Method for manufacturing tubular solid oxide fuel cell and cell stack

By using high-temperature metal solder and welding technology in SOFC battery packs, the problems of sealing and electrical switching are solved, and efficient and reliable SOFC battery pack assembly is achieved, which is suitable for high-temperature and rapid heating applications of microtubular SOFCs.

CN118765449APending Publication Date: 2024-10-11TOPAZ LLC (TOPAZ LLC)
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202280092764.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2021-12-29
Filing Date
2022-12-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing technology, when manufacturing high-temperature solid oxide fuel cells (SOFC), the sealant is intolerant to temperature changes, resulting in a decrease in the performance of the microtubular SOFC at high heating rates, and ohmic losses due to differences in thermal expansion coefficients during the electrical switching process. increase, affecting the reliability and efficiency of the battery pack.

Method used

Using high-temperature metal solder and welding operations, a single tubular SOFC is placed in a through hole of the substrate, and welded using conductive solder with a melting point higher than the SOFC operating temperature and a thermal expansion coefficient close to the substrate and electrode materials, combined with pre-coated heat-resistant conductive materials to Improves solder joint reliability and electrical contact, simplifies the assembly process and reduces material consumption.

Benefits of technology

It achieves simultaneous high-quality sealing and electrical switching of SOFC battery packs in one operation, shortens assembly time, reduces material costs, and improves the reliability and efficiency of the battery pack. It is suitable for high-temperature rapid heating applications of microtubular SOFCs. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765449A_ABST
    Figure CN118765449A_ABST
Patent Text Reader

Abstract

The invention relates to the field of electrical engineering, in particular to a method for manufacturing a high-temperature solid oxide fuel cell (SOFC) with a tubular shape and a tubular SOFC battery pack. The battery pack includes at least two tubular SOFCs and a support plate having through-holes for the tubular SOFCs. The method includes applying a solder to a region of the support plate in which the individual SOFC is arranged, followed by soldering, where the solder is made of an electrically conductive material having a melting point higher than the operating temperature of the SOFC and a thermal expansion coefficient close to the thermal expansion coefficients of the support plate material and the SOFC electrode material. As a result, the sealing quality between each individual tubular SOFC and the support plate during the welding process is improved, which in turn maintains the power characteristics of the battery pack during the thermal cycling process.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to the field of electrical engineering, namely to a high temperature solid oxide fuel cell (SOFC) having a tubular shape with a supported anode electrode, which SOFC can be used to manufacture a fuel cell stack.

[0002] Currently, there are two important tasks when manufacturing electrochemical generators using solid oxide fuel cells (SOFCs): sealing the SOFCs when assembling them into cells to ensure reliable separation of the gas spaces for supply and exhaust gases (fuel gas and oxidant gas); and ensuring efficient electrical switching of the SOFCs while minimizing the ohmic resistance in the cell stack.

[0003] To solve the first task, eg sealing tubular or planar SOFCs in a stack, specialized glass-ceramic sealants based on oxides of silicon, boron, aluminum and other metals are usually used (eg glass-ceramic high temperature adhesives in patent RU 2138885).

[0004] The main disadvantages of this sealing method are the low tolerance of the glass in the sealant composition to sudden temperature changes (especially when the SOFC reaches an operating temperature of 650°C-850°C) and the narrow operating temperature range. This limitation is acceptable in power plants for stationary applications, which gradually reach operating temperature within a few hours and do not operate under frequent start-stop conditions. For micro-tubular SOFCs (SOFCs with a tubular shape, typically less than 10 mm in diameter), one of the main advantages of using them in mobile power devices and backup power systems is the high temperature rise rate allowed (more than 200°C per minute) without being damaged, so in order to maintain its operating performance under significant temperature changes (especially due to glass breakage or changes in its morphological properties), it is not advisable to use glass in the battery pack of micro-tubular SOFCs.

[0005] The second task - ensuring efficient electrical switching of tubular and micro-tubular SOFCs in a stack - is usually solved by using coils on the surface of the SOFC (i.e., anode and / or cathode electrodes). The coils have wires made of silver or platinum or precious metal-based alloys that are further interconnected, which is a solution to the electrical switching problem of individual tubular SOFCs.

[0006] However, when a power supply device having a SOFC is operated, slowly increasing (e.g., due to surface oxidation) or rapidly increasing ohmic losses (e.g., due to separation) may occur due to the different thermal expansion coefficients in the materials of the SOFC electrodes (ceramic, metal, or cermet) and the wire conductive elements and the destruction of such electrical contact caused by the small electrical contact area between the wire and the electrode.

[0007] There are some technical solutions, such as patent RU 2138885, which propose to use various types of bushings and gaskets to connect and transform fuel cells into assemblies.

[0008] The disadvantages of this solution are the complex design and high material consumption, as well as the high complexity of the assembly process and the low reliability of the structure, since additional sealing of the matching boundaries of the bushings and gaskets is required.

[0009] The claimed effect of the present technical solution is to improve the quality and reliability of the manufactured tubular (especially micro-tubular) SOFC cell stack, while reducing the process cost by simplifying the process, improving manufacturability and shortening the duration of the assembly process of the SOFC cell stack by combining electrical switching and sealing into a single operation through the use of high-temperature metal solders and welding operations.

[0010] This effect is achieved by manufacturing a stack of tubular SOFCs in such a way that a single tubular SOFC is placed in a through hole of a substrate, solder is applied to the area of ​​the tubular SOFC location in the hole of the substrate, and then soldering is performed, such as by induction soldering, using a high temperature solder made of a conductive material having a melting point above the operating temperature of the SOFC and a coefficient of thermal expansion (CTE) close to that of the substrate and the SOFC electrodes.

[0011] The substrate is made of a material that is resistant to high temperatures and has a low ohmic resistance, such as a metal, or of a non-conductive material with conductive elements in the hole areas, such as metal tracks or metallized areas.

[0012] When soldering, a solder is used which is made of an electrically conductive material, for example an alloy of a metal, in particular an alloy based on Ni, Co, Si, but other metals may also be used.

[0013] If necessary, a portion of the tubular SOFC, in particular the surface of the electrode in the welding area of ​​each single SOFC placed in the hole of the substrate, can be pre-coated with a layer of conductive material resistant to the SOFC operating temperature (chemically stable at the SOFC operating temperature) to improve the reliability of the weld. The welding area is usually the end of the SOFC. The layer of heat-resistant conductive material is, for example, a layer made of nickel, platinum or titanium hydride. The coating is usually applied by chemical deposition or other coating methods, in particular using a suspension. The pre-coated surface is the surface of the anode electrode and the surface of the electrolyte near the anode electrode, or the surface of the cathode electrode, or the surface of the cathode electrode and the surface of the electrolyte near the cathode electrode.

[0014] Using solder made of a conductive material with a melting point higher than the operating temperature of the SOFC and a CTE close to the CTE of the SOFC substrate material and electrode material can simultaneously provide high-quality sealing and electrical switching of the battery pack, which in turn greatly shortens the assembly time of the battery pack, simplifies the assembly process and reduces material costs.

[0015] Furthermore, prior to the welding operation, the tubular SOFC may be subjected to preliminary surface treatment at the welding region.

[0016] Previously, the key difficulty in welding was to achieve reliable mechanical and electrical contact between the metal solder and the supporting substrate made of the initial metal ceramic material, especially composed of NiO composite material and ceramic electrolyte material (such as YSZ or SSZ), and with the ceramic material of the cathode electrode (such as LSC or LSCF).

[0017] Currently, there are methods for welding ceramic products and metal ceramics with compositions similar to SOFC metal ceramics, however, in addition to being costly (due to the precious metals in their composition), active silver-based solders that maintain (wet) the surface of the ceramic products are not suitable for use in tubular SOFC stacks operating at high temperatures, because the SOFC material in the welding area is destroyed due to the large difference in the coefficient of thermal expansion (CTE) during thermal cycling, which drastically reduces the power characteristics of the SOFC stack, and causes a complete loss of its operability due to the direct mixing of the fuel gas (on the SOFC anode electrode side) with the oxidant (oxygen in the air on the SOFC cathode electrode side).

[0018] The second disadvantage of using silver-based solder is the lateral migration of silver along the grain boundaries of ceramic microcrystals in the electrolyte layer at high temperatures. Therefore, when solder is applied to the cathode electrode layer, anode electrode layer or electrolyte layer, after the SOFC has been operating for a period of time, the operating voltage drops due to the short circuit of the anode electrode and cathode electrode in the solder application area, which in turn leads to a decrease in the power characteristics of the SOFC.

[0019] According to the technical solution, a metal alloy, in particular an alloy based on Ni, Co, and Si, is used as a solder material. In order to improve the reliability of mechanical and electrical contact in the area where the solder is subsequently applied, and to improve the wettability of the ceramic surface with the solder during welding, the surface of the anode electrode, or the surface of the anode electrode and the surface of the electrolyte or the surface of the cathode electrode of a material resistant to welding temperature (mainly Ni or platinum or titanium hydride) can be preliminarily tinned, which can be applied to the surface of the tubular SOFC in the welding area by chemical deposition or physical coating (for example, using a suspension). During the welding operation, the melting point of the solder used should not exceed the limit temperature for maintaining the stability of the materials in the SOFC and its components, and the welding operation is especially performed by heating the welding object in a furnace. For the SOFC embodiment used as an example of the technical solution claimed for protection, the SOFC consists of an anode substrate Ni-YSZ, a functional anode layer Ni-YSZ, an electrolyte YSZ, a buffer layer GDC, and a cathode layer LSCF, and the melting point of the solder is lower than 1200°C. When using soldering methods (particularly induction soldering) that allow local heating of the SOFC / substrate connection area, solder materials can be used that exceed the thermochemical stability temperature of the material of each SOFC layer but do not exceed the melting point of the substrate material.

[0020] To ensure the reliability of the SOFC / substrate connection in terms of tightness and electrical contact, the solder material and substrate material are selected based on the consistency of the thermal expansion coefficients of these materials. Typically, the difference in thermal expansion coefficients of adjacent SOFC layers is less than 10*10 in the temperature range of 20°C-800°C. -6 K -1 , preferably less than 5*10 -6 K -1 In particular, the solder material may be selected based on nickel (eg BNi-2 grade) and the substrate material may be a heat resistant steel, in particular AISI 444.

[0021] The use of solders, in particular nickel-based (e.g. BNi-2 grade) solders, which do not contain precious metals in their composition and have a melting point above the SOFC operating temperature, allows tubular SOFCs in modules or stacks to be sealed and electrically switched simultaneously (in a single operation).

[0022] The claimed technical solution is economically more advantageous because cheaper materials are used and no specialized equipment is required, and the production process can be scaled up without major changes to it, for example, by sequentially assembling SOFC cell stacks on a conveyor belt in each welding cycle, or by manufacturing multiple SOFC modules or cell stacks simultaneously.

[0023] The claimed invention is illustrated by means of diagrams.

[0024] Figure 1 shows an overall view of a cell stack (module) of a SOFC with two substrates and a gas collector (without solder for clarity);

[0025] Figure 2 The position of the tubular SOFC in the substrate is shown (with solder);

[0026] Figure 3 A schematic diagram showing the application of a pre-coating layer to the end of a tubular SOFC (using a suspension application method by immersing the object in the suspension);

[0027] Figure 4 A single tubular SOFC is shown.

[0028] Next, let us consider a cell stack 1 of tubular SOFCs having two substrates.

[0029] A single SOFC is made in the form of a tubular substrate of an anode electrode 2, on which a functional anode layer (optional layer), an electrolyte layer 3 and a cathode electrode layer 4 are applied. The ends of the SOFC are placed in the corresponding through holes 5 and 6 of the substrates 7 and 8. In this case, the cathode current collector is provided by a bus 9. For the supply and distribution of the fuel gas, a collector 10 with a fuel supply pipe 11 is used. Even if only one substrate is installed, one gas collector can be used.

[0030] In order to ensure a reliable seal (mainly in the fuel gas supply area), a rigid connection of the tubular SOFC to the substrate by solder 12 is used. To this end, after pre-coating the tubular SOFC, the solder is applied to the welding area and then the tubular SOFC is welded to the hole of the steel substrate, for example by induction. In this case, the surface of the anode electrode (anode substrate with or without a functional anode layer) and the surface of the anode electrode to which the solid electrolyte layer is applied are simultaneously in contact with the solder in the hole area of ​​the substrate, and the surface of the cathode electrode is connected to the solder without ensuring that the solder is in contact with the solid electrolyte layer in the hole area. Due to the heating, the solder material flows into the cavity of the hole, sealing them. At the same time, in the cathode electrode area, the solder is in close contact with the collector bus 9 and / or the SOFC collector (not shown), thereby ensuring reliable electrical switching with minimal ohmic resistance.

[0031] Due to the pre-coating, the fluidity of the solder at the welding surface is increased and the welding location is sealed. When the thickness of the pre-coating layer (eg titanium hydride) is less than 10 microns, an acceptable electrical contact resistance between the solder material and the SOFC electrode can be achieved.

[0032] Thus, due to the use of high temperature solder and the method of welding tubular SOFC, the problem of electrical switching and the problem of sealing are solved simultaneously (in one operation) because the solder is able to penetrate into the pores of the substrate to seal the space of the entire contact area between the substrate and the SOFC surface. In addition, the solder simultaneously provides electrical contact with the substrate (or the conductive element thereon) of the anode electrode or cathode electrode of the SOFC.

[0033] The following is a specific embodiment of a method for manufacturing a battery pack of SOFC:

[0034] Example 1. Two tubular solid oxide fuel cells with layer structure:

[0035] - a supporting substrate for the anode electrode, the supporting substrate consisting of NiO / 8YSZ in the ratio 70 wt % / 30 wt %, having a thickness of 400 μm, the porosity of the layer being 50%;

[0036] - an anode functional layer consisting of NiO / 8YSZ in a ratio of 50 wt % / 50 wt % and having a thickness of 10 μm;

[0037] - an electrolyte layer consisting of 8YSZ and having a thickness of 5 micrometers;

[0038] - a cathode functional layer consisting of LSCF / GDC in a ratio of 40 wt % / 60 wt % and correspondingly having a thickness of 10 μm;

[0039] - a cathode collector layer, the cathode collector layer is composed of LSCF, has a thickness of 80 micrometers and a porosity of 50%;

[0040] - a metallization layer consisting of nickel chemically deposited on the surface of the carrier substrate, the anodic functional layer and the electrolyte in the welding area, with a thickness of 10 micrometers;

[0041] - A cathode current collector made of AISI 444 steel wire fixed to the surface of the cathode current collector layer, vertically in the holes of a 5 mm thick substrate made of AISI 444 steel.

[0042] The position of the fuel cell in the substrate is chosen so that the metallized surface intersects the substrate plane. Solder grade BNi-4 in the form of solder paste is applied to the surface where the substrate intersects the fuel cell. The applied solder is dried at 200°C for one hour. The assembly is then placed in a high temperature furnace and soldered in an argon medium at 1080°C for 10 minutes.

[0043] Example 2. Two tubular shaped solid oxide fuel cells with layer structure:

[0044] - a supporting substrate for the anode electrode, the supporting substrate consisting of NiO / 8YSZ in the ratio 60 wt % / 40 wt %, having a thickness of 500 μm, the porosity of the layer being 40%;

[0045] - an anode functional layer consisting of NiO / 8YSZ in a ratio of 60 wt % / 40 wt % and having a thickness of 10 μm;

[0046] - an electrolyte layer consisting of SSZ and having a thickness of 5 μm;

[0047] - buffer layer GDC, thickness 3 microns;

[0048] - a cathode functional layer consisting of LSCF / GDC in a ratio of 40 wt % / 60 wt % and correspondingly having a thickness of 10 μm;

[0049] - a cathode collector layer, the cathode collector layer is composed of LSCF, has a thickness of 80 micrometers and a porosity of 50%;

[0050] - a metallization layer consisting of platinum, placed (by immersion in the prepared suspension) on the surface of the supporting substrate of the anode electrode, the anode functional layer and the electrolyte in the welding area, with a thickness of 10 micrometers;

[0051] - A cathode current collector made of a platinum nickel wire fixed to the surface of the cathode current collector layer, vertically located in the holes of a 5 mm thick substrate made of AISI 444 steel.

[0052] The position of the fuel cell in the substrate is chosen so that the metallized surface intersects the plane of the substrate. Solder grade BNi-2 in the form of solder paste is applied to the surface of the substrate where it intersects the fuel cell. The applied solder is dried at 200°C for one hour. The assembly is then placed inside an induction heating coil where the substrate and solder material are heated to the melting point of the solder.

[0053] Therefore, the use of solder made of a conductive material with a melting point higher than the SOFC operating temperature and a thermal expansion coefficient close to that of the substrate material and the SOFC electrode material allows high-quality sealing and electrical switching of the battery pack simultaneously (in one operation), which in turn greatly shortens the time and simplifies the battery pack assembly process and reduces material costs.

Claims

1. A method for manufacturing a tubular SOFC battery pack, characterized in that: A single tubular SOFC is placed in a through hole of a substrate, solder is applied to the area of ​​the hole of the substrate where the tubular SOFC is placed, and then soldering is performed, wherein the solder is made of a conductive material having a melting point higher than the operating temperature of the SOFC and a thermal expansion coefficient (CTE) close to the thermal expansion coefficient of the substrate material and the SOFC electrode material.

2. The method according to claim 1, characterized in that The surface of the SOFC electrode in the welding region of each individual SOFC placed in the hole of the substrate is pre-coated with a layer of conductive material resistant to the operating temperature of the SOFC.

3. The method according to claim 2, characterized in that The pre-coated surfaces are the surface of the anode electrode and the surface of the electrolyte close to the anode electrode.

4. The method according to claim 2, characterized in that: The pre-coated surface is the surface of the cathode electrode or the surface of the cathode electrode and the surface of the electrolyte close to the surface of the cathode electrode.

5. The method according to claim 2, characterized in that: The layer of conductive material is, for example, a nickel layer, a platinum layer or a titanium hydride layer.

6. A cell stack of tubular SOFCs, comprising at least two tubular SOFCs and a substrate having through holes for the tubular SOFCs, characterized in that: The tubular SOFC cell stack is manufactured according to the method of any one of claims 1 to 5.

Citation Information

Patent Citations

  • Unit of assemblies of solid oxide fuel elements with coefficient of thermal expansion exceeding that of their electrolyte

    RU2138885C1