas were transferred at 50 sccm for 1 second for adsorption, and then the unreacted compound was removed by 2000 sccm of argon for 3 seconds. Then, a molybdenum silicide cover layer was formed by 2000 sccm of hydrogen and 100 W of plasma. Finally, the unreacted compound was removed by 2000 sccm of argon for 3 seconds. The above-mentioned process was regarded as one cycle and repeated for 200 cycles, thereby forming a molybdenum silicide cover layer.
[0083] The thickness of the formed molybdenum silicide capping layer was measured by electron scanning microscopy. The thickness of each cycle grown under different diiodosilane injection times was as follows: Figure 2 The confirmation shown is 1.85 to
[0084] X-ray photoelectric analysis of the deposited capping layer confirmed the ratio of silicon to molybdenum at different diiodosilane injection times. Figure 3 The values are shown to be 1.68 to 2.41 at different injection times of diiodosilane.
[0085] The crystal phase of the molybdenum silicide capping layer formed at a ratio of silicon to molybdenum of 2 was analyzed by X-ray diffraction analysis. It was found that the crystal phase was confirmed to be a hexagonal phase before the heat treatment, but a phase transition to a tetragonal phase occurred after the heat treatment.
[0086] Analysis of a pellicle film having a structure with a silicon nitride thin film as the core layer and a molybdenum silicide capping layer formed with a silicon to molybdenum ratio of 2 showed a transmittance of 92% and a reflectance of 0.036.
[0087] [Example 2]
[0088] A molybdenum silicide capping layer is formed by atomic layer deposition.
[0089] The silicon wafer formed of silicon nitride on which the molybdenum silicide capping layer was to be formed was transferred into the deposition chamber and maintained at 450° C. Dichlorosilane (SiH2Cl2) filled in the stainless steel container was transferred through the MFC for 1 to 7 seconds for adsorption, and then the unreacted compound was removed by 2000 sccm of argon for 3 seconds.
[0090] Then, molybdenum pentachloride (MoCl5) filled in the stainless steel container and argon gas 50 sccm as a transport gas were transferred for 1 second for adsorption, and then unreacted compounds were removed by 2000 sccm of argon gas for 3 seconds. Then, a molybdenum silicide capping layer was formed by using 2000 sccm of hydrogen gas and 100 W plasma. Finally, unreacted compounds were removed by 2000 sccm of argon gas for 3 seconds.
[0091] The above-described steps were repeated 200 times as one cycle, thereby forming a molybdenum silicide cap layer.
[0092] X-ray photoelectric analysis of the deposited covering layer showed that a covering layer with a molar ratio of molybdenum to silicon of 2 could be obtained by adjusting the injection time of dichlorosilane.
[0093] [Example 3]
[0094] A tungsten silicide capping layer is formed by atomic layer deposition.
[0095] A silicon wafer formed of silicon nitride, which is to be covered with a silicide layer of tungsten, is transferred into a deposition chamber and maintained at 450° C. Diiodosilane (SiH2I2) filled in a stainless steel container and 50 sccm of argon as a delivery gas are transferred for 1 to 7 seconds for adsorption, and then unreacted compounds are removed for 3 seconds using 2000 sccm of argon.
[0096] Then, tungsten pentachloride (WCl5) filled in the stainless steel container and argon gas 50sccm as a transport gas were transferred for 1 second for adsorption, and then unreacted compounds were removed by 2000sccm of argon gas for 3 seconds. Then, a tungsten silicide capping layer was formed by using 2000sccm of hydrogen gas and 100W plasma. Finally, unreacted compounds were removed by 2000sccm of argon gas for 3 seconds.
[0097] The above-described steps were repeated 200 times as one cycle, thereby forming a tungsten silicide cap layer.
[0098] X-ray photoelectron analysis of the deposited capping layer confirmed the formation of a tungsten silicide capping layer.
[0099] As described above, the present invention is illustrated through specific matters and limited embodiments and comparative examples, but they are only provided to help a more complete understanding of the present invention. The present invention is not limited to the above-mentioned embodiments, and any technician in the field to which the present invention belongs can make various revisions and modifications based on such records.
[0100] Therefore, the concept of the present invention is not limited to the illustrated embodiments, and not only the scope of protection claimed by the present invention, but also all forms that are equivalent to or have equivalent modifications to the scope of protection claimed by the present invention belong to the category of the concept of the present invention.
Claims
1. A method for manufacturing a protective film, comprising the steps of forming a metal silicide capping layer on a central layer using a silicon precursor and a metal precursor represented by the following chemical formula 1, [Chemical formula 1] SiH n X 4-n In the chemical formula 1, X is a halogen; n is an integer of 1 to 3.
2. The method for manufacturing a pellicle membrane according to claim 1, wherein: The central layer is Si, SiN x 、SiC x or their mixed films.
3. The method for manufacturing a pellicle membrane according to claim 1, wherein: The central layer is a layer of Si material and SiN x The material layer is a 2-layer membrane structure.
4. The method for manufacturing a pellicle membrane according to claim 2, wherein: The protective film has one or more protective layers between the layers where the central layer and the covering layer meet, below the central layer, or at these locations simultaneously, and the protective layer is selected from B x N, B, Zr, Zn, B x C. SiC x or SiN x It is composed of one or two or more substances.
5. The method for manufacturing a pellicle membrane according to claim 1, wherein: The metal of the metal precursor is Mo, Ni, Ru, Pt, Cu, Ti, Zr, Nb, Hf, Ta, W or Cr.
6. The method for manufacturing a pellicle membrane according to claim 1, wherein: The molar ratio of metal:silicon of the silicon precursor and the metal precursor is 1:0.2 to 6.
7. The method for manufacturing a pellicle membrane according to claim 1, wherein: The metal silicide capping layer is formed by atomic layer deposition (ALD) or chemical vapor deposition (CVD).
8. The method for manufacturing a pellicle membrane according to claim 1, wherein: The formation of the metal silicide capping layer comprises the following steps: a) step of heating the core layer installed in the chamber; b) a step of adsorbing a silicon precursor and a metal precursor on the core layer; and c) A step of injecting a reaction gas into the central layer on which the silicon precursor and the metal precursor are adsorbed to produce a metal silicide capping layer.
9. The method for manufacturing a pellicle membrane according to claim 8, wherein: The reaction gas is any one or more selected from oxygen (O2), ozone (O3), distilled water (H2O), hydrogen peroxide (H2O2), nitric oxide (NO), nitrous oxide (N2O), nitrogen dioxide (NO2), ammonia (NH3), nitrogen (N2), hydrazine (N2H4), amines, diamines, carbon monoxide (CO), carbon dioxide (CO2), C1 to C12 saturated or unsaturated hydrocarbons, hydrogen (H2), argon (Ar) and helium (He).
10. A protective film comprising a core layer and a metal silicide capping layer, wherein the metal silicide capping layer is manufactured on the core layer using a silicon precursor and a metal precursor represented by the following chemical formula 1, [Chemical formula 1] SiH n X 4-n In the chemical formula 1, X is a halogen; n is an integer of 1 to 3.
11. The protective film according to claim 10, wherein: The molar ratio of metal to silicon in the metal silicide capping layer is 1:0.2 to 6.