Flash evaporation HDPE non-woven fabric enhanced para-aromatic polyamide composite membrane and preparation method thereof
Through the combination of flash evaporated HDPE nonwoven fabric and para-aromatic polyamide casting liquid, the complex problems of dissolution and preparation of existing separation membrane materials under harsh conditions have been solved, and an efficient, environmentally friendly, and durable separation technology has been achieved, providing A solution with low cost, high permeation flux and high separation accuracy.
Patent Information
- Application Number
- CN202411152121.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-08-21
AI Technical Summary
Existing separation membrane materials are easily soluble under harsh conditions such as high temperatures and organic solvents, and the preparation process is complex and costly, which limits their use in industrial applications.
A method for preparing a flash-evaporated HDPE nonwoven-reinforced para-aromatic polyamide composite membrane is used, by combining the flash-evaporated HDPE non-woven fabric with the para-aromatic polyamide film casting liquid, using weakly polar organic liquid and oxygen plasma The bulk treatment improves the fiber strength, and the porogen is used to adjust the uniformity of the casting liquid to achieve high permeation flux and high separation accuracy.
A composite membrane with excellent performance is prepared, which has high mechanical strength, high temperature resistance, solvent resistance, low dye molecular weight cutoff, high flux, low cost, and is suitable for industrial production under harsh conditions.
Smart Images

Figure CN118767702A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of membranes, and in particular to a flash-evaporated HDPE nonwoven fabric-reinforced para-aromatic polyamide composite membrane and a preparation method thereof. Background Art
[0002] With the development of modern industry, especially in the fields of petrochemicals, paint printing and dyeing, food and pharmaceuticals, the demand for efficient, environmentally friendly and durable separation technologies is growing. Common separation membrane materials are polyacrylonitrile, polyvinylidene fluoride and polyvinyl chloride. Due to their poor physical and chemical stability, they are prone to swelling or even dissolution under harsh conditions such as high temperature and organic solvents, which seriously restricts the service life of membrane materials. Inorganic ceramic membranes have the advantages of high flux, good solvent resistance and long service life, but they have complex preparation processes, high production costs and high brittleness.
[0003] Para-aromatic polyamide molecular chains contain a large number of benzene rings and amide bond structures. The molecular chain segments are in the form of a planar rigid straight chain, with high crystallinity and strong hydrogen bonding ability. The molecular chain contains more polar amide groups, which gives PPTA excellent hydrophilicity, mechanical properties, heat resistance and solvent resistance. It is an ideal material for preparing high-performance separation membranes and can be widely used in sewage separation and purification in the fields of chemical, pharmaceutical, biological, and food. However, due to its "insoluble and infusible" characteristics, it is generally only soluble in a few inorganic acid solutions such as concentrated sulfuric acid, which hinders its application in functional membranes, functional fibers and other fields.
[0004] In the prior art, Chinese invention patent publication number CN104801205A discloses a method for preparing a homogeneous enhanced para-aromatic polyamide hollow fiber membrane. The obtained hollow fiber membrane has a thick outer diameter (>2mm), high membrane component cost, low packing density, poor permeation efficiency, and the problem of easy detachment of the separation layer, which limits its wide application. Chinese invention patent publication numbers CN115532078A and CN113117534A disclose a heterogeneous enhanced para-aromatic polyamide hollow fiber membrane, which can effectively improve the tensile fracture strength of the hollow fiber membrane. However, the former method requires the preparation of solid sulfuric acid particles by a complex and harsh process, and the latter requires precise control of the uniform distribution of filament fibers and embedding in the membrane wall, which puts forward high difficulty requirements for the film forming process and reduces production efficiency. In addition, the surface separation layer of both has a high solid content concentration and poor permeation efficiency, which limits their wide use in practical applications. Summary of the invention
[0005] Therefore, in view of the above problems, the present invention provides a flash HDPE nonwoven fabric reinforced para-aromatic polyamide composite membrane and a preparation method thereof, which solves the defects of the prior art separation membrane preparation process being complex, high cost and ordinary mechanical properties.
[0006] To achieve the above object, the present invention adopts the following technical scheme: a method for preparing a flash-evaporated HDPE nonwoven reinforced para-aromatic polyamide composite film, comprising the following steps:
[0007] (1) Flash-steamed HDPE nonwoven fabric reinforcement: a nonwoven fabric made of fibers produced by flash-steaming high-density polyethylene (HDPE) and then bonded by heat and pressure, and the nonwoven fabric is used as a reinforcement for the composite film; the nonwoven fabric has a gram weight of 50 to 160 g / m 2 , thickness is 25-200μm, average pore size is 1-5μm, porosity is 50-90%, and fracture strength is >50MPa;
[0008] (2) Surface pretreatment of flash-evaporated HDPE nonwoven fabric: using a weakly polar organic liquid to perform an infiltration treatment or an oxygen plasma treatment on the flash-evaporated HDPE nonwoven fabric prepared in step (1), wherein the weakly polar organic liquid is methanol, ethanol, or isopropanol, the infiltration time is 1 to 3 hours, and the oxygen plasma treatment time is 5 to 60 seconds;
[0009] (3) preparing a para-aromatic polyamide casting solution: the para-aromatic polyamide casting solution is prepared by first dissolving the para-aromatic polyamide resin in an inorganic acid solvent at 50 to 90° C. at a speed of more than 600 rpm for 2 to 5 hours, adding porogens in sequence, and then controlling the temperature and continuing to stir at a high speed for 0.5 to 2.5 hours, and vacuum degassing for 1 to 2 hours to obtain a highly uniform para-aromatic polyamide casting solution;
[0010] (4) Preparing a para-aromatic polyamide composite membrane: the para-aromatic polyamide casting solution prepared in step (3) is evenly coated on the surface of the flash-evaporated HDPE non-woven fabric fixed on a heatable glass plate by a manual or automatic scraper, and after being in an air bath for 0 to 120 seconds, it is immersed in a coagulation bath at 0 to 65° C. for curing and forming, thereby obtaining the para-aromatic polyamide composite membrane; the temperature of the heated glass plate is maintained at 50 to 90° C., and the scraping speed is 30 to 100 mm / s; the medium of the coagulation bath is water, or an aqueous solution of the inorganic acid solvent, and the mass fraction of the solvent is 0 to 30%.
[0011] Furthermore, the mass fraction composition of each substance in the para-aromatic polyamide casting solution is: 0.5-5wt% para-aromatic polyamide resin, 6-10wt% porogen, 85-93.5wt% inorganic acid solvent, and the sum of each component is 100wt%.
[0012] Furthermore: the mesh size of the para-aromatic polyamide resin is 50 to 1000 mesh; the porogen is at least one of PEG with an average molecular weight of 200 to 20,000 Da and PVP with an average molecular weight of 8,000 to 58,000 Da, and the two are mixed in a mass ratio of PEG / PVP=10 / 0 to 1 / 1; adding the porogens in sequence means first adding PEG and stirring at high speed for 0.5 to 1 hour, and then adding PVP and stirring at high speed for 0.5 to 1.5 hours.
[0013] Further: the temperature control refers to a temperature of 60 to 80°C.
[0014] Furthermore: the high-speed stirring rate is greater than 1200 rpm.
[0015] Furthermore: the inorganic acid solvent refers to concentrated sulfuric acid with a mass concentration of 93 to 100 wt%.
[0016] A flash-steamed HDPE nonwoven fabric reinforced para-aromatic polyamide composite film is prepared by adopting the above-mentioned method for preparing the flash-steamed HDPE nonwoven fabric reinforced para-aromatic polyamide composite film.
[0017] Furthermore: the average pore size of the composite membrane is 3-50 nm, the thickness is 50-300 μm, the water contact angle is 40-60°, and the pure water flux is 200-1000 L / m 2 / h / bar, organic solvent flux is 40~400L / m 2 / h / bar, a cut-off molecular weight of 3000-60000Da, a dye retention molecular weight as low as 697.7g / mol, and a breaking strength of 50-200MPa; after 3.5 bovine serum albumin-water cycles, the pure water flux recovery rate of the composite membrane after simple water washing is as high as 84%; after the composite membrane is immersed in an organic solvent for one month, the Congo red retention rate is still stable at more than 98%.
[0018] By adopting the above technical solution, the beneficial effects of the present invention are:
[0019] 1. The preparation method of the present invention is based on the adjustment of the existing casting liquid formula, and adopts the method of flash HDPE non-woven fabric reinforcement. The para-aromatic polyamide casting liquid is evenly coated on the surface of the flash HDPE non-woven fabric fixed on a heatable glass plate by a manual or automatic scraper, and the film is formed by a phase inversion method in a coagulation bath under a certain air bath to obtain a flash HDPE non-woven fabric reinforced para-aromatic polyamide composite membrane with excellent performance and low price (low cost, high permeation flux, high separation accuracy and high interface bonding strength).
[0020] 2. Compared with the existing enhanced membrane, the present invention not only maintains the original good properties of the membrane material, but also greatly improves the mechanical strength of the para-aromatic polyamide composite membrane (breaking strength>50MPa); the product has better interface bonding strength, higher peel strength, can be backwashed under high pressure, and can operate stably for a long time under conditions of high temperature (>60°C) and polar aprotic organic solvents (such as DMF, DMSO, NMP).
[0021] 3. By selecting the types of porogens and simply optimizing a series of precise controls and fine operations such as the proportion of porogens, the order of addition, and the preparation conditions, the agglomeration phenomenon in the dissolution process of para-aromatic polyamide resins, PEG, and PVP is avoided, the degradation of resins, and the carbonization degree of porogens are reduced, thereby improving the mixing uniformity of the casting liquid, effectively shortening the dissolution time, and increasing the dissolution rate. The controllable preparation of highly homogeneous and low-concentration para-aromatic polyamide casting liquid can be achieved, and the precise regulation of membrane structure and performance can be achieved. While maintaining high-precision separation, narrower pore size (small pore size and narrow distribution, 3-6nm), low dye retention molecular weight (≥697.7g / mol), high temperature resistance (>60℃), ultra-high flux, solvent resistance, acid and alkali resistance, simple preparation, high packing density and low cost are achieved, thereby meeting the industrial production of demanding special separation fields (such as high temperature, organic solvents, acid and alkali solutions, etc.), and providing a high-efficiency, environmentally friendly and durable separation technology solution for modern industry.
[0022] 4. The para-aromatic polyamide composite membrane of the present invention has the characteristics of super hydrophilicity (contact angle <60°) and excellent anti-pollution performance, and can achieve high flux recovery through simple backwashing.
[0023] 5. Compared with the reinforcement obtained by the limitation of existing supporting materials, which has large pore size, low porosity, thick thickness and poor flexibility, different reinforcement tissue structures are designed through flash evaporation technology to obtain flash-evaporated HDPE non-woven fabrics with excellent mechanical properties, smaller pore size, high porosity, thinner thickness and strong flexibility, which can effectively increase the interfacial bonding force and reduce the penetration of casting liquid into the flash-evaporated HDPE non-woven fabric, thereby increasing the penetration efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a SEM surface morphology image of the flash-evaporated HDPE nonwoven fabric of the present invention;
[0025] Figure 2 The SEM surface morphology and cross-sectional morphology of the composite membrane of the present invention;
[0026] Figure 3 is the pure water flux of the composite membrane of the present invention;
[0027] Figure 4The pore size distribution of the composite membrane prepared in Example 1 of the present invention;
[0028] Figure 5 The organic reagent permeation flux of the composite membrane prepared in Example 1 of the present invention;
[0029] Figure 6 The separation performance of the composite membrane of the present invention for bovine serum albumin, (a) the permeation flux of the composite membrane changing with time, (b) the retention rate of the composite membrane changing with time;
[0030] Figure 7 The anti-pollution performance of the composite membrane prepared in Example 1 of the present invention, wherein (a) is the normalized flux of the composite membrane; and (b) is the flux recovery and the anti-pollution ratio of the composite membrane (after 3 cycles). DETAILED DESCRIPTION
[0031] The specific embodiments of the present invention are given below. The specific embodiments are only used to further illustrate the present invention in detail and do not limit the protection scope of the claims of the present invention.
[0032] refer to Figures 1 to 6 , a flash-steamed HDPE nonwoven fabric-reinforced para-aromatic polyamide composite film and a preparation method thereof, comprising the following steps:
[0033] (1) Flash-evaporated HDPE nonwoven reinforcement: HDPE was dissolved in dichloromethane at 200°C and heated with carbon dioxide at 690,000 cN / cm 2 Saturated treatment under high pressure, the resulting spinning solution is pressed into the air chamber through the spinneret hole to form a bundle of filaments, which are ejected at high speed. The dichloromethane solvent evaporates instantly, and the speed gradient is changed to stretch the filament bundle at a high multiple to form ultra-fine mesh fiber strips. At the same time, an electrostatic method is used to open the filament bundle to maintain a single filament state, and an electrostatic device is used to condense the fibers into a net. This fiber net is hot-rolled to make a flash-steamed HDPE nonwoven fabric;
[0034] The HDPE concentration is controlled at 12% to 13%; the filament fineness is 1000 to 2000d; the high-speed ejection is 10,000 to 11,000 m / min; the single filament fineness of the ultrafine mesh fiber strip is 0.10 to 0.15 dtex; the coagulation speed is 90 to 110 m / min; the flash-steamed HDPE nonwoven fabric has a gram weight of 50 to 160 g / m2, a thickness of 25 to 200 μm, a pore size of 1 to 5 μm, a porosity of 50 to 90%, and a breaking strength of >50 MPa;
[0035] (2) pretreatment of the surface of the flash-evaporated HDPE nonwoven fabric; using a weakly polar organic liquid to perform an infiltration treatment or an oxygen plasma treatment on the flash-evaporated HDPE nonwoven fabric prepared in step (1), wherein the weakly polar organic liquid is methanol, ethanol, or isopropanol, the infiltration time is 1 to 3 hours, and the oxygen plasma treatment time is 5 to 60 seconds;
[0036] (3) preparing a para-aromatic polyamide casting solution; the para-aromatic polyamide casting solution is prepared by first dissolving a para-aromatic polyamide resin in an inorganic acid solvent at 50 to 90° C. at a stirring speed of more than 600 rpm for 2 to 5 hours, adding porogens in sequence, and then controlling the temperature and continuing to stir at a high speed for 0.5 to 2.5 hours, and vacuum degassing for 1 to 2 hours to obtain a highly uniform para-aromatic polyamide casting solution, the mass fraction of which is as follows:
[0037] Para-aromatic polyamide resin 0.5-5wt%;
[0038] Porogen 6-10wt%;
[0039] Inorganic acid solvent 85-93.5wt%, the sum of all components is 100wt%,
[0040] The mesh size of the para-aromatic polyamide resin is 50 to 1000 meshes; the porogen is at least one of PEG with an average molecular weight of 200 to 20000Da and PVP with an average molecular weight of 8000 to 58000Da, and the two are mixed in a mass ratio of PEG / PVP=10 / 0 to 1 / 1; the sequential addition of the porogens refers to first adding PEG and stirring at high speed for 0.5 to 1h, and then adding PVP and stirring at high speed for 0.5 to 1.5h; the temperature control refers to a temperature of 60 to 80°C; the high-speed stirring rate is greater than 1200 rpm; the inorganic acid solvent refers to concentrated sulfuric acid with a mass concentration of 93 to 100wt%;
[0041] (4) preparing a para-aromatic polyamide composite film; applying the prepared para-aromatic polyamide casting liquid evenly to the surface of the flash-evaporated HDPE nonwoven fabric fixed on a heatable glass plate by a manual or automatic scraper, and after being in an air bath for 0 to 120 seconds, immersing the nonwoven fabric in a coagulation bath at 0 to 65° C. to solidify and form the para-aromatic polyamide composite film; the temperature of the heated glass plate is maintained at 50 to 90° C., and the scraping speed is 30 to 100 mm / s; the medium of the coagulation bath is water or an aqueous solution of the inorganic acid solvent, and the mass fraction of the solvent is 0 to 30%.
[0042] Since the flash-evaporated HDPE nonwoven reinforcement will undergo a certain etching phenomenon in the solvent, the immersion time in the casting liquid must be effectively controlled. On the one hand, if the immersion time is too long, the flash-evaporated HDPE nonwoven reinforcement will be severely etched, and the mechanical properties of the composite film will be reduced; on the other hand, if the immersion time is too short, the casting liquid will have a poor infiltration effect on the reinforcement, and the interface bonding strength is not high, which affects the comprehensive performance of the composite film. Therefore, the air gap and the scraping speed jointly determine the infiltration or residence time of the reinforcement in the casting liquid, that is, determine the degree of etching. The present invention recommends an air bath of 0 to 120 seconds and a scraping speed of 30 to 100 mm / s. The comprehensive performance of the composite film obtained under this process condition is better.
[0043] According to the preparation method of the flash-steamed HDPE nonwoven fabric reinforced composite membrane of the present invention, a flash-steamed HDPE nonwoven fabric reinforced para-aromatic polyamide composite membrane can be prepared. The composite membrane has the characteristics of flash spinning film making and liquid crystal spinning film making, can significantly improve the interface bonding strength of the para-aromatic polyamide composite membrane, and at the same time improve the mechanical properties of the membrane.
[0044] Any matters not described in the present invention are applicable to the prior art.
[0045] Specific embodiments of the present invention are given below.
[0046] Example 1
[0047] A flash-evaporated HDPE nonwoven fabric-reinforced para-aromatic polyamide composite film and a preparation method thereof, comprising the following steps:
[0048] (1) Preparation of reinforcement: HDPE with a concentration of 12% was dissolved in dichloromethane at 200°C and heated to 690,000 cN / cm 2 Saturated treatment under high pressure, the resulting spinning solution is pressed into the air chamber through the spinneret hole to form a bundle of filaments with a fineness of 1200d, and is ejected at a high speed of 11,000 m / min. The dichloromethane solvent evaporates instantly, and the filament bundle is stretched at a high multiple by using the speed gradient change to form an ultra-fine mesh fiber strip with a single filament fineness of 0.14d. At the same time, an electrostatic method is used to open the filament bundle to maintain a single filament state, and an electrostatic device is used to condense the fibers into a net at a speed of 100m / min. After hot rolling, it is made into a flash-steamed HDPE non-woven fabric with a gram weight of 50g / m2, a thickness of 90μm, a pore size of 3μm, a porosity of 60%, and a breaking strength of 60MPa;
[0049] (2) impregnating the flash-evaporated HDPE nonwoven fabric prepared in step (1) with ethanol for 1 h;
[0050] (3) 1.5 wt% para-aromatic polyamide resin (100 mesh) was first dissolved in 98 wt% concentrated sulfuric acid at 70°C at 800 rpm for 4 h, then 10 wt% PEG (molecular weight 2000) was added, and then 1200 rpm was stirred for 0.5 h, and then PVP (K30, molecular weight 40000) was added in sequence, and the two were mixed at a mass ratio of PEG / PVP = 9:1, and then the high-speed stirring was continued at 65°C for 0.5 h, and then vacuum degassing was performed for 2 h to obtain a highly uniform para-aromatic polyamide casting solution;
[0051] (4) preparing a para-aromatic polyamide composite membrane; the prepared para-aromatic polyamide casting liquid is evenly coated on the surface of a flash-evaporated HDPE nonwoven fabric fixed on a 65°C glass plate by a manual or automatic scraper at a scraping speed of 75 mm / s, and after being placed in an air bath for 15 seconds, the nonwoven fabric is immersed in a coagulation bath (water) at 30°C for curing to obtain the para-aromatic polyamide composite membrane.
[0052] According to measurement, the composite membrane obtained in this embodiment has a room temperature pure water flux of 585.1LMH / bar at 1 bar, a DMF solvent flux of 219.8LMH / bar, and bovine serum albumin is still greater than 99.0% after being immersed in DMF solvent for 30 days.
[0053] Comparative Example 1
[0054] A para-aromatic polyamide composite film with PET non-woven fabric as a reinforcement was prepared as a comparative example of the present invention: according to the casting solution formula of Example 1, the preparation process was exactly the same as that of Example 1.
[0055] After testing, the flux of pure water at room temperature is 64.9LMH / bar at 1 bar, and the flux of DMF solvent is 21.4LMH / bar. After soaking in DMF solvent for 30 days, the bovine serum albumin is still >99.0%.
[0056] Example 2
[0057] It is basically the same as Example 1, except that 10 wt % of porogens PEG (molecular weight 2000) and PVP (K30, molecular weight 40000) (PEG / PVP=4:1) are added.
[0058] The measured flux of the composite membrane obtained in this embodiment at room temperature pure water under 1 bar is 760.4 + 4.5LMH / bar, DMF solvent flux is 286.6LMH / bar, after immersion in DMF solvent for 30 days, BSA is still >99.0%.
[0059] Example 3
[0060] It is basically the same as Example 1, except that 10 wt % of porogens PEG (molecular weight 2000) and PVP (K30, molecular weight 40000) (PEG / PVP=7:3) are added.
[0061] According to the measurement, the composite membrane obtained in this embodiment has a room temperature pure water flux of 930.0LMH / bar at 1 bar, a DMF solvent flux of 343.8LMH / bar, and bovine serum albumin is still greater than 99.0% after being immersed in DMF solvent for 30 days.
[0062] Example 4
[0063] It is basically the same as Example 1, except that 10 wt % of porogens PEG (molecular weight 2000) and PVP (K30, molecular weight 40000) (PEG / PVP=10:0) are added.
[0064] According to measurement, the composite membrane obtained in this embodiment has a room temperature pure water flux of 322.2LMH / bar at 1 bar, a DMF solvent flux of 121.1LMH / bar, and bovine serum albumin is still greater than 99.0% after being immersed in DMF solvent for 30 days.
[0065] Example 5
[0066] Characterization of the composite membrane dye desalination performance: According to Example 1, the composite membrane was subjected to five dye separation performance tests, namely, Bengal rose red (RB, 1017.6 g / mol), Coomassie brilliant blue (BBR, 826.0 g / mol), Congo red (CR, 697.7 g / mol), acid fuchsin (AF, 584.5 g / mol), and methyl orange (MO, 327.3 g / mol). The composite membrane showed a retention rate of more than 99.4% for dyes with a molecular weight greater than 697.7 g / mol, and even 56.2% of MO with a molecular weight of 327.3 g / mol was retained.
[0067] Example 6
[0068] Characterization of the anti-fouling property of the composite membrane: The obtained composite membrane was subjected to a bovine serum albumin cycle test as described in Example 1. The test showed that after simple washing with clean water, the recovery rate of pure water flux of the composite membrane was as high as 84%, and after 3.5 cycles, it was still superior to commercial PES and PVDF membranes.
[0069] Although the present invention has been specifically shown and described in conjunction with the preferred embodiments, it should be understood by those skilled in the art that various changes may be made to the present invention in form and details without departing from the spirit and scope of the present invention as defined by the appended claims, all of which are within the scope of protection of the present invention.
Claims
1. A method for preparing a flash-evaporated HDPE nonwoven reinforced para-aromatic polyamide composite film, It is characterized in that Use the following steps: (1) Flash-steamed HDPE nonwoven fabric reinforcement: a nonwoven fabric made of fibers produced by flash-steaming high-density polyethylene (HDPE) and then bonded by heat and pressure, and the nonwoven fabric is used as a reinforcement for the composite film; the nonwoven fabric has a gram weight of 50 to 160 g / m 2 , thickness is 25-200μm, average pore size is 1-5μm, porosity is 50-90%, and fracture strength is >50MPa; (2) Surface pretreatment of flash-evaporated HDPE nonwoven fabric: using a weakly polar organic liquid to perform an infiltration treatment or an oxygen plasma treatment on the flash-evaporated HDPE nonwoven fabric prepared in step (1), wherein the weakly polar organic liquid is methanol, ethanol, or isopropanol, the infiltration time is 1 to 3 hours, and the oxygen plasma treatment time is 5 to 60 seconds; (3) preparing a para-aromatic polyamide casting solution: the para-aromatic polyamide casting solution is prepared by first dissolving the para-aromatic polyamide resin in an inorganic acid solvent at 50 to 90° C. at a speed of more than 600 rpm for 2 to 5 hours, adding porogens in sequence, and then controlling the temperature and continuing to stir at a high speed for 0.5 to 2.5 hours, and then vacuum degassing for 1 to 2 hours to obtain a highly uniform para-aromatic polyamide casting solution; (4) Preparing a para-aromatic polyamide composite membrane: the para-aromatic polyamide casting solution prepared in step (3) is evenly coated on the surface of the flash-evaporated HDPE non-woven fabric fixed on a heatable glass plate by a manual or automatic scraper, and after being in an air bath for 0 to 120 seconds, it is immersed in a coagulation bath at 0 to 65° C. for curing and forming, thereby obtaining the para-aromatic polyamide composite membrane; the temperature of the heated glass plate is maintained at 50 to 90° C., and the scraping speed is 30 to 100 mm / s; the medium of the coagulation bath is water, or an aqueous solution of the inorganic acid solvent, and the mass fraction of the solvent is 0 to 30%.
2. The method for preparing a flash-evaporated HDPE nonwoven reinforced para-aromatic polyamide composite film according to claim 1, Features: The mass fraction composition of the substances in the para-aromatic polyamide casting solution is: 0.5-5wt% of para-aromatic polyamide resin, 6-10wt% of porogen, 85-93.5wt% of inorganic acid solvent, and the sum of the components is 100wt%.
3. The method for preparing a flash-evaporated HDPE nonwoven reinforced para-aromatic polyamide composite film according to claim 1, Features: The mesh number of the para-aromatic polyamide resin is 50 to 1000 meshes; the porogen is at least one of PEG with an average molecular weight of 200 to 20,000 Da and PVP with an average molecular weight of 8,000 to 58,000 Da, and the two are mixed in a mass ratio of PEG / PVP=10 / 0 to 1 / 1; adding the porogens in sequence means first adding PEG and stirring at high speed for 0.5 to 1 hour, and then adding PVP and stirring at high speed for 0.5 to 1.5 hours.
4. The method for preparing a flash-evaporated HDPE nonwoven reinforced para-aromatic polyamide composite film according to claim 1, Features: The temperature control refers to a temperature of 60 to 80°C.
5. The method for preparing a flash-evaporated HDPE nonwoven reinforced para-aromatic polyamide composite film according to claim 1, Features: The high-speed stirring rate is greater than 1200 revolutions / min.
6. The method for preparing a flash-evaporated HDPE nonwoven reinforced para-aromatic polyamide composite film according to claim 1, Features: The inorganic acid solvent refers to concentrated sulfuric acid with a mass concentration of 93-100wt%.
7. A flash-steamed HDPE nonwoven reinforced para-aromatic polyamide composite film, Features: The composite film is prepared by the method for preparing a flash-evaporated HDPE nonwoven fabric-reinforced para-aromatic polyamide composite film as described in any one of claims 1 to 6.
8. The flash-steamed HDPE nonwoven reinforced para-aromatic polyamide composite film according to claim 7, Features: The composite membrane has an average pore size of 3 to 50 nm, a thickness of 50 to 300 μm, a water contact angle of 40 to 60°, and a pure water flux of 200 to 1000 L / m 2 / h / bar, organic solvent flux is 40~400L / m 2 / h / bar, a cut-off molecular weight of 3000-60000Da, a dye retention molecular weight as low as 697.7g / mol, and a breaking strength of 50-200MPa; after 3.5 bovine serum albumin-water cycles, the composite membrane has a pure water flux recovery rate of up to 84% after simple water washing; after the composite membrane has been immersed in an organic solvent for one month, the Congo red retention rate is still stable at more than 98%.
Citation Information
Patent Citations
Preparation method of aromatic polyamide hollow fiber porous membrane
CN104353372A
Preparation method of fiber-reinforced aromatic polyamide hollow fiber membrane and hollow fiber membrane prepared by preparation method
CN113117534A
PE / HDPE composite flash non-woven fabric and preparation method thereof
CN114775170A
Polyethylene hollow fiber composite membrane as well as preparation method and application thereof
CN117619170A
Method for preparing aromatic polyamide porous hollow fiber membrane
US20160001234A1
Cited By
Polyvinylidene fluoride hollow fiber ultrafiltration membrane and preparation method thereof
CN122516856A