Injectable collapse-resistant silicon-calcium-based self-curing material as well as preparation method and application thereof
By using a combination of tricalcium silicate, strontium carbonate, nano-hydroxyapatite and Pluronic F-127 in calcium silicate-based materials, the problems of poor operability, insufficient collapse resistance and insufficient curing performance of calcium silicate-based materials are solved, achieving Efficient dental filling and restorative materials.
Patent Information
- Application Number
- CN202410746002.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-15
AI Technical Summary
The existing calcium silicon-based bioceramic self-curing materials have difficulties in synergistic enhancement in operability, collapse resistance and curing performance, making it difficult to meet the multiple performance requirements of dental filling and restorative materials.
An injectable anti-collapse self-curing material composed of tricalcium silicate powder, strontium carbonate powder, nano-hydroxyapatite and Pluronic F-127 is used. Through the temperature-sensitive gelling properties of Pluronic F-127 and nano-hydroxyphosphorus Limestone promotes hydration kinetics, optimizing rheology and curing characteristics.
It achieves the excellent collapse resistance, injectability and good curing performance of calcium silicon-based materials, avoids the phenomenon of free powder collapse, and ensures the filling effect and biological activity.
Smart Images

Figure CN118766769A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomedical materials, and in particular relates to an injectable anti-collapse type silicon-calcium-based self-solidifying material and a preparation method and application thereof. Background Art
[0002] The dental pulp is mainly composed of blood vessels, nerves and connective tissue. It is a necessary condition for the development of tooth roots and apical closure, and is of great significance for maintaining normal function and long-term retention of teeth. Pulp and periapical diseases caused by caries and mechanical damage are common oral diseases in clinical practice. Dental filling and restorative materials are one of the key factors that determine the therapeutic efficacy of endodontic diseases. Although there are many dental filling materials used in clinical practice, including zinc oxide eugenol cement, glass ionomer cement, bioceramic self-curing materials, etc., there is no dental material that meets all performance requirements.
[0003] Mineral Trioxide Aggregate (MTA) is a bioceramic material with excellent performance. It is composed of tricalcium silicate, dicalcium silicate, calcium silicate and bismuth oxide. It has good biocompatibility, bioactivity, apatite mineralization ability and sealing properties. Therefore, it is successfully used in root canal treatment, pulpotomy, revascularization, pulp capping, root canal backfilling and other pulp and periapical disease treatment. However, traditional MTA still has poor operating performance and cannot be injected. It has a strong sense of sand during mixing, which can easily lead to uneven mixing of solid and liquid phases, resulting in problems such as decreased curing performance and biological performance; and the material is prone to disintegration and freeing when encountering a water-containing liquid phase.
[0004] At present, the operability, injectability and anti-collapse properties of calcium-silicon-based materials are mainly improved by polymer materials such as sodium alginate, chitosan, and gelatin. The main mechanism of this strategy is that these organic substances can be dissolved in water to form a gelling material of a certain viscosity, thereby effectively enhancing the rheological properties and cohesion of calcium-silicon-based materials. For example, studies have found that sodium alginate can effectively enhance the anti-collapse properties of calcium phosphate-based bone cement, but it inevitably prolongs the curing time (H. Mabroum, et al. Ceramics International, 2021, 47 (17): 23973-23983.). Although the above strategies can improve the operability and anti-collapse properties of the material, they will also hinder its hydration dynamics, ultimately leading to a delay in the curing time of the material and a reduction in mechanical strength.
[0005] For this type of problem, the currently effective method is to use organic-inorganic composites to synergistically enhance the injectability, anti-collapse and curing properties of silicon-calcium-based materials. For example, CN114099352A discloses a kind of anti-collapse silicon-calcium-based root canal filling self-curing material and its preparation method and application, which effectively improves the injectability and anti-collapse of silicon-calcium-based materials through konjac gum. On the other hand, calcium formate is used to promote the curing of silicon-calcium-based materials, effectively shortening the curing time.
[0006] In addition, the powder material is pre-mixed with the non-aqueous phase to form a self-curing material slurry, which can significantly enhance the handling performance and injectability of the silicon-calcium-based material. For example, CN116492230A discloses a storable, injectable root canal filling material, which mixes a magnesium phosphate-based powder with a caprylic / caprylic acid triglyceride liquid phase to form a premixed self-curing material. The material is injectable, does not require on-site mixing, and is easy to operate. During use, the liquid phase in the material and the water in the repair tissue diffuse and exchange, thereby inducing the self-curing material to solidify. Therefore, the material has poor curing performance, slow hydration rate, and low mechanical strength.
[0007] In summary, the MTA-type calcium-silicon-based bioceramic self-curing materials used in clinical practice have poor operability, are difficult to inject, and have insufficient anti-collapse performance. Although researchers have proposed many improvement strategies to effectively improve its shortcomings, the existing methods cannot solve the major problem of synergistically enhancing the operability, anti-collapse and curing properties of calcium-silicon-based materials.
[0008] Therefore, how to construct a bioactive curing material that is resistant to collapse, injectable, and has good curing properties is still a bottleneck problem that needs to be solved urgently in this field. Summary of the invention
[0009] Purpose of the invention: The purpose of the present invention is to provide an injectable anti-collapse type silicon-calcium-based self-curing material and its preparation method and application in view of the deficiencies of the prior art. The present invention solves the defects of the existing silicon-calcium-based materials that are difficult to inject, have poor operating performance and anti-collapse performance, and solves the technical problem that the prior art cannot synergistically enhance the anti-collapse and curing performance.
[0010] Technical solution: The purpose of the present invention is achieved through the following technical solution:
[0011] The invention provides an injectable anti-collapse type calcium-silicon-based self-curing material, which consists of solid phase and liquid phase components; the solid phase comprises tricalcium silicate powder and strontium carbonate powder; the liquid phase comprises at least an aqueous solution containing nano-hydroxyapatite and Pluronic F-127; and the mass ratio of the liquid phase to the solid phase is 0.4-0.6:1.
[0012] Strontium carbonate has good ability to promote osteogenesis, odontoblast formation and angiogenesis, is beneficial to promoting biological functions such as cell adhesion, proliferation and differentiation, and can improve the osteogenesis / odontoblast formation ability of the silicon-calcium based material of the present invention.
[0013] Within the range of the liquid-to-solid mass ratio selected by the present invention, the calcium-silicon-based self-curing material has excellent anti-collapse and injectability, and excellent rheological properties.
[0014] The present invention uses the reversible thermosensitive gelling property of Pluronic F-127 to give the calcium silicate base good injection performance and operability at room temperature and excellent anti-collapse ability at body temperature. Nano-hydroxyapatite is used to promote the nucleation and growth process of tricalcium silicate hydration products, accelerate the hydration kinetic reaction, and solve the technical problem that the anti-collapse performance and curing characteristics of bioceramic self-curing materials cannot be synergistically enhanced.
[0015] A preferred embodiment of the present invention is that the liquid phase may also contain disodium hydrogen phosphate. Disodium hydrogen phosphate has a certain effect of promoting the solidification of silicon-calcium based materials.
[0016] Preferably, in the solid phase, the mass percentage of tricalcium silicate powder is 70% to 90%, the mass percentage of strontium carbonate powder is 10% to 30%, and the sum of the mass percentages of the two is 100%. The component ratio in the powder of the present invention can ensure that the self-solidification ability of tricalcium silicate can be preserved, and the biological function of strontium carbonate can be guaranteed.
[0017] Preferably, in the liquid phase, the mass percentage of nano-hydroxyapatite is 1% to 4%, and the mass percentage of Pluronic F-127 is 17.5% to 22.5%. The concentration range of Pluronic F-127 in the liquid phase of the present invention has sufficient temperature-sensitive gelling properties, which can make the silicon-calcium-based self-curing material of the present invention have excellent fluidity at room temperature and can show stronger anti-collapse performance at body temperature.
[0018] Preferably, the particle size of the tricalcium silicate powder is 0.1-100 μm. Within this particle size range, the tricalcium silicate powder has good fineness and a good feel for powder handling.
[0019] Furthermore, the particle size of the tricalcium silicate powder is 0.1 to 10 μm.
[0020] The present invention also provides a method for preparing the injectable anti-collapse type calcium-silicon-based self-curing material, comprising the following steps:
[0021] (1) mixing tricalcium silicate powder and strontium carbonate powder to obtain a solid phase component;
[0022] (2) adding Pluronic F-127 to water to dissolve it, and then ultrasonically dispersing nano-hydroxyapatite in the Pluronic F-127 aqueous solution to obtain a liquid phase component;
[0023] (3) The obtained liquid phase component and solid phase component are uniformly blended in proportion to obtain the injectable anti-collapse type silicon-calcium based self-solidifying material.
[0024] The present invention also provides the use of the injectable anti-collapse type calcium-silicon-based self-curing material as a dental repair and filling material.
[0025] The dental restoration and filling at least include root canal filling, apexification and pulp capping.
[0026] Beneficial effects:
[0027] (1) The present invention uses tricalcium silicate, strontium carbonate, Pluronic F-127 and nano-hydroxyapatite for the first time to solve the defects of existing calcium silicate-based materials, such as poor operability, poor anti-collapse performance and insufficient curing performance. Compared with existing calcium phosphate or calcium silicate-based self-curing materials reinforced with organic polymer materials, the reversible thermosensitive gelling property of Pluronic F-127 gives calcium silicate-based materials good injection performance and operability at room temperature and excellent anti-collapse ability at body temperature. Nano-hydroxyapatite is used to promote the nucleation and growth process of tricalcium silicate hydration products, accelerate the hydration kinetic reaction, and solve the technical problem that the anti-collapse performance and curing properties of bioceramic self-curing materials cannot be synergistically enhanced.
[0028] (2) The injectable anti-collapse type silicon-calcium-based self-curing material of the present invention has a strong anti-collapse ability, can maintain its original shape in an aqueous solution, does not cause free powder collapse, and has good curing properties.
[0029] (3) The silicon-calcium-based self-curing material of the present invention is easy to inject, convenient to operate, and has a good filling effect. The silicon-calcium-based self-curing material of the present invention has a strong injection capacity and does not cause filter pressing during the injection process, which can ensure that the injection process of the self-curing material is smooth and can smoothly reach the repair position, thereby forming a good filling effect.
[0030] (4) The calcium-silicon-based self-curing material of the present invention can induce dense apatite deposition, promote the bonding between the material and the repair tissue, and has excellent biological activity. The apatite-forming ability is the guarantee for good bonding between the repair material and the repair tissue. The apatite at the interface can form a physiological bonding effect, and is beneficial to the biological properties of cells and enhances the biological activity of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1The injection rate results of the injectable anti-collapse type silicon-calcium-based self-curing materials in Examples 1-3 and Comparative Examples 1-2 of the present invention;
[0032] Figure 2 The injection rate results of the injectable anti-collapse type calcium-silicon based self-curing material at different times in Example 2 of the present invention;
[0033] Figure 3 The injection rate results of the injectable anti-collapse type silicon-calcium-based self-curing material in Examples 4-7 of the present invention;
[0034] Figure 4 The anti-collapse results of the injectable anti-collapse type silicon-calcium-based self-curing materials in Examples 1-3 of the present invention and Comparative Examples 1-2;
[0035] Figure 5 The anti-collapse results of the injectable anti-collapse type silicon-calcium-based self-curing materials in Examples 4 and 5 of the present invention;
[0036] Figure 6 The anti-collapse results of the injectable anti-collapse type silicon-calcium-based self-curing materials in Examples 6 and 7 of the present invention;
[0037] Figure 7 This is the XRD diagram of the hydration product of the injectable anti-collapse type silicon-calcium based self-curing material in Example 1 of the present invention;
[0038] Figure 8 This is the XRD diagram of the surface mineralization of the injectable anti-collapse type calcium-silicon-based self-curing material in Example 3 of the present invention. DETAILED DESCRIPTION
[0039] The technical solution of the present invention is described in detail below through specific embodiments, but the protection scope of the present invention is not limited to the embodiments.
[0040] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.
[0041] The tricalcium silicate used in the following examples was purchased from Kunshan Huaqiao Technology New Materials Co., Ltd., strontium carbonate and disodium hydrogen phosphate were purchased from Aladdin Reagent Co., Ltd., Pluronic F-127 was purchased from Sigma-Aldrich Reagent Co., Ltd., and nano-hydroxyapatite was purchased from Xi'an Ruilin Biotechnology Co., Ltd.
[0042] Example 1
[0043] 80% by mass of tricalcium silicate powder and 20% by mass of strontium carbonate powder were weighed and mechanically mixed to obtain a solid phase.
[0044] The raw materials are weighed according to the following mass fractions: component (a) 20% Pluronic F-127, component (b) 1% nano-hydroxyapatite, and component (c) 1.5% disodium hydrogen phosphate. Component (a) is dissolved in deionized water, and component (c) is added. After dissolution, component (b) is added and ultrasonic dispersion is performed to obtain a liquid phase.
[0045] Finally, the obtained liquid phase and solid phase were fully and evenly stirred at a mass ratio of 0.5:1 to obtain an injectable anti-collapse type silicon-calcium based self-curing material.
[0046] Example 2
[0047] 80% by mass of tricalcium silicate powder and 20% by mass of strontium carbonate powder were weighed and mechanically mixed to obtain a solid phase.
[0048] The raw materials are weighed according to the following mass fractions: component (a) 20% Pluronic F-127, component (b) 2% nano-hydroxyapatite, and component (c) 1.5% disodium hydrogen phosphate. Component (a) is then dissolved in deionized water, and component (c) is added. After dissolution, component (b) is added and ultrasonic dispersion is performed to obtain a liquid phase.
[0049] Finally, the liquid phase and the solid phase are fully and evenly stirred at a mass ratio of 0.5:1 to obtain an anti-collapse injectable silicon-calcium-based self-curing material.
[0050] Example 3
[0051] 80% by mass of tricalcium silicate powder and 20% by mass of strontium carbonate powder were weighed and mechanically mixed to obtain a solid phase.
[0052] The raw materials are weighed according to the following mass fractions: component (a) 20% Pluronic F-127, component (b) 4% nano-hydroxyapatite, and component (c) 1.5% disodium hydrogen phosphate. Component (a) is then dissolved in deionized water, and component (c) is added. After dissolution, component (b) is added and ultrasonic dispersion is performed to obtain a liquid phase.
[0053] Finally, the liquid phase and the solid phase are fully and evenly stirred at a mass ratio of 0.5:1 to obtain an anti-collapse injectable silicon-calcium-based self-curing material.
[0054] Example 4
[0055] 70% by mass of tricalcium silicate powder and 30% by mass of strontium carbonate powder were weighed and mechanically mixed to obtain a solid phase.
[0056] The raw materials are weighed according to the following mass fractions: component (a) 20% Pluronic F-127, component (b) 2% nano-hydroxyapatite, and component (c) 1.5% disodium hydrogen phosphate. Component (a) is then dissolved in deionized water, and component (c) is added. After dissolution, component (b) is added and ultrasonic dispersion is performed to obtain a liquid phase.
[0057] Finally, the liquid phase and the solid phase are fully and evenly stirred at a mass ratio of 0.5:1 to obtain an anti-collapse injectable silicon-calcium-based self-curing material.
[0058] Example 5
[0059] 90% by mass of tricalcium silicate powder and 10% by mass of strontium carbonate powder were weighed and mechanically mixed to obtain a solid phase.
[0060] The raw materials are weighed according to the following mass fractions: component (a) 20% Pluronic F-127, component (b) 2% nano-hydroxyapatite, and component (c) 1.5% disodium hydrogen phosphate. Component (a) is then dissolved in deionized water, and component (c) is added. After dissolution, component (b) is added and ultrasonic dispersion is performed to obtain a liquid phase.
[0061] Finally, the liquid phase and the solid phase are fully and evenly stirred at a mass ratio of 0.5:1 to obtain an anti-collapse injectable silicon-calcium-based self-curing material.
[0062] Example 6
[0063] 80% by mass of tricalcium silicate powder and 20% by mass of strontium carbonate powder were weighed and mechanically mixed to obtain a solid phase.
[0064] The raw materials are weighed according to the following mass fractions: component (a) 17.5% Pluronic F-127, component (b) 2% nano-hydroxyapatite. Component (a) is then dissolved in deionized water, and after being dissolved, component (b) is added and ultrasonically dispersed to obtain a liquid phase.
[0065] Finally, the liquid phase and the solid phase are fully and evenly stirred at a mass ratio of 0.4:1 to obtain an anti-collapse injectable calcium-silicon-based self-curing material.
[0066] Example 7
[0067] 80% by mass of tricalcium silicate powder and 20% by mass of strontium carbonate powder were weighed and mechanically mixed to obtain a solid phase.
[0068] The raw materials are weighed according to the following mass fractions: component (a) 22.5% Pluronic F-127, component (b) 2% nano-hydroxyapatite. Component (a) is then dissolved in deionized water, and after dissolution, component (b) is added and ultrasonically dispersed to obtain a liquid phase.
[0069] Finally, the liquid phase and the solid phase are fully and evenly stirred at a mass ratio of 0.6:1 to obtain an anti-collapse injectable calcium-silicon-based self-curing material.
[0070] Comparative Example 1
[0071] Weigh 80% by mass of tricalcium silicate powder and 20% by mass of strontium carbonate powder, mix them mechanically to obtain a solid phase, and use deionized water as a liquid phase;
[0072] The liquid phase and the solid phase are fully and evenly stirred at a mass ratio of 0.5:1 to obtain a silicon-calcium based self-curing material.
[0073] Comparative Example 2
[0074] 80% by mass of tricalcium silicate powder and 20% by mass of strontium carbonate powder were weighed and mechanically mixed to obtain a solid phase.
[0075] The raw materials were weighed according to the following mass fractions: component (a) 20% Pluronic F-127, component (b) 1.5% disodium hydrogen phosphate. Component (a) was then dissolved in deionized water, and component (b) was added to obtain a liquid phase after dissolution.
[0076] Finally, the liquid phase and the solid phase are fully and evenly stirred at a mass ratio of 0.5 to obtain a silicon-calcium based self-curing material.
[0077] Comparative Example 3
[0078] 60% by mass of tricalcium silicate powder and 40% by mass of strontium carbonate powder were weighed and mechanically mixed to obtain a solid phase.
[0079] The raw materials are weighed according to the following mass fractions: component (a) 20% Pluronic F-127, component (b) 2% nano-hydroxyapatite, and component (c) 1.5% disodium hydrogen phosphate. Component (a) is then dissolved in deionized water, and component (c) is added. After dissolution, component (b) is added and ultrasonic dispersion is performed to obtain a liquid phase.
[0080] Finally, the liquid phase and the solid phase are fully and evenly stirred at a mass ratio of 0.5:1 to obtain an anti-collapse injectable silicon-calcium-based self-curing material.
[0081] Comparative Example 4
[0082] 80% by mass of tricalcium silicate powder and 20% by mass of strontium carbonate powder were weighed and mechanically mixed to obtain a solid phase.
[0083] The raw materials are weighed according to the following mass fractions: component (a) 25% Pluronic F-127, component (b) 2% nano-hydroxyapatite, and component (c) 1.5% disodium hydrogen phosphate. Component (a) is then dissolved in deionized water, and component (c) is added. After dissolution, component (b) is added and ultrasonic dispersion is performed to obtain a liquid phase.
[0084] Finally, the liquid phase and the solid phase are fully and evenly stirred at a mass ratio of 0.5:1 to obtain an anti-collapse injectable silicon-calcium-based self-curing material.
[0085] The following are performance characteristics of each embodiment and comparative example:
[0086] In order to demonstrate the superiority of the material of the present invention, the present invention tests the injection characteristics, anti-collapse, curing time, and apatite mineralization performance of the prepared calcium-silicon-based self-curing material.
[0087] Injection performance measurement: The calcium-silicon-based self-curing material prepared by the present invention is loaded into a syringe and then placed in a universal testing machine for testing, with the loading speed and maximum load set to 15 mm / min and 100 N, respectively. The injection rate of the self-curing material is the percentage of the weight of the self-curing material after extrusion to the total weight of the original self-curing material.
[0088] The prepared silicon-calcium based self-curing material was tested for injection performance. Figure 1 As shown, the injection performance of the self-curing material in Comparative Example 1 is poor, the injection rate is 72.37%, and the solid and liquid phases are separated during the injection process, and filter pressing occurs. However, the self-curing materials in Comparative Example 2 and Examples 1-3 have excellent injection performance, the injection rate is about 93%, and the injection is smooth and stable during the whole process, and there is no filter pressing problem. This result proves that Pluronic F-127 significantly enhances the injection ability of silicon-calcium-based self-curing materials and gives them good rheological properties. In addition, the introduction of nano-hydroxyapatite will not have an adverse effect on the injection performance of the self-curing material.
[0089] In addition, the present invention measured the injection performance of the self-curing material in Example 2 when it was mixed and placed for different times. The results are as follows: Figure 2 As shown in the figure, the injection rate of the self-curing material still reaches more than 90% after being placed for 15 minutes and 30 minutes, showing excellent injection ability. This result shows that the self-curing material of the present invention has a long working time and maintains a high injection rate. In addition, Figure 3 It can be seen that the self-curing materials in Examples 4 to 7 have excellent injection properties, the self-curing materials are extruded smoothly, and there is no filter pressing phenomenon during the injection process.
[0090] Anti-collapse performance test: The calcium-silicon-based self-curing material prepared by the present invention is loaded into a syringe and immediately injected into a glass dish containing water, and then placed in a 37° C. water bath for curing. After 10 minutes, the collapse of the self-curing material is observed.
[0091] The prepared material was tested for anti-collapse performance. The results are as follows Figure 4 As shown, the injection of the self-curing material in Comparative Example 1 was intermittent and difficult to be continuously injected for a long period. When it came into contact with water, the particles began to disintegrate. After being immersed in water for 10 minutes, the particle disintegration phenomenon intensified, and more powders disintegrated, showing poor anti-disintegration properties. However, the calcium-silicon-based self-curing material containing Pluronic F-127 and nano-hydroxyapatite exhibited excellent anti-disintegration performance. For example, in Comparative Example 2 and Examples 1-3, the self-curing material maintained a good filament shape when injected into water, without the powder particles disintegrating freely. After immersion, it was still able to maintain the original filament shape, and no obvious particle disintegration occurred. In addition, Figure 5 As shown, the self-curing materials prepared in Examples 4 and 5 have excellent anti-collapse performance, and the self-curing materials do not have obvious powder release and collapse in water, and maintain the initial injection shape. Figure 6 It can be seen that the self-curing materials prepared in Examples 6 and 7 can maintain a good injection shape when injected into water and do not collapse (observation results after 10 minutes). The above results prove the effectiveness of Pluronic F-127 and nano-hydroxyapatite in improving the anti-collapse performance of silicon-calcium based self-curing materials.
[0092] Determination of curing time: The calcium silicon-based self-curing material prepared by the present invention is placed in a mold with a diameter of 8 mm and a height of 2 mm, and then placed in a water bath at 37° C. for curing, and the curing time of the self-curing material is measured by a Vicat apparatus.
[0093] The curing time of Examples 1-3 and Comparative Examples 2-4 was tested, and the results are shown in Table 1. The curing time of the self-curing material in Comparative Example 2 was 290 min, while the curing time of the silicon-calcium-based self-curing material in Examples 1-3 was significantly lower than that of the self-curing material in Comparative Example 2. Compared with Comparative Example 2, 1%-4% nano-hydroxyapatite was introduced into the silicon-calcium-based self-curing material in Examples 1-3, which shows that the introduction of nano-hydroxyapatite can effectively shorten the curing time of the self-curing material and promote the hydration kinetic reaction of the silicon-calcium-based material.
[0094] The results of Comparative Example 2 and Comparative Example 1 demonstrate the anti-collapse effect of Pluronic F-127 in the liquid phase of the present invention. Compared with Examples 1-3, it can be shown that nano-hydroxyapatite can have a good synergistic effect with Pluronic F-127, maintain excellent anti-collapse properties, and nano-hydroxyapatite does not produce adverse effects.
[0095] In addition, in Comparative Example 3, when the mass fraction of tricalcium silicate in the solid phase powder of the calcium silicate-based self-curing material is 60%, its curing time is significantly extended to 302 min, and the curing speed is slowed down, so the content of tricalcium silicate in the solid phase powder needs to be higher than 60%. It can be seen from Comparative Example 4 that when the concentration of Pluronic F-127 in the liquid phase of the calcium silicate-based self-curing material reaches 25%, its curing time is also greatly extended, and the curing kinetics are limited, so the concentration of Pluronic F-127 in the liquid phase should be lower than 25%.
[0096] Table 1 Curing time of self-curing materials
[0097]
[0098] In addition, the phase structure analysis of the hydration product of the silicon-calcium based self-curing material in Example 1 was carried out by XRD. Figure 7 As shown, the material undergoes a typical hydration reaction to generate calcium silicate hydrate (CSH) and calcium hydroxide, and there is also a small amount of tricalcium silicate phase. From this result, it can be seen that the calcium silicate-based material prepared by the present invention can undergo a hydration reaction and gradually solidify, showing good self-solidification performance.
[0099] Apatite mineralization experiment: The calcium-silicon-based self-curing material prepared by the present invention was placed in a mold with a diameter of 8 mm and a height of 2 mm for curing, then demolded and immersed in simulated body fluid (SBF), and the surface thereof was subjected to phase analysis.
[0100] Figure 8 This is the XRD result of the surface of the silicon-calcium-based self-curing material in Example 3 of the present invention after being immersed in SBF solution. It can be seen from the figure that after the material is immersed in SBF, an apatite phase is formed on the surface, which has a good ability to induce apatite deposition and exhibits biological activity.
[0101] As described above, although the present invention has been shown and described with reference to specific preferred embodiments, it should not be construed as limiting the present invention itself. Various changes in form and details may be made without departing from the spirit and scope of the present invention as defined in the appended claims.
Claims
1. An injectable anti-collapse type silicon-calcium based self-curing material, characterized in that: It consists of solid phase and liquid phase components; the solid phase contains tricalcium silicate powder and strontium carbonate powder; the liquid phase at least includes an aqueous solution containing nano hydroxyapatite and Pluronic F-127; the mass ratio of the liquid phase to the solid phase is 0.4-0.6:
1.
2. The injectable anti-collapse type calcium-silicon based self-curing material according to claim 1, characterized in that: In the solid phase, the mass percentage of tricalcium silicate powder is 70% to 90%, the mass percentage of strontium carbonate powder is 10% to 30%, and the sum of the mass percentages of the two is 100%.
3. The injectable anti-collapse type calcium-silicon based self-curing material according to claim 1, characterized in that: In the liquid phase, the mass percentage of nano-hydroxyapatite is 1% to 4%, and the mass percentage of Pluronic F-127 is 17.5% to 22.5%.
4. The injectable anti-collapse type silicon-calcium based self-curing material according to claim 1, characterized in that: The particle size of the tricalcium silicate powder is 0.1-100 μm.
5. The injectable anti-collapse type silicon-calcium based self-curing material according to claim 4, characterized in that: The particle size of the tricalcium silicate powder is 0.1-10 μm.
6. The injectable anti-collapse type silicon-calcium based self-curing material according to claim 1, characterized in that: The liquid phase also contains disodium hydrogen phosphate.
7. The method for preparing the injectable anti-collapse type silicon-calcium based self-curing material according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) mixing tricalcium silicate powder and strontium carbonate powder to obtain a solid phase component; (2) adding Pluronic F-127 to water to dissolve it, and then ultrasonically dispersing nano-hydroxyapatite in the Pluronic F-127 aqueous solution to obtain a liquid phase component; (3) The obtained liquid phase component and solid phase component are uniformly blended in proportion to obtain the injectable anti-collapse type silicon-calcium based self-solidifying material.
8. Use of the injectable anti-collapse type calcium-silicon based self-curing material according to any one of claims 1 to 6 as a dental repair and filling material.