Aerogel composite material as well as preparation method and application thereof

By loading MXene nanosheets and vinyl polymers on the surface of graphene aerogel, an aerogel composite material with super-hydrophobic, super-oil-absorbing properties and demulsifying ability was prepared, which solved the problem of low oil-water separation efficiency of emulsified oil and achieved Efficient separation and improved material stability are suitable for large-scale production.

CN118767883APending Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202310372400.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing oil-water separation technology is difficult to effectively handle complex emulsified oil. Traditional adsorption materials have low or ineffective separation efficiency in emulsified oil-oil-water, and the prepared materials have poor stability and are difficult to produce on a large scale.

Method used

Graphene airgel composite materials are prepared by loading MXene nanosheets and in-situ grown vinyl polymers on the surface of the graphene airgel, combined with hydrothermal reaction and freeze-drying technology, to form a super-hydrophobic, super-oil-absorbing and destructible composite material. Milk-capable airgel composites.

Benefits of technology

Efficient oil-water separation of emulsified oil is achieved. The material has low density, high specific surface area, excellent mechanical properties and stability, and is suitable for large-scale production and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767883A_ABST
    Figure CN118767883A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of oil-water separation, and discloses an aerogel composite material as well as a preparation method and application thereof. The aerogel composite material comprises graphene aerogel, an MXene nanosheet loaded on the surface of the graphene aerogel, and a vinyl polymer grown on the MXene nanosheet in situ, the graphene aerogel contains reduced graphene oxide, polydopamine and an iron element. The aerogel composite material has the advantages of low density, high specific surface area, excellent mechanical property and super-hydrophobic and super-oil absorption performance, has demulsification capability, and can realize oil-water separation of emulsified oil.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil-water separation, and in particular to an aerogel composite material and a preparation method and application thereof. Background Art

[0002] Marine crude oil spills and industrial wastewater discharges produce a large amount of oil and organic pollutant waste liquids, causing serious ecological and human health problems. Effectively solving the environmental pollution problems caused by oil and organic waste liquids and realizing recycling and reuse has always been one of the difficulties that people urgently need to solve. Traditional solutions to oil pollution problems are mainly through biological methods, flotation methods, flocculation methods, membrane separation methods and adsorption methods. Among them, the adsorption method has become a hot spot for research and application because it has the advantages of simple operation, environmental friendliness, high efficiency, low cost and no secondary pollution when dealing with oil leakage and recycling and reuse.

[0003] Graphene is a two-dimensional material consisting of one or more layers of carbon atoms arranged in six-membered rings with a length of 2630 m 2 / g theoretical specific surface area and excellent transport performance. The ultra-large specific surface area combined with the inherent hydrophobicity of graphene makes graphene a highly competitive material in the field of oil-water separation. To date, the most promising way to use graphene for oil-water separation is to construct a porous structure and perform hydrophobic modification. Graphene-based foams, sponges, aerogels and hydrogels are some of the three-dimensional graphene-derived structures reported in the literature. Many researchers have applied the unique properties of these three-dimensional structures in the adsorption process and proved that they have superior adsorption capacity. Among them, three-dimensional graphene aerogels have a fixed macroscopic block structure, which is easy to recycle, and also have the characteristics of low density, high porosity and flexible structural regulation.

[0004] In actual oil-water mixtures, there are several different forms of dispersion depending on the size of the dispersed phase particles: floating oil (particle size > 150μm), dispersed oil (particle size 20-150μm), emulsified oil (particle size 0.1-20μm) and dissolved oil. Complex oil-water mixed systems often contain a large amount of surfactants. Under this condition, the oil dispersed phase is easy to produce small droplets of small size and stable properties in the water continuous phase to form an emulsion, which is emulsified oil. However, current adsorption materials including graphene aerogel can only effectively separate floating oil on the water surface or dispersed oil in water. The efficiency of oil-water separation for complex emulsified oil is extremely low or even ineffective. Therefore, how to simply and effectively remove emulsified oil has become the focus and difficulty of oil-water separation research.

[0005] Patent application CN114681953A discloses a method for preparing an asymmetric wettability wood membrane capable of converting separation of oil-water emulsions. The asymmetric wettability wood membrane capable of converting separation of oil-water emulsions has superhydrophilicity / underwater superoleophobicity on one side and superhydrophobicity / superoleophilicity on the other side; the wood membrane can separate oil-in-water and oil-in-water emulsions. However, the asymmetric wettability wood membrane prepared by this method has the disadvantages of poor stability, poor mechanical properties, poor durability, etc., and can only meet laboratory applications, and cannot yet achieve large-scale industrial production of the membrane.

[0006] Patent application CN112691649A discloses an organosilicon foam with in-situ demulsification and adsorption functions and its application in oil-water separation. It is prepared by the following steps: after uniformly mixing a single-end unsaturated polyether monomer and a transition metal complex catalyst, adding dopamine modified foam impregnated with a 2-bromoisobutyryl bromide dichloromethane solution, performing an atom transfer radical polymerization reaction, adding a single-end unsaturated organosilicon during the reaction, and obtaining the foam with in-situ demulsification and adsorption functions. However, transition metal complexes will remain during the atom transfer radical polymerization process, and are difficult to purify, which easily leads to polymer aging. The presence of water in the oil-water separation process exacerbates the aging process and reduces the stability of the material. Summary of the invention

[0007] The purpose of the present invention is to overcome the problems of unstable demulsification effect and easy penetration in the prior art, poor cyclic mechanical stability of the material, and difficulty in large-scale production, and to provide an aerogel composite material and a preparation method and application thereof.

[0008] In order to achieve the above object, the present invention provides an aerogel composite material on one hand, wherein the aerogel composite material comprises: a graphene aerogel, a MXene nanosheet supported on the surface of the graphene aerogel, and a vinyl polymer in situ grown on the MXene nanosheet;

[0009] The graphene aerogel contains reduced graphene oxide, polydopamine and iron element.

[0010] Preferably, the contact angle of the aerogel composite material is ≥143°;

[0011] Preferably, the oil absorption rate of the aerogel composite material is ≥115 g / g.

[0012] A second aspect of the present invention provides a method for preparing an aerogel composite material, the method comprising the following steps:

[0013] (1) mixing graphene oxide, dopamine, iron salt and water, and then performing a hydrothermal reaction and freeze drying to obtain a graphene aerogel;

[0014] (2) soaking the graphene aerogel in a MXene dispersion, taking it out, and then freeze-drying it to obtain a MXene-modified graphene aerogel;

[0015] (3) mixing the MXene-modified graphene aerogel with a solution containing a vinyl silane coupling agent to react, thereby obtaining a MXene-modified graphene aerogel modified with a silane coupling agent;

[0016] (4) In the presence of an initiator, the MXene-modified graphene aerogel modified with a silane coupling agent is mixed with a vinyl monomer for reaction.

[0017] Preferably, in step (1), the weight ratio of graphene oxide, dopamine and iron salt is 10-20:1-5:1.

[0018] Preferably, in step (1), the conditions for the hydrothermal reaction include: temperature of 100-140° C.; time of 10-20 h.

[0019] Preferably, in step (2), the concentration of MXene in the MXene dispersion is 0.02-0.1 mg / mL.

[0020] Preferably, in step (2), the liquid-to-solid ratio of the MXene dispersion to the graphene aerogel is 10-100 mL / g.

[0021] Preferably, in step (2), the soaking time is 1-60 min.

[0022] Preferably, in step (3), the weight ratio of MXene-modified graphene aerogel to vinyl silane coupling agent is 1:1-10.

[0023] Preferably, in step (3), the concentration of the vinyl silane coupling agent in the solution containing the vinyl silane coupling agent is 4-8% by weight.

[0024] Preferably, in step (3), the vinyl silane coupling agent is selected from one or more of vinyl trimethoxysilane, vinyl trichlorosilane, vinyl tri-tert-butoxysilane and vinyl triethoxysilane.

[0025] Preferably, in step (3), the reaction conditions include: temperature of 80-120° C.; time of 1-4 h.

[0026] Preferably, the specific process of step (4) includes: mixing the MXene-modified graphene aerogel modified by a silane coupling agent with a solution containing a vinyl monomer and an initiator for reaction.

[0027] Preferably, the concentration of the vinyl monomer in the solution containing the vinyl monomer and the initiator is 0.05-0.5 mg / mL.

[0028] Preferably, the concentration of the initiator in the solution containing the vinyl monomer and the initiator is 3-5 mg / mL.

[0029] Preferably, in step (4), the weight ratio of the MXene-modified graphene aerogel modified by the silane coupling agent to the vinyl monomer is 200-1200:1.

[0030] Preferably, in step (4), the vinyl monomer is styrene or divinylbenzene.

[0031] Preferably, in step (4), the reaction conditions include: temperature of 80-140° C. and time of 12-36 h.

[0032] The third aspect of the present invention provides an aerogel composite material prepared by the method described above.

[0033] A fourth aspect of the present invention provides use of the aerogel composite material described above in oil-water separation.

[0034] Complex oil-water mixed systems often contain a large amount of surfactants. Under this condition, the oil dispersed phase is prone to produce small droplets of small size and stable properties in the water continuous phase to form emulsified oil. Existing oil-water separation adsorbents can only target floating oil and dispersed oil in water, but will lose the effect of oil-water separation in emulsified oil systems.

[0035] The present invention further studies the adsorption material and discloses an aerogel composite material. The aerogel composite material has low density, high specific surface area, excellent mechanical properties, super hydrophobic and super oil absorption properties, and has demulsification ability, and can achieve oil-water separation of emulsified oil. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 is a schematic diagram of the SEM characterization results in Test Example 1;

[0037] Figure 2 This is a picture taken of the demulsification effect in Test Example 2;

[0038] Figure 3 This is a picture of the product prepared in Example 3 when the contact angle test was performed;

[0039] Figure 4 It is a schematic diagram of the device for measuring the density, porosity and open porosity of the products prepared in the embodiments and comparative examples in Test Example 3.

[0040] Description of Reference Numerals

[0041] 1 Balance pan; 2 Placement area for samples to be tested; 3 Weighing pan in liquid; 4 Tray; 5 Placement area for working liquid; 6 Liquid container. DETAILED DESCRIPTION

[0042] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0043] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0044] In one aspect, the present invention provides an aerogel composite material, the aerogel composite material comprising: a graphene aerogel, a MXene nanosheet supported on the surface of the graphene aerogel, and a vinyl polymer in situ grown on the MXene nanosheet;

[0045] The graphene aerogel contains reduced graphene oxide, polydopamine and iron element.

[0046] Preferably, the contact angle of the aerogel composite material is ≥143°;

[0047] Preferably, the oil absorption rate of the aerogel composite material is ≥115 g / g.

[0048] Preferably, the compressive strength of the aerogel composite material is ≥2.9 MPa.

[0049] The gel composite material provided by the present invention has the characteristics of low density, high specific surface area, high mechanical strength, super hydrophobic and super oleophilic, and has demulsification ability, which solves the problem of oil-water separation of emulsified oil that cannot be solved by the prior art, is easy to operate, and has broad application prospects.

[0050] A second aspect of the present invention provides a method for preparing an aerogel composite material, the method comprising the following steps:

[0051] (1) mixing graphene oxide, dopamine, iron salt and water, and then performing a hydrothermal reaction and freeze drying to obtain a graphene aerogel;

[0052] (2) soaking the graphene aerogel in a MXene dispersion, taking it out, and then freeze-drying it to obtain a MXene-modified graphene aerogel;

[0053] (3) mixing the MXene-modified graphene aerogel with a solution containing a vinyl silane coupling agent to react, thereby obtaining a MXene-modified graphene aerogel modified with a silane coupling agent;

[0054] (4) In the presence of an initiator, the MXene-modified graphene aerogel modified with a silane coupling agent is mixed with a vinyl monomer for reaction.

[0055] In the present invention, graphene aerogel is first prepared by a hydrothermal method; secondly, two-dimensional nanosheets MXene are fixed on the surface of graphene aerogel by freeze drying, and nanostructures are constructed on the surface; then, the abundant hydroxyl groups on the surface of MXene react with vinyl silane coupling agents to introduce vinyl groups on the surface of graphene aerogel; and then, super-hydrophobic polymer long chains are generated in situ on the surface of graphene aerogel by free radical polymerization. The aerogel composite material prepared in this way has low density, high specific surface area, excellent mechanical properties, super-hydrophobic and super-oil absorption properties, and has demulsification ability, which can realize oil-water separation of emulsified oil.

[0056] The tiny oil particles in the emulsified oil are wrapped by water molecules. The traditional hydrophobic and lipophilic adsorption materials for oil-water separation can only contact the water molecules but not the oil molecules wrapped by the water molecules. Therefore, the traditional adsorption materials cannot absorb the oil droplets, and the oil-water separation effect is not ideal. The demulsification principle of the aerogel composite material described in the present invention is: the surface of the material has a nano-scale rough structure. When the water-in-oil molecule enters the interior of the aerogel, it will collide with the inner surface of the aerogel in the pore structure. During the collision, the nano-rough structure of the inner surface will be inserted into the water molecules to contact the small oil droplets. Therefore, the tiny oil droplets will gradually gather on the surface of the nano-structure to form large oil droplets, and the water molecules will pass through the aerogel pores, thereby achieving the effect of oil-water separation of the emulsified oil.

[0057] In a preferred embodiment, in step (1), the weight ratio of graphene oxide, dopamine and iron salt is 10-20:1-5:1.

[0058] In a specific embodiment, in step (1), the weight ratio of graphene oxide to iron salt can be 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1 or 20:1.

[0059] In a specific embodiment, in step (1), the weight ratio of dopamine to iron salt can be 1:1, 2:1, 3:1, 4:1 or 5:1.

[0060] In the method of the present invention, in step (1), the graphene oxide can be prepared according to conventional methods in the art or commercially available.

[0061] In the method of the present invention, the iron salt can be a conventional choice in the art. The role of the iron salt is to provide iron ions, which are conducive to the uniform dispersion of graphene oxide sheets. The oxygen-containing functional groups on the graphene oxide can coordinate with the iron ions to form a three-dimensional structure, and the iron ions can form an electrostatic force with the MXene in the next step, so that the MXene is attached to the surface of the graphene aerogel. In a specific embodiment, the iron salt is selected from one or more of ferric chloride hexahydrate, ferric sulfate heptahydrate and ferric nitrate nonahydrate.

[0062] In the method described in the present invention, in step (1), dopamine can form polydopamine through self-polymerization to improve the stability of the gel structure.

[0063] In a preferred embodiment, in step (1), the specific process of mixing graphene oxide, dopamine, iron salt and water includes: dispersing graphene oxide and mixing with water and ultrasonically treating, then adding dopamine aqueous solution, stirring, and then adding iron salt under stirring.

[0064] In a preferred embodiment, in step (1), the hydrothermal reaction is carried out in a high-pressure reactor lined with polytetrafluoroethylene.

[0065] In the present invention, in step (1), the conditions of the hydrothermal reaction include: a temperature of 100-140° C., preferably 100-130° C.; and a time of 10-20 h, preferably 10-15 h.

[0066] In a specific embodiment, in step (1), the temperature of the hydrothermal reaction can be 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C or 140°C; the time of the hydrothermal reaction can be 10h, 1h, 12h, 13h, 14h or 15h.

[0067] In the method of the present invention, in step (1), the freeze drying can be performed according to conventional operations in the art. In a preferred embodiment, the freeze drying conditions include: temperature of -50°C, vacuum degree of 10 Pa, and time of 20 hours.

[0068] In the method described in the present invention, the addition of MXene can construct a micro-nano structure on the surface of the aerogel, and the surface of MXene has abundant hydroxyl groups, which can provide a secondary reaction platform for the introduction of vinyl siloxane.

[0069] In a preferred embodiment, in step (2), the concentration of MXene in the MXene dispersion is 0.02-0.1 mg / mL. Specifically, the concentration of MXene can be 0.02 mg / mL, 0.03 mg / mL, 0.04 mg / mL, 0.05 mg / mL, 0.06 mg / mL, 0.07 mg / mL, 0.08 mg / mL, 0.09 mg / mL or 0.1 mg / mL.

[0070] In the present invention, in step (2), the liquid-to-solid ratio of the MXene dispersion to the graphene aerogel may be 10-100 mL / g, preferably 20-80 mL / g, and more preferably 50-60 mL / g.

[0071] In a specific embodiment, the liquid-to-solid ratio of the MXene dispersion to the graphene aerogel can be 10 mL / g, 20 mL / g, 30 mL / g, 40 mL / g, 50 mL / g, 60 mL / g, 70 mL / g, 80 mL / g, 90 mL / g or 100 mL / g.

[0072] In a preferred embodiment, in step (2), the MXene dispersion may be a MXene aqueous dispersion.

[0073] In a preferred embodiment, in step (2), the MXene is selected from Ti 3 C 2 T x 、Ti 2 CT x or Ti 3 CNT x .

[0074] In the present invention, in step (2), the soaking time may be 1-60 min, preferably 5-50 min, and more preferably 5-20 min.

[0075] In a specific embodiment, in step (2), the soaking time can be 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min.

[0076] In the method of the present invention, in step (2), there is no special requirement for freeze-drying conditions, and the freeze-drying can be performed according to conventional operations in the art. In a specific embodiment, the freeze-drying conditions include: temperature of -50°C, vacuum degree of 10 Pa, and time of 24 hours.

[0077] In the method of the present invention, in step (3), the weight ratio of the MXene-modified graphene aerogel to the vinyl silane coupling agent in the solution containing the vinyl silane coupling agent can be 1:1-10, preferably 1:1-5, and more preferably 1:2-4.

[0078] In a specific embodiment, in step (3), the weight ratio of the MXene-modified graphene aerogel to the vinyl silane coupling agent in the solution containing the vinyl silane coupling agent can be 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10.

[0079] In a preferred embodiment, in step (3), the concentration of the vinyl silane coupling agent in the solution containing the vinyl silane coupling agent is 4-8% by weight, and specifically, it can be 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5% or 8% by weight.

[0080] In a preferred embodiment, in step (3), the solvent used in the solution containing the vinyl silane coupling agent may be a mixed solution of sodium hydroxide aqueous solution and ethanol, wherein the concentration of the sodium hydroxide aqueous solution is 1.33 g / mL, and the volume ratio of the sodium hydroxide aqueous solution to the ethanol is 0.075:1.

[0081] In a preferred embodiment, in step (3), the vinyl silane coupling agent is selected from one or more of vinyl trimethoxysilane, vinyl trichlorosilane, vinyl tri-tert-butoxysilane and vinyl triethoxysilane.

[0082] In the method of the present invention, in step (3), the reaction conditions include: temperature of 80-120° C., preferably 90-110° C.; time of 1-4 h, preferably 1.5-3.5 h.

[0083] In a specific embodiment, in step (3), the reaction temperature can be 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C or 120°C; the reaction time can be 1h, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h.

[0084] In the method described in the present invention, in step (4), long polymer chains are generated in situ on the surface of the material by free radical polymerization, which can control the molecular weight of the polymer and a narrower molecular weight distribution, so that the hydrophobic long-chain polymer has a considerable degree of polymerization, which can make the hydrophobicity of the aerogel composite material more stable and uniform.

[0085] Preferably, the specific process of step (4) includes: mixing the MXene-modified graphene aerogel modified by a silane coupling agent with a solution containing a vinyl monomer and an initiator for reaction.

[0086] In a preferred embodiment, the concentration of the vinyl monomer in the solution containing the vinyl monomer and the initiator is 0.05-0.5 mg / mL. Specifically, it can be 0.05 mg / mL, 0.06 mg / mL, 0.07 mg / mL, 0.08 mg / mL, 0.1 mg / mL, 0.12 mg / mL, 0.14 mg / mL, 0.15 mg / mL, 0.16 mg / mL, 0.18 mg / mL, 0.2 mg / mL, 0.3 mg / mL, 0.4 mg / mL or 0.5 mg / mL.

[0087] In a preferred embodiment, the concentration of the initiator in the solution containing the vinyl monomer and the initiator is 3-5 mg / mL, specifically, 3 mg / mL, 3.5 mg / mL, 4 mg / mL, 4.5 mg / mL or 5 mg / mL.

[0088] In a preferred embodiment, in step (4), the initiator used is an oil-soluble initiator. In a specific embodiment, the initiator can be azobisisobutyronitrile, azobisisoheptanenitrile or benzoyl peroxide.

[0089] In a preferred embodiment, the solvent used in the solution containing the vinyl monomer and the initiator is usually an organic solvent, such as methanol, diethyl ether, ethyl acetate, etc.

[0090] In the method of the present invention, in step (4), the weight ratio of the MXene-modified graphene aerogel modified by the silane coupling agent to the vinyl monomer can be 200-1200:1.

[0091] In a specific embodiment, in step (4), the weight ratio of the MXene-modified graphene aerogel modified with a silane coupling agent to the vinyl monomer can be 200:1, 240:1, 300:1, 400:1, 500:1, 600:1, 700:1, 800:1, 900:1, 1000:1 or 1200:1.

[0092] In a preferred embodiment, in step (4), the vinyl monomer is acrylic acid, styrene or divinylbenzene.

[0093] In a preferred embodiment, in step (4), the reaction conditions include: a temperature of 80-140°C and a time of 12-36 hours. Specifically, the temperature may be 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C or 140°C; and the time may be 12h, 14h, 16h, 18h, 20h, 22h, 24h, 26h, 28h, 30h, 32h, 34h or 36h.

[0094] In a preferred embodiment, step (4) further comprises: washing and drying the material obtained after the reaction. More preferably, the detergent used for washing is ethanol, and the drying method is vacuum drying. There are no special requirements for the vacuum drying conditions, and it can be carried out in a conventional manner in the art. In a specific embodiment, the vacuum drying conditions include: a temperature of 60°C and a vacuum degree of -0.1MPa.

[0095] The third aspect of the present invention provides an aerogel composite material prepared by the method described above.

[0096] A fourth aspect of the present invention provides use of the aerogel composite material described above in oil-water separation.

[0097] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.

[0098] In the following examples and comparative examples, graphene oxide was purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.; ferric chloride hexahydrate (FeCl 3 6H 2 O), ferric sulfate heptahydrate and ferric nitrate nonahydrate were purchased from Tianjin Baishi Chemical Co., Ltd., China; Ti 3 C 2 T x 、Ti 2 CT x The dispersion was purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.; dopamine was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; vinyl triethoxysilane was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; divinylbenzene and styrene were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; azobisisobutyronitrile was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; anhydrous ethanol was purchased from Sinopharm Chemical Reagent Co., Ltd.; and ethyl acetate was purchased from Sinopharm Chemical Reagent Co., Ltd. Other reagents, unless otherwise specified, were commercially available products.

[0099] Example 1

[0100] The aerogel composite material S1 is prepared, and the specific process includes the following steps:

[0101] (1) 30 mg of graphene oxide (GO) was dispersed in 10 mL of water and ultrasonically treated for 4 h to obtain a GO dispersion. Then, 0.6 mL of dopamine aqueous solution (concentration: 20 mg / mL) was added to the GO dispersion and stirred for 10 min. Subsequently, 0.25 mL of iron salt aqueous solution (iron salt: FeCl 3 6H 2 O, with a concentration of 10 mg / mL) and stirred for 1 hour, then the mixture was transferred to a polytetrafluoroethylene-lined stainless steel autoclave, and hydrothermally treated at 120° C. for 12 hours to form a gel-like product, and then the gel-like product was transferred to a freeze dryer and treated at -50° C. and 10 Pa for 24 hours to remove internal moisture to obtain a graphene aerogel; wherein the weight ratio of graphene oxide, dopamine and iron salt is 12:4.8:1;

[0102] (2) Placing graphene aerogel on MXene (Ti 2 CT x ) dispersion (concentration 0.02 mg / mL) for 5 min, taken out, transferred to a freeze dryer and treated at -50°C and 10 Pa for 24 h to remove internal moisture to obtain MXene-modified graphene aerogel; wherein the liquid-to-solid ratio of MXene dispersion to graphene aerogel is 50 mL / g;

[0103] (3) adding the MXene-modified graphene aerogel to an alkaline ethanol solution containing 6 wt % of a vinyl silane coupling agent (vinyl triethoxysilane), stirring evenly, and then heating in an oven at 100° C. for 4 hours to obtain a MXene-modified graphene aerogel modified with a silane coupling agent, wherein the weight ratio of the MXene-modified graphene aerogel to the vinyl silane coupling agent is 1:3, and the alkaline ethanol solution is obtained by mixing a sodium hydroxide aqueous solution with a concentration of 1.33 g / mL and ethanol in a volume ratio of 0.075:1;

[0104] (4) The MXene-modified graphene aerogel modified by the silane coupling agent was added to an ethyl acetate solution containing a vinyl monomer (divinylbenzene) and an initiator (azobisisobutyronitrile), stirred evenly, and then transferred to a hydrothermal reactor, reacted at a temperature of 110°C for 20 hours, washed three times with ethanol and then dried (drying temperature was 60°C, vacuum degree was -0.1MPa), wherein the concentration of the vinyl monomer in the ethyl acetate solution containing the vinyl monomer and the initiator was 0.1mg / mL, and the concentration of the initiator was 3mg / mL; the weight ratio of the MXene-modified graphene aerogel modified by the silane coupling agent to the vinyl monomer was 1200:1.

[0105] Example 2

[0106] The aerogel composite material S2 is prepared, and the specific process includes the following steps:

[0107] The method described in Example 1 was followed, except that in step (2), the concentration of the MXene dispersion was 0.06 mg / mL.

[0108] Example 3

[0109] The aerogel composite material S2 is prepared, and the specific process includes the following steps:

[0110] The method described in Example 1 was followed, except that in step (2), the concentration of the MXene dispersion was 0.1 mg / mL.

[0111] Example 4

[0112] The aerogel composite material S4 is prepared, and the specific process includes the following steps:

[0113] (1) 30 mg of graphene oxide (GO) was dispersed in 10 mL of water and ultrasonically treated for 4 h to obtain a GO dispersion. Then, 0.6 mL of dopamine aqueous solution (concentration: 20 mg / mL) was added to the GO dispersion and stirred for 10 min. Subsequently, 0.25 mL of iron salt aqueous solution (iron salt: FeCl 3 6H 2 O, with a concentration of 10 mg / mL) and stirred for 1 hour, then the mixture was transferred to a polytetrafluoroethylene-lined stainless steel autoclave, and hydrothermally treated at 120° C. for 12 hours to form a gel-like product, and then the gel-like product was transferred to a freeze dryer and treated at -50° C. and 10 Pa for 24 hours to remove internal moisture to obtain a graphene aerogel; wherein the weight ratio of graphene oxide, dopamine and iron salt is 12:4.8:1;

[0114] (2) Placing graphene aerogel on MXene (Ti 2 CT x ) dispersion (concentration of 0.1 mg / mL) for 5 min, taken out, transferred to a freeze dryer and treated at -50°C and 10 Pa for 24 h to remove internal moisture to obtain MXene-modified graphene aerogel; wherein the liquid-to-solid ratio of MXene dispersion to graphene aerogel is 50 mL / g;

[0115] (3) adding the MXene-modified graphene aerogel to an alkaline ethanol solution containing 4 wt % of a vinyl silane coupling agent (vinyl triethoxysilane), stirring evenly, and then heating in an oven at 100° C. for 4 hours to obtain a MXene-modified graphene aerogel modified with a silane coupling agent, wherein the weight ratio of the MXene-modified graphene aerogel to the vinyl silane coupling agent is 1:2, and the alkaline ethanol solution is obtained by mixing a sodium hydroxide aqueous solution having a concentration of 1.33 g / mL and ethanol in a volume ratio of 0.075:1;

[0116] (4) The MXene-modified graphene aerogel modified by the silane coupling agent was added to an ethyl acetate solution containing a vinyl monomer (divinylbenzene) and an initiator (azobisisobutyronitrile), stirred evenly, and then transferred to a hydrothermal reactor, reacted at a temperature of 110°C for 20 hours, washed three times with ethanol and then dried (drying temperature was 60°C, vacuum degree was -0.1MPa), wherein the concentration of the vinyl monomer in the ethyl acetate solution containing the vinyl monomer and the initiator was 0.1mg / mL, and the concentration of the initiator was 3mg / mL; the weight ratio of the MXene-modified graphene aerogel modified by the silane coupling agent to the vinyl monomer was 1200:1.

[0117] Example 5

[0118] The aerogel composite material S5 is prepared, and the specific process includes the following steps:

[0119] (1) 30 mg of graphene oxide (GO) was dispersed in 10 mL of water and ultrasonically treated for 4 h to obtain a GO dispersion. Then, 0.6 mL of dopamine aqueous solution (concentration: 20 mg / mL) was added to the GO dispersion and stirred for 10 min. Subsequently, 0.25 mL of iron salt aqueous solution (iron salt: FeCl 3 6H 2 O, with a concentration of 10 mg / mL) and stirred for 1 hour, then the mixture was transferred to a polytetrafluoroethylene-lined stainless steel autoclave, and hydrothermally treated at 120° C. for 12 hours to form a gel-like product, and then the gel-like product was transferred to a freeze dryer and treated at -50° C. and 10 Pa for 24 hours to remove internal moisture to obtain a graphene aerogel; wherein the weight ratio of graphene oxide, dopamine and iron salt is 12:4.8:1;

[0120] (2) Placing graphene aerogel on MXene (Ti 2 CT x) dispersion (concentration of 0.1 mg / mL) for 5 min, taken out, transferred to a freeze dryer and treated at -50°C and 10 Pa for 24 h to remove internal moisture to obtain MXene-modified graphene aerogel; wherein the liquid-to-solid ratio of MXene dispersion to graphene aerogel is 50 mL / g;

[0121] (3) adding the MXene-modified graphene aerogel to an alkaline ethanol solution containing 8 wt % of a vinyl silane coupling agent (vinyl triethoxysilane), stirring evenly, and then heating in an oven at 100° C. for 4 hours to obtain a MXene-modified graphene aerogel modified with a silane coupling agent, wherein the weight ratio of the MXene-modified graphene aerogel to the vinyl silane coupling agent is 1:4, and the alkaline ethanol solution is obtained by mixing a sodium hydroxide aqueous solution having a concentration of 1.33 g / mL and ethanol in a volume ratio of 0.075:1;

[0122] (4) The MXene-modified graphene aerogel modified by the silane coupling agent was added to an ethyl acetate solution containing a vinyl monomer (divinylbenzene) and an initiator (azobisisobutyronitrile), stirred evenly, and then transferred to a hydrothermal reactor, reacted at a temperature of 110°C for 20 hours, washed three times with ethanol and then dried (drying temperature was 60°C, vacuum degree was -0.1MPa), wherein the concentration of the vinyl monomer in the ethyl acetate solution containing the vinyl monomer and the initiator was 0.1mg / mL, and the concentration of the initiator was 3mg / mL; the weight ratio of the MXene-modified graphene aerogel modified by the silane coupling agent to the vinyl monomer was 1200:1.

[0123] Example 6

[0124] The aerogel composite material S6 is prepared, and the specific process includes the following steps:

[0125] (1) 30 mg of graphene oxide (GO) was dispersed in 10 mL of water and ultrasonically treated for 4 h to obtain a GO dispersion. Then, 0.6 mL of dopamine aqueous solution (concentration: 20 mg / mL) was added to the GO dispersion and stirred for 10 min. Subsequently, 0.25 mL of iron salt aqueous solution (iron salt: FeCl 3 6H 2 O, with a concentration of 10 mg / mL) and stirred for 1 hour, then the mixture was transferred to a polytetrafluoroethylene-lined stainless steel autoclave, and hydrothermally treated at 120° C. for 12 hours to form a gel-like product, and then the gel-like product was transferred to a freeze dryer and treated at -50° C. and 10 Pa for 24 hours to remove internal moisture to obtain a graphene aerogel; wherein the weight ratio of graphene oxide, dopamine and iron salt is 12:4.8:1;

[0126] (2) Placing graphene aerogel on MXene (Ti 2 CT x ) dispersion (concentration of 0.06 mg / mL) for 5 min, taken out, transferred to a freeze dryer and treated at -50°C and 10 Pa for 24 h to remove internal moisture to obtain MXene-modified graphene aerogel; wherein the liquid-to-solid ratio of MXene dispersion to graphene aerogel is 60 mL / g;

[0127] (3) adding the MXene-modified graphene aerogel to an alkaline ethanol solution containing 6 wt % of a vinyl silane coupling agent (vinyl triethoxysilane), stirring evenly, and then heating in an oven at 100° C. for 4 hours to obtain a MXene-modified graphene aerogel modified with a silane coupling agent, wherein the weight ratio of the MXene-modified graphene aerogel to the vinyl silane coupling agent is 1:3, and the alkaline ethanol solution is obtained by mixing a sodium hydroxide aqueous solution having a concentration of 1.33 g / mL and ethanol in a volume ratio of 0.075:1;

[0128] (4) The MXene-modified graphene aerogel modified by the silane coupling agent was added to an ethyl acetate solution containing a vinyl monomer (divinylbenzene) and an initiator (azobisisobutyronitrile), stirred evenly, and then transferred to a hydrothermal reactor, reacted at a temperature of 110°C for 20 hours, washed three times with ethanol and then dried (drying temperature was 60°C, vacuum degree was -0.1MPa), wherein the concentration of the vinyl monomer in the ethyl acetate solution containing the vinyl monomer and the initiator was 0.2mg / mL, and the concentration of the initiator was 3mg / mL; the weight ratio of the MXene-modified graphene aerogel modified by the silane coupling agent to the vinyl monomer was 600:1.

[0129] Example 7

[0130] The aerogel composite material S7 is prepared, and the specific process includes the following steps:

[0131] The method described in Example 6 is used for implementation, except that in step (4), in the ethyl acetate solution containing the vinyl monomer and the initiator, the concentration of the vinyl monomer is 0.3 mg / mL, and the weight ratio of the silane coupling agent-modified MXene-modified graphene aerogel to the vinyl monomer is 400:1.

[0132] Example 8

[0133] The aerogel composite material S8 is prepared, and the specific process includes the following steps:

[0134] The method described in Example 6 is used for implementation, except that in step (4), in the ethyl acetate solution containing the vinyl monomer and the initiator, the concentration of the vinyl monomer is 0.5 mg / mL, and the weight ratio of the silane coupling agent-modified MXene-modified graphene aerogel to the vinyl monomer is 240:1.

[0135] Example 9

[0136] (1) 35 mg of graphene oxide (GO) was dispersed in 10 mL of water and ultrasonically treated for 4 h to obtain a GO dispersion. Then, 0.5 mL of dopamine aqueous solution (concentration: 20 mg / mL) was added to the GO dispersion and stirred for 10 min. Subsequently, 0.25 mL of iron salt aqueous solution (iron salt: FeCl 3 6H 2 O, with a concentration of 10 mg / mL) and stirred for 1 hour, then the mixture was transferred to a polytetrafluoroethylene-lined stainless steel autoclave, and hydrothermally treated at 120° C. for 12 hours to form a gel-like product, and then the gel-like product was transferred to a freeze dryer and treated at -50° C. and 10 Pa for 24 hours to remove internal moisture to obtain a graphene aerogel; wherein the weight ratio of graphene oxide, dopamine and iron salt is 14:4:1;

[0137] (2) Placing graphene aerogel on MXene (Ti 2 CT x ) dispersion (concentration 0.05 mg / mL) for 8 min, taken out, transferred to a freeze dryer and treated at -50°C and 10 Pa for 24 h to remove internal moisture to obtain MXene-modified graphene aerogel; wherein the liquid-to-solid ratio of MXene dispersion to graphene aerogel is 60 mL / g;

[0138] (3) adding the MXene-modified graphene aerogel to an alkaline ethanol solution containing 6 wt % of a vinyl silane coupling agent (vinyl tri-tert-butoxysilane), stirring evenly, and then heating in an oven at 95° C. for 4 hours to obtain a MXene-modified graphene aerogel modified with a silane coupling agent, wherein the weight ratio of the MXene-modified graphene aerogel to the vinyl silane coupling agent is 1:3, and the alkaline ethanol solution is obtained by mixing a sodium hydroxide aqueous solution having a concentration of 1.33 g / mL and ethanol in a volume ratio of 0.075:1;

[0139] (4) The MXene-modified graphene aerogel modified by the silane coupling agent was added to an ethyl acetate solution containing a vinyl monomer (styrene) and an initiator (azobisisobutyronitrile), stirred evenly, and then transferred to a hydrothermal reactor, reacted at a temperature of 120°C for 18 hours, washed three times with ethanol and then dried (drying temperature was 60°C, vacuum degree was -0.1MPa), wherein the concentration of the vinyl monomer in the ethyl acetate solution containing the vinyl monomer and the initiator was 0.2mg / mL, and the concentration of the initiator was 3mg / mL; the weight ratio of the MXene-modified graphene aerogel modified by the silane coupling agent to the vinyl monomer was 600:1.

[0140] Example 10

[0141] (1) 35 mg of graphene oxide (GO) was dispersed in 10 mL of water and ultrasonically treated for 4 h to obtain a GO dispersion, and then 0.5 mL of dopamine aqueous solution (concentration of 20 mg / mL) was added to the GO dispersion and stirred for 10 min; then 0.25 mL of iron salt aqueous solution (iron salt is ferrous sulfate heptahydrate, concentration of 10 mg / mL) was added under magnetic stirring and stirred for 1 h, and then the mixture was transferred to a polytetrafluoroethylene-lined stainless steel autoclave and hydrothermally treated at 125° C. for 11 h to form a gel-like product, and then the gel-like product was transferred to a freeze dryer and treated at -50° C. and 10 Pa for 24 h to remove internal moisture to obtain a graphene aerogel; wherein the weight ratio of graphene oxide, dopamine and iron salt was 14:4:1;

[0142] (2) Placing graphene aerogel on MXene (Ti 3 C 2 T x ) dispersion (concentration 0.02 mg / mL) for 5 min, taken out, transferred to a freeze dryer and treated at -50°C and 10 Pa for 24 h to remove internal moisture to obtain MXene-modified graphene aerogel; wherein the liquid-to-solid ratio of MXene dispersion to graphene aerogel is 60 mL / g;

[0143] (3) adding the MXene-modified graphene aerogel to an alkaline ethanol solution containing 6 wt % of a vinyl silane coupling agent (vinyl triethoxysilane), stirring evenly, and then heating in an oven at 100° C. for 4 hours to obtain a MXene-modified graphene aerogel modified with a silane coupling agent, wherein the weight ratio of the MXene-modified graphene aerogel to the vinyl silane coupling agent is 1:3, and the alkaline ethanol solution is obtained by mixing a sodium hydroxide aqueous solution having a concentration of 1.33 g / mL and ethanol in a volume ratio of 0.075:1;

[0144] (4) The MXene-modified graphene aerogel modified by the silane coupling agent was added to an ethyl acetate solution containing a vinyl monomer (styrene) and an initiator (azobisisobutyronitrile), stirred evenly, and then transferred to a hydrothermal reactor, reacted at a temperature of 110°C for 20 hours, washed three times with ethanol and then dried (drying temperature was 60°C, vacuum degree was -0.1MPa), wherein the concentration of the vinyl monomer in the ethyl acetate solution containing the vinyl monomer and the initiator was 0.2mg / mL, and the concentration of the initiator was 3mg / mL; the weight ratio of the MXene-modified graphene aerogel modified by the silane coupling agent to the vinyl monomer was 600:1.

[0145] Comparative Example 1

[0146] The preparation of graphene aerogel includes the following steps:

[0147] (1) 30 mg of graphene oxide (GO) was dispersed in 10 mL of water and ultrasonically treated for 4 h to obtain a GO dispersion, and then 0.6 mL of dopamine aqueous solution (concentration of 20 mg / mL) was added to the GO dispersion and stirred for 10 min; then 0.25 mL of iron salt aqueous solution (iron salt is FeCl3·6H2O, concentration of 10 mg / mL) was added under magnetic stirring and stirred for 1 h, and then the mixture was transferred to a polytetrafluoroethylene-lined stainless steel autoclave and hydrothermally treated at 120°C for 12 h to form a gel-like product, and then the gel-like product was transferred to a freeze dryer and treated at -50°C and 10 Pa for 24 h to remove internal moisture to obtain a graphene aerogel; wherein the weight ratio of graphene oxide, dopamine and iron salt is 12:4.8:1;

[0148] Comparative Example 2

[0149] The preparation of MXene-modified graphene aerogel includes the following steps:

[0150] (1) 30 mg of graphene oxide (GO) was dispersed in 10 mL of water and ultrasonically treated for 4 h to obtain a GO dispersion. Then, 0.6 mL of dopamine aqueous solution (concentration: 20 mg / mL) was added to the GO dispersion and stirred for 10 min. Subsequently, 0.25 mL of iron salt aqueous solution (iron salt: FeCl 3 6H 2 O, with a concentration of 10 mg / mL) and stirred for 1 hour, then the mixture was transferred to a polytetrafluoroethylene-lined stainless steel autoclave, and hydrothermally treated at 120° C. for 12 hours to form a gel-like product, and then the gel-like product was transferred to a freeze dryer and treated at -50° C. and 10 Pa for 24 hours to remove internal moisture to obtain a graphene aerogel; wherein the weight ratio of graphene oxide, dopamine and iron salt is 12:4.8:1;

[0151] (2) Placing graphene aerogel on MXene (Ti 2 CT x ) dispersion (concentration 0.02 mg / mL) for 5 min, taken out, transferred to a freeze dryer and treated at -50°C and 10 Pa for 24 h to remove internal moisture to obtain MXene-modified graphene aerogel; wherein the liquid-to-solid ratio of MXene dispersion to graphene aerogel is 50 mL / g.

[0152] Comparative Example 3

[0153] The preparation of tetradecylamine-modified MXene-modified graphene aerogel includes the following steps:

[0154] (1) preparing MXene-modified graphene aerogel according to the method described in Comparative Example 2;

[0155] (2) The MXene-modified graphene aerogel was added to 100 mL of tetradecylamine ethanol solution (concentration of 0.1 mg / mL), soaked for 5 min, and vacuum dried for 10 h at 60 ° C and -0.1 MPa. The aerogel was taken out, washed with ethanol three times, and then vacuum dried for 10 h at 60 ° C and -0.1 MPa to obtain a tetradecylamine-modified MXene-modified graphene aerogel.

[0156] Test Example 1

[0157] The products prepared in Example 3 and Comparative Example 1 were characterized using SEM. Figure 1 The test process includes the following steps: first, the sample to be tested is placed in liquid nitrogen for brittle fracture, then gold is sprayed on the brittle fracture surface for 40 seconds, and finally the surface morphology of the brittle fracture surface is analyzed by S4800 SEM. Figure 1 A is the characterization result of the product prepared in Comparative Example 1, Figure 1 B is the characterization result of the product prepared in Example 3.

[0158] As can be seen from the figure, graphene aerogel has a connected pore structure and a relatively smooth surface, while the surface of graphene aerogel modified by MXene nanosheets has a rough structure.

[0159] Test Example 2

[0160] Demulsification ability test: Diesel: sodium dodecyl sulfate and water are mixed in a volume ratio of 10:1:2000 and stirred for 30 minutes to completely emulsify them to obtain a test liquid; the test liquid is filtered through a syringe blocked with an aerogel material, and the oil content in the system before and after filtration is tested by infrared spectrophotometry. The emulsified oil disposal rate can be calculated by comparing the two.

[0161] The demulsification ability test results of the products prepared in the examples and comparative examples are shown in Table 1. The demulsification adsorption effect pictures of the products prepared in Example 3 are shown in Table 1. Figure 2 shown.

[0162] Table 1

[0163]

[0164]

[0165] From Table 1 and Figure 2 The results show that the aerogel composite material prepared by the present invention has excellent demulsification ability, which may be due to the synergistic effect of the surface nano-rough structure and the long chain of super-hydrophobic polymer. The emulsified oil treatment rate can be as high as 98%.

[0166] Test Example 3

[0167] 1. Contact angle test.

[0168] The test process includes the following steps: fracture the sample in liquid nitrogen, cut a suitable size and flat fracture surface for testing, slowly drip deionized water on the sample surface through a micro syringe, and measure the contact angle of the liquid on the sample.

[0169] The photographs taken when the product prepared in Example 3 was subjected to contact angle test are as follows: Figure 3 The contact angle test results of the embodiments and comparative examples are shown in Table 2.

[0170] Table 2

[0171]

[0172]

[0173] 2. Density, porosity and open porosity test.

[0174] This experiment uses the Archimedean principle, that is, by measuring the buoyancy of the sample in a liquid with a known density, the density, porosity and open porosity of the aerogel are determined. This process is similar to the balance weighing method. First, the sample is immersed in a liquid medium, and the liquid medium is completely filled in the sample gap, and then weighed to calculate the porosity of the porous material. The schematic diagram of the experimental device is shown in Figure 4 shown.

[0175] The specific measurement process is as follows: prepare a cubic sample with a size of 5 mm and ensure that the surface is flat. First, measure the net weight of the sample in air w 1 Then, the sample was immersed in methyl silicone oil and the negative pressure vacuum method was used to promote the removal of air in the gaps. After the medium completely filled the aerogel gaps, the sample was taken out and the excess silicone oil on its surface was gently wiped off. The wet weight of the sample at this time was weighed.2 Then, the sample is placed in a sling immersed in a density measuring component filled with methyl silicone oil. The total weight of the sling and the sample is recorded as w 3 , take out the sample and weigh it. The weight of the sling in the silicone oil is w 4 .

[0176] The porosity θ of the porous material is obtained 0 for:

[0177]

[0178] Where: L is the density of the working fluid; ρ S is the density of the porous material relative to the dense solid material.

[0179] The open porosity θ of porous materials is:

[0180]

[0181] Where: ME is the density of the saturated medium.

[0182] Finally, the density of the porous material is calculated according to the following formula:

[0183] ρ=ρ S (1-θ 0 )

[0184] The test results are shown in Table 3.

[0185] Table 3

[0186] serial number Porosity (%) <![CDATA[Density (mg / cm 3 )]]> Example 1 97.9 11.4 Example 2 97.2 11.8 Example 3 97.3 12.6 Example 4 97.5 11.9 Example 5 96.7 12.7 Example 6 97.1 11.9 Example 7 96.7 12.5 Example 8 96.5 12.8 Example 9 96.1 12.6 Example 10 96.9 12.1 Comparative Example 1 98.1 11.2 Comparative Example 2 98.2 11.6 Comparative Example 3 97.9 11.5

[0187] 3. Compression strength test

[0188] The compression test was carried out at room temperature using a CMT 4204 universal tensile testing machine at a compression rate of 1 mm / min. Each group of samples was tested 3 times and the average value was taken.

[0189] The compressive strength test results of the products prepared in the examples and comparative examples are shown in Table 4.

[0190] Table 4

[0191]

[0192]

[0193] 4. Oil absorption test

[0194] The oil absorption characteristics of the products prepared in the examples and comparative examples were characterized using crude oil. The oil absorption rate is the ratio of the mass of the absorbed crude oil to the mass of the sample to be tested. The results are shown in Table 5.

[0195] Table 5

[0196] serial number Oil absorption rate (g / g) serial number Oil absorption rate (g / g) Example 1 115 Example 8 135 Example 2 126 Example 9 130 Example 3 138 Example 10 131 Example 4 136 Comparative Example 1 79 Example 5 137 Comparative Example 2 88 Example 6 129 Comparative Example 3 85 Example 7 131

[0197] It can be seen from the results in Tables 2-5 that the aerogel composite material prepared in the present invention has super hydrophobicity, low density, high porosity, high oil absorption rate and high compressive strength, and can meet the mechanical property requirements in practical applications.

[0198] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. An aerogel composite material, characterized in that: The aerogel composite material comprises: graphene aerogel, MXene nanosheets loaded on the surface of the graphene aerogel, and vinyl polymer in-situ grown on the MXene nanosheets; The graphene aerogel contains reduced graphene oxide, polydopamine and iron element.

2. The aerogel composite material according to claim 1, characterized in that: The contact angle of the aerogel composite material is ≥143°; Preferably, the oil absorption rate of the aerogel composite material is ≥115 g / g.

3. A method for preparing an aerogel composite material, characterized in that: The method comprises the following steps: (1) mixing graphene oxide, dopamine, iron salt and water, and then performing a hydrothermal reaction and freeze drying to obtain a graphene aerogel; (2) soaking the graphene aerogel in a MXene dispersion, taking it out, and then freeze-drying it to obtain a MXene-modified graphene aerogel; (3) mixing the MXene-modified graphene aerogel with a solution containing a vinyl silane coupling agent to react, thereby obtaining a MXene-modified graphene aerogel modified with a silane coupling agent; (4) In the presence of an initiator, the MXene-modified graphene aerogel modified with a silane coupling agent is mixed with a vinyl monomer for polymerization reaction.

4. The preparation method according to claim 3, characterized in that: In step (1), the weight ratio of graphene oxide, dopamine and iron salt is 10-20:1-5:

1.

5. The preparation method according to claim 3 or 4, characterized in that: In step (1), the conditions of the hydrothermal reaction include: temperature of 100-140° C.; time of 10-20 h.

6. The preparation method according to claim 3 or 4, characterized in that: In step (2), the concentration of MXene in the MXene dispersion is 0.02-0.1 mg / mL.

7. The preparation method according to claim 3 or 6, characterized in that: In step (2), the liquid-to-solid ratio of the MXene dispersion to the graphene aerogel is 10-100 mL / g.

8. The preparation method according to any one of claims 3 to 7, characterized in that: In step (2), the soaking time is 1-60 minutes.

9. The preparation method according to claim 3, characterized in that: In step (3), the weight ratio of MXene-modified graphene aerogel to vinyl silane coupling agent is 1:1-10.

10. The preparation method according to claim 3 or 9, characterized in that: In step (3), the concentration of the vinyl silane coupling agent in the solution containing the vinyl silane coupling agent is 4-8% by weight.

11. The preparation method according to claim 3 or 10, characterized in that: In step (3), the vinyl silane coupling agent is selected from one or more of vinyl trimethoxysilane, vinyl trichlorosilane, vinyl tri-tert-butoxysilane and vinyl triethoxysilane.

12. The preparation method according to claim 3, characterized in that: In step (3), the reaction conditions include: temperature of 80-120° C.; time of 1-4 h.

13. The preparation method according to claim 3, characterized in that: The specific process of step (4) includes: mixing the MXene-modified graphene aerogel modified by a silane coupling agent with a solution containing a vinyl monomer and an initiator for reaction.

14. The preparation method according to claim 14, characterized in that: The concentration of the vinyl monomer in the solution containing the vinyl monomer and the initiator is 0.05-0.5 mg / mL.

15. The preparation method according to claim 13 or 14, characterized in that: The concentration of the initiator in the solution containing the vinyl monomer and the initiator is 3-5 mg / mL.

16. According to the preparation method according to claim 3 or 13, in step (4), the weight ratio of the MXene-modified graphene aerogel modified by a silane coupling agent to the vinyl monomer is 200-1200:

1.

17. The preparation method according to claim 3 or 16, characterized in that: In step (4), the vinyl monomer is styrene or divinylbenzene.

18. The preparation method according to claim 3, characterized in that: In step (4), the reaction conditions include: temperature of 80-140° C. and time of 12-36 h.

19. An aerogel composite material prepared by the method according to any one of claims 3 to 18.

20. Use of the aerogel composite material according to any one of claims 1 to 2 or the aerogel composite material according to claim 19 in oil-water separation.

Citation Information

Patent Citations

  • Organic silicon foam with in-situ demulsification and adsorption function and application of organic silicon foam in oil-water separation

    CN112691649A

  • Preparation method of asymmetric wettability wood film capable of converting and separating oil-water emulsion

    CN114681953A

  • Preparation method for oxidized graphene-poly-dopamine composite aerogel

    CN105254916A

  • Superhydrophobic composite carbon aerogel oil absorbent material and preparation method thereof