Ruthenium-based catalyst for ammonia synthesis reaction as well as preparation method and application of ruthenium-based catalyst

The Ru/HfB2 catalyst prepared by using HfB2 carrier and high-voltage electric field drying technology solves the problem of high activity but poor stability of existing ammonia synthesis catalysts under high temperature and high pressure, and achieves high ammonia synthesis activity and stability under mild conditions. Reduce energy consumption and carbon emissions.

CN118767911APending Publication Date: 2024-10-15CHINA ENERGY INVESTMENT CORP LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310355376.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing ammonia synthesis catalysts have high activity but poor stability under high temperature and high pressure conditions, and have low single-pass conversion rates, resulting in increased energy consumption and carbon emissions. New catalysts with low temperature and high activity need to be developed to replace the traditional Haber-Bosch process.

Method used

A Ru/HfB2 catalyst with high catalytic activity and stability was prepared using HfB2 carrier through a specific preparation method, including mixing HfO2 and boron, performing multiple heating reduction and ball milling treatments, combined with high-voltage electric field drying.

Benefits of technology

Under mild conditions, the catalytic activity and stability of ammonia synthesis can be significantly improved, energy consumption and carbon emissions can be reduced, and the preparation process cost is low, making it suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767911A_ABST
    Figure CN118767911A_ABST
Patent Text Reader

Abstract

The invention provides a ruthenium-based catalyst for an ammonia synthesis reaction as well as a preparation method and application of the ruthenium-based catalyst. The ruthenium-based catalyst prepared by the invention has good catalytic activity and stability in catalysis of the ammonia synthesis reaction. The preparation method comprises the following steps: 1) preparing an HfB2 carrier by adopting a method comprising the following steps: 1a) mixing HfO2 and boron, and carrying out first heating reduction on a pressed material obtained by pressing an obtained powder mixture; 1b) immersing the pressed material in hot water for treatment, and then carrying out secondary heating reduction on the pressed material; the temperature conditions of the first heating reduction and the second heating reduction are respectively 1550-1700 DEG C; and 1c) carrying out ball milling on the pressed material to obtain the HfB2 carrier, and 2) impregnating the HfB2 carrier prepared in the step 1) in an impregnation liquid containing ruthenium ions, and then drying to obtain the ruthenium-based catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ammonia synthesis catalysts, and in particular to a ruthenium-based catalyst for ammonia synthesis reaction, a preparation method thereof and an application thereof. Background Art

[0002] The synthetic ammonia industry requires catalysts with higher activity at lower temperatures and pressures. For more than 90 years, countries around the world have never stopped researching and developing synthetic ammonia catalysts. At present, the catalytic efficiency of industrial catalysts has reached more than 90% at high temperatures, close to the equilibrium ammonia concentration (depending on the pressure). For example, the catalytic efficiency of A301 catalyst is close to 100% at 15MPa and 475°C. To improve the activity of the catalyst, the only way is to lower the reaction temperature. On the other hand, the single-pass conversion rate of industrial synthetic ammonia is only 15%-25%, and most of the gas needs to be circulated, thereby increasing power consumption. In order to increase the single-pass conversion rate, it is only possible to lower the reaction temperature. Therefore, the overall development trend of synthetic ammonia catalyst research is to develop new catalysts with low temperature and high activity, reduce the reaction temperature, increase the equilibrium conversion rate and single-pass conversion rate of ammonia, or achieve low-pressure synthetic ammonia.

[0003] The Haber-Bosch process has been the industry standard for ammonia synthesis for the past 100 years and is considered one of the greatest innovations of the 20th century. Today, the process produces 146 million tons of ammonia per year and utilizes approximately 1% of the world's total energy supply. The HB process has been fine-tuned and its efficiency has been massively improved over this period. Catalyst development for the process has been extensively studied, but the fused iron catalyst developed in the 70s is the most efficient catalyst to date, however the cost of the more active metals is prohibitive. Since there is little potential for significant process development with the catalyst, most improvements to the HB process have been in optimizing the overall plant design. Major technological breakthroughs are needed to transform the current ammonia synthesis process. Due to the high energy utilization, high carbon emissions, and little technological advancement, there is a push for smaller-scale ammonia production processes that can use renewable energy closer to crops and other end users of ammonia. One of the main barriers to using renewable energy is the intermittent electricity it runs on.

[0004] Patent application CN114733551A reports a high-performance ruthenium-based mild ammonia synthesis catalyst and its preparation method and application. The Ru / BN catalyst is synthesized by synthesizing a BN carrier, and then the rare earth element is loaded on the Ru / BN catalyst by an equal volume impregnation method, and finally a RuM / BN catalyst is obtained. The catalyst has a high ammonia yield of 43.8 mmol g at 400 °C and 1 MPa. cat -1 h -1 The ammonia synthesis rate was increased, but the catalyst could only run for 140 h and the stability problem was not solved.

[0005] Patent application CN114789053A reports a ruthenium-based mild ammonia synthesis catalyst and its preparation method and application. The catalyst provided comprises an active component Ru, an additive and a carrier. 2 or ZrO 2 The composition of N 2 The activation path of the catalyst can achieve the modulation of the performance of synthetic ammonia under mild conditions. The catalyst can reach 35.3mmol g cat -1 h -1 The ammonia synthesis rate is increased, but according to the data of the patent application, although it can run smoothly for 300 hours, the performance of the catalyst is significantly inferior to that of other inventions.

[0006] The efficiency of the current HB process relies on large-scale production that needs to be continuously operated. The system has a long rise / fall time and shortens the service life of the catalyst. Moreover, large-scale processes are now the main contributors to carbon emissions. In terms of carrier selection, the current carriers of synthetic ammonia catalysts are mainly: carbon materials, metal oxides, and other carriers. Although carbon materials have a large specific surface area, good thermal conductivity and electronic conductivity, and a rich pore structure, methanation will occur in the catalytic reaction of synthetic ammonia, which is not conducive to long-term use; and although metal oxides have high mechanical strength and rich acid-base active sites on the surface, the application of metal oxide carriers in synthetic ammonia basically requires a harsh high temperature and high pressure environment, which also limits its application under relatively mild conditions. Other carriers mainly include molecular sieve carriers, hexagonal boron nitride (BN), metal hydrides and metal nitrides, rare earth oxide carriers, electronic compound carriers, MXene carriers, etc. These carriers have good chemical and thermal stability, good thermal conductivity and small metal-carrier interaction, and are considered to be potential carriers for synthetic ammonia. At present, there are few reports on the use of HfB 2 Report on the preparation of ruthenium-based catalysts for ammonia synthesis using carriers.

[0007] In summary, in the context of my country's carbon peak and carbon neutrality, it is urgent to develop an alternative to the HB process. Therefore, the development of a ruthenium-based catalyst that can be used for the synthesis of ammonia in an efficient and mild manner will have great industrial application value. Summary of the invention

[0008] In view of this, the present invention provides a ruthenium-based catalyst for ammonia synthesis reaction and a preparation method and application thereof. The ruthenium-based catalyst prepared by the present invention has good stability in catalyzing ammonia synthesis reaction and can exhibit high synthetic ammonia performance under mild conditions.

[0009] To achieve the purpose, the present invention provides the following technical solutions:

[0010] The first aspect of the present invention provides a method for preparing a ruthenium-based catalyst for an ammonia synthesis reaction, comprising the following steps:

[0011] 1) HfB is prepared by a method comprising the following steps 2 Carrier:

[0012] 1a) HfO 2 and boron in a molar ratio of less than 0.3 and greater than 0, and the obtained powder mixture is pressed to obtain a pressed product and subjected to a first heating reduction;

[0013] 1b) then immersing the pressed product in hot water for treatment, and then taking out the pressed product and performing a second heating reduction; the temperature conditions of the first heating reduction and the second heating reduction are 1550-1700° C. respectively;

[0014] 1c) grinding the pressed product after the treatment in step 1b) by ball milling to obtain the HfB 2 Carrier;

[0015] 2) The HfB prepared in step 1) 2 The carrier is impregnated in an impregnation solution containing ruthenium ions and then dried to obtain the ruthenium-based catalyst.

[0016] The ruthenium-based catalyst prepared by the above-mentioned preparation method provided by the present invention has good catalytic activity for ammonia synthesis and good catalytic activity stability. 2 carrier, HfO 2 and boron in a molar ratio of less than 0.3 and greater than 0, and then pressed and molded, and then heated and reduced for the first time, and then hot water treatment, and then heated and reduced for the second time, and then ball milled, and the carrier prepared according to the above specific process has B 2 O 3 It can be removed more thoroughly, and it is easy to obtain a carrier with a smaller particle size and good mechanical strength. The obtained carrier can load ruthenium well and evenly. The prepared ruthenium-based catalyst can exert good catalytic activity for ammonia synthesis under milder conditions and has good catalytic activity stability.

[0017] In the present invention, in step 1a), HfO 2Mixing HfB with boron in a molar ratio of less than 0.3 and greater than 0 can not only ensure the smooth progress of the reaction but also ensure the presence of residual boron. The inventors found that the catalyst finally obtained by using this molar ratio has significantly improved catalytic activity and stability for ammonia synthesis compared with a higher molar ratio. In steps 1a) and 1b), the temperature conditions of the first heating reduction and the second heating reduction are respectively controlled to 1550-1700°C. Compared with a lower heating reduction temperature, the catalyst finally obtained has significantly improved catalytic activity for ammonia synthesis. In the preparation method of the present invention, HfB is prepared in a specific order of first heating reduction-hot water treatment-second heating reduction-ball milling. 2 The preparation of the carrier is beneficial to 2 O 3 The removal is more thorough, which helps to significantly reduce the particle size of the final powder, improve the mechanical strength of the powder, and improve the catalytic activity and stability of the ammonia synthesis of the final ruthenium-based catalyst.

[0018] In some preferred embodiments, in step 2), the drying is performed using a high-voltage electric field drying technique. This drying method not only has high drying efficiency and low energy consumption, but also allows water molecules to move freely on the inner and outer surfaces of the catalyst, forming more pores and increasing the specific surface area of ​​the catalyst, thereby further improving its catalytic performance. Preferably, the drying is performed at an electric field strength of 10 to 20 kV / cm.

[0019] In some preferred embodiments, in step 1a), the HfO 2 and boron in ethanol and Si 3 N 4 The mixing is carried out in the presence of spherical particles, and in step 1a), the powder mixture is dried before the pressing. 3 N 4 The ball is helpful to accelerate the reaction of boron powder and HfO 2 There is no special requirement for the amount of ethanol used, as long as it can immerse the HfO 2 and boron, Si 3 N 4 There is no special requirement for the amount of balls, as long as they can promote HfO 2 The amount of HfO mixed with boron can be any, for example, in step 1a), 50-150 g of HfO 2 Add several (e.g. 2-6, e.g. 4) Si 3 N 4 The ball can be.

[0020] Specifically, the first heating reduction and the second heating reduction can be carried out in a graphite element furnace. In some preferred embodiments, the time for the first heating reduction in step 1a) and the second heating reduction in step 1b) is 1-3 hours respectively.

[0021] In some preferred embodiments, in step 1a), when the first heating reduction is performed, the heating rate to 1550-1700° C. is 5-15° C. / min.

[0022] In some preferred embodiments, in step 1b), the treatment time in the hot water is 20 to 100 minutes; specifically, the temperature of the hot water is preferably 70-90°C. The preferred hot water treatment conditions are conducive to more thorough removal of B 2 O 3 .

[0023] The preparation process of HfB is used to prepare 2 The carrier can obtain carrier particles with small particle size with a shorter ball milling time and a relatively low ball milling speed. In some preferred embodiments, in step 1c), the ball milling speed is 200-400 r / min and the time is 2-4 h. In some embodiments, the HfB prepared by the present invention 2 The carrier has a particle size of 1.6 μm or less.

[0024] In some preferred embodiments, in step 2), based on the HfB 2 The mass of the carrier, the ruthenium loading is 2-4wt.%. The ruthenium-based catalyst prepared by the preparation method of the present invention controls the ruthenium loading within the above range, not only does not require a large amount of ruthenium loading, but the obtained catalyst has good catalytic activity and stability for ammonia synthesis under mild conditions.

[0025] In some embodiments, in step 2), the impregnation liquid is an aqueous solution of a precursor of ruthenium ions. Preferably, ethanol is also added to the impregnation liquid. The amount of ethanol is not particularly limited. For example, in some embodiments, the amount of ethanol is 3-10 times the volume of the aqueous solution of the precursor.

[0026] Specifically, the precursor of the ruthenium ion can be a precursor type conventionally used in the art, for example, one or more selected from but not limited to ruthenium acetylacetonate, ruthenium nitrosyl nitrate, ruthenium trichloride, and ruthenium acetate.

[0027] The second aspect of the present invention provides a ruthenium-based catalyst for ammonia synthesis reaction prepared by the preparation method described above. The catalyst has good catalytic activity and stability when used in ammonia synthesis reaction.

[0028] A third aspect of the present invention provides the use of the ruthenium-based catalyst described above in an ammonia synthesis reaction. Preferably, the ruthenium-based catalyst is particularly suitable for catalyzing the synthesis of ammonia from nitrogen and hydrogen, and not only exhibits good catalytic activity under mild conditions, but also has excellent catalytic activity stability.

[0029] The technical solution provided by the present invention has the following beneficial effects:

[0030] 1) The preparation method provided by the present invention comprises: 2 and boron in a molar ratio of less than 0.3 and greater than 0 and prepared HfB by a first heating reduction-hot water treatment-second heating reduction-ball milling method 2 The carrier can easily obtain a carrier with a small particle size and good mechanical strength, and based on the carrier, a ruthenium-based catalyst with high catalytic activity and good stability for ammonia synthesis can be obtained.

[0031] 2) Compared with traditional preparation methods, the preparation process provided by the present invention has lower energy consumption and cost, and is more in line with the principle of green and sustainable development.

[0032] 3) The ruthenium-based catalyst prepared by the present invention has excellent electrical conductivity, mechanical strength and catalytic activity for ammonia synthesis. The catalyst has good catalytic stability for ammonia synthesis, low preparation cost and simple preparation process.

[0033] 4) The reagents used in the preparation method provided by the present invention are easily available and non-toxic and harmless, the process is simple, and it is easy to mass produce and realize industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 HfB prepared in one embodiment 2 、Ru / HfB 2 XRD pattern;

[0035] Figure 2 The Ru / HfB prepared in one embodiment is 2 Electron micrograph of the catalyst;

[0036] Figure 3 The Ru / HfB prepared in one embodiment is 2 Energy spectrum of

[0037] Figure 4 It is a summary diagram of the performance of the catalysts in various embodiments and comparative examples at 400°C and 1 MPa. DETAILED DESCRIPTION

[0038] In order to facilitate the understanding of the present invention, the present invention will be further described below in conjunction with examples. It should be understood that the following examples are only for a better understanding of the present invention and do not mean that the present invention is limited to the following examples.

[0039] Where specific experimental steps or conditions are not specified in the examples, the corresponding conventional experimental steps or conditions in the art can be used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.

[0040] In the following examples and comparative examples, HfO 2 and boron are commercially available products, HfO 2 The purity is >99.5%, and the BET specific surface area is about 11.3m 2 / g, average particle size 100nm; the boron used is amorphous boron with a purity of >96% and an average particle size of <1μm.

[0041] Example 1

[0042] A ruthenium-based catalyst for ammonia synthesis reaction, the preparation process of which comprises the following steps:

[0043] 1) Preparation of carrier:

[0044] Weigh 52.561g HfO 2 and 11.297 g of boron in a polyethylene bottle using ethanol (20 ml) and Si 3 N 4 The balls (4 pieces) were mixed and then dried by rotary evaporation to remove the ethanol. The dried powder mixture was dry-pressed into a disc (about 10 mm in diameter and 10 mm thick). The disc was then placed in a graphite crucible and heated to 1600°C in a graphite element furnace at a heating rate of 10°C / min and maintained at this temperature for 1 hour. The heat-treated disc was immersed in hot water (temperature of 80°C) for 1 hour, after which the disc was placed in a graphite crucible again, heated to 1600°C and maintained for 1 hour, and then cooled naturally. The cooled disc was placed in a ball mill and ground for 2 hours at a speed of 300r·min. -1 , and obtain HfB 2 The particle size of carrier 1 was tested to be 1.5 μm.

[0045] 2) Preparation of catalyst:

[0046] Pour an appropriate amount of ethanol (10 ml of ethanol) into a petri dish, then pour in 2 mL of a 0.989 M ruthenium trichloride aqueous solution, stir thoroughly, and obtain an impregnation solution. Add 10 g of carrier 1 to the impregnation solution, and stir the mixture at 200 r / min for 6 h using a magnetic stirrer. After stirring, filter out the upper layer of liquid, and then dry the residue with a high-voltage electric field drying device under an electric field strength of 20 kV / cm for 8 h to obtain Ru / HfB for ammonia synthesis reaction. 2Catalyst 1, wherein the loading amount of ruthenium is 2% based on the mass of carrier 1.

[0047] 3) Application of catalyst 1 in ammonia synthesis reaction:

[0048] 0.2 g of catalyst 1 was weighed and reacted in a continuous flow micro fixed bed reactor at a reaction pressure of 1 MPa, a temperature of 400 °C, and a mass space velocity of 60000 mL g -1 h -1 The ammonia synthesis performance was measured, and the amount of substance introduced was n(N 2 ):n(H 2 )=1:3N 2 and H 2 At the beginning of the reaction, the ammonia synthesis rate of catalyst 1 (corresponding to Figure 4 The "highest activity" in the above text is 33.4 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 1 (corresponding to Figure 4 The "400-hour activity" in the above text is 33.1 mmol gcat -1 h -1 .

[0049] Example 2

[0050] A ruthenium-based catalyst for ammonia synthesis reaction, the preparation process of which comprises the following steps:

[0051] 1) Preparation of carrier:

[0052] Weigh 42.121 g HfO 2 and 11.297 g of boron in a polyethylene bottle using ethanol (10 ml) and Si 3 N 4 The balls (4 pieces) are mixed and then dried by rotary evaporation to remove the ethanol. The dried powder mixture is dry-pressed into a disc (about 10 mm diameter and 10 mm thick). The disc is then placed in a graphite crucible and heated to 1550°C in a graphite element furnace at a heating rate of 10°C / min and maintained at this temperature for 1 hour. The heat-treated disc is immersed in hot water (temperature of 80°C) for 20 minutes, after which the disc is placed in the graphite crucible again, heated to 1550°C and maintained for 2 hours, and then cooled naturally. The cooled disc is placed in a ball mill and milled at 200r·min -1 Grind for 2 hours to obtain HfB 2 The particle size of carrier 2 was tested to be 1.53 μm.

[0053] 2) Preparation of catalyst:

[0054] Pour an appropriate amount of ethanol (10 mL of ethanol) into a petri dish, then pour in 2 mL of 0.989 M ruthenium acetylacetonate aqueous solution, stir thoroughly, and obtain an impregnation solution. Add 10 g of carrier 2 to the impregnation solution, and stir the mixture at 200 r / min for 6 h using a magnetic stirrer. After stirring, filter out the upper layer of liquid, and then dry the residue with a high-voltage electric field drying device under an electric field strength of 20 kV / cm for 8 h to obtain Ru / HfB for ammonia synthesis reaction. 2 Catalyst 2, wherein the loading amount of ruthenium is 2% based on the mass of carrier 1.

[0055] 3) Application of catalyst 2 in ammonia synthesis reaction:

[0056] 0.2 g of catalyst 2 was weighed and reacted in a continuous flow micro fixed bed reactor at a reaction pressure of 1 MPa, a temperature of 400 °C, and a mass space velocity of 60000 mL g -1 h -1 The ammonia synthesis performance was measured, and the amount of substance introduced was n(N 2 ):n(H 2 )=1:3N 2 and H 2 At the beginning of the reaction, the ammonia synthesis rate of catalyst 2 was 31.9 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 2 was 31.4 mmol gcat -1 h -1 .

[0057] Example 3

[0058] A ruthenium-based catalyst for ammonia synthesis reaction, the preparation process of which comprises the following steps:

[0059] 1) Preparation of carrier:

[0060] Weigh 42.121 g HfO 2 and 11.297 g of boron in a polyethylene bottle using ethanol (20 mL) and Si 3 N 4 The balls (4 pieces) are mixed and then dried by rotary evaporation to remove the ethanol. The dried powder mixture is dry-pressed into a disc (about 10 mm diameter and 10 mm thick). The disc is then placed in a graphite crucible and heated to 1700°C in a graphite element furnace at a heating rate of 10°C / min and maintained at this temperature for 1 hour. The heat-treated disc is immersed in hot water (temperature of 80°C) for 20 minutes, after which the disc is placed in the graphite crucible again, heated to 1550°C and maintained for 2 hours, and then cooled naturally. The cooled disc is placed in a ball mill and milled at 400r·min-1 Grind for 4 hours to obtain HfB 2 The particle size of carrier 3 was tested to be 1.55 μm.

[0061] 2) Preparation of catalyst:

[0062] Pour an appropriate amount of ethanol (10 mL of ethanol) into a petri dish, then pour in 2 mL of 0.989 M ruthenium acetate aqueous solution, stir thoroughly, and obtain an impregnation solution. Add 10 g of carrier 3 to the above impregnation solution, and stir the mixture at 300 r / min for 6 h using a magnetic stirrer. After stirring, filter out the upper layer of liquid, and then dry the residue with a high-voltage electric field drying device under an electric field strength of 15 kV / cm for 8 h to obtain Ru / HfB for ammonia synthesis reaction. 2 Catalyst 3, wherein the loading amount of ruthenium is 2% based on the mass of carrier 1.

[0063] 3) Application of catalyst 3 in ammonia synthesis reaction:

[0064] 0.2 g of catalyst 3 was weighed and reacted in a continuous flow micro fixed bed reactor at a reaction pressure of 1 MPa, a temperature of 400 °C, and a mass space velocity of 60000 mL g -1 h -1 The ammonia synthesis performance was measured, and the amount of substance introduced was n(N 2 ):n(H 2 )=1:3N 2 and H 2 At the beginning of the reaction, the ammonia synthesis rate of catalyst 3 was 30.6 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 3 was 30.2 mmol gcat -1 h -1 .

[0065] Example 4

[0066] A ruthenium-based catalyst for ammonia synthesis reaction, the preparation process of which comprises the following steps:

[0067] 1) Preparation of carrier:

[0068] Weigh 42.121 g HfO 2 and 11.297 g of boron in a polyethylene bottle using ethanol (20 mL) and Si 3 N 4The balls (4 pieces) are mixed and then dried by rotary evaporation to remove the ethanol. The dried powder mixture is dry-pressed into a disc (about 10 mm diameter and 10 mm thick). The disc is then placed in a graphite crucible and heated to 1700°C in a graphite element furnace at a heating rate of 10°C / min and maintained at this temperature for 1 hour. The heat-treated disc is immersed in hot water (temperature of 80°C) for 80 minutes, after which the disc is placed in the graphite crucible again, heated to 1700°C and maintained for 2 hours, and then cooled naturally. The cooled disc is placed in a ball mill and milled at 400r·min -1 Grind for 4 hours to obtain HfB 2 The particle size of carrier 4 was tested to be 1.58 μm.

[0069] 2) Preparation of catalyst:

[0070] Pour an appropriate amount of ethanol (10 mL of ethanol) into a petri dish, then pour in 2 mL of a 0.989 M nitrosyl nitrate ruthenium aqueous solution, stir thoroughly, and obtain an impregnation solution. Add 10 g of carrier 4 to the impregnation solution, and stir the mixture at 300 r / min for 6 h using a magnetic stirrer. After stirring, filter out the upper layer of liquid, and then dry the residue with a high-voltage electric field drying device under an electric field strength of 15 kV / cm for 8 h to obtain Ru / HfB for ammonia synthesis reaction. 2 Catalyst 4, wherein the loading amount of ruthenium is 2% based on the mass of carrier 1.

[0071] 3) Application of catalyst 4 in ammonia synthesis reaction:

[0072] 0.2 g of catalyst 4 was weighed and reacted in a continuous flow micro fixed bed reactor at a reaction pressure of 1 MPa, a temperature of 400 °C, and a mass space velocity of 60000 mL g -1 h -1 The ammonia synthesis performance was measured, and the amount of substance introduced was n(N 2 ):n(H 2 )=1:3N 2 and H 2 At the beginning of the reaction, the ammonia synthesis rate of catalyst 4 was 30.3 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 4 was 29.7 mmol gcat -1 h -1 .

[0073] Comparative Example 1: HfO 2 / boron molar ratio is 0.5

[0074] Comparative Example 1 is compared with Example 1 to illustrate the preparation of the carrier HfO2 Importance of the boron / boron molar ratio.

[0075] A ruthenium-based catalyst for ammonia synthesis reaction and a preparation method and application thereof, comprising the following steps:

[0076] 1) Preparation of carrier:

[0077] Weigh 105.303 g HfO 2 and 11.297 g of boron in a polyethylene bottle using ethanol (20 mL) and Si 3 N 4 The balls (4 pieces) are mixed and then dried by rotary evaporation to remove the ethanol. The dried powder mixture is pressed into a disc (about 10 mm in diameter and 10 mm thick). The disc is then placed in a graphite crucible and heated to 1600°C in a graphite element furnace at a heating rate of 10°C / min and maintained for 1 hour. The heat-treated disc is immersed in 80°C hot water for 60 minutes, after which the disc is placed in the graphite crucible again, heated to 1600°C and maintained for 1 hour, and cooled naturally. The cooled disc is placed in a ball mill and milled at 400r·min -1 The ruthenium-based catalyst HfB was obtained for the synthesis of ammonia at a speed of 4 h. 2 Carrier 5, the tested particle size is 2.55 μm. The carrier prepared in this comparative example was ball milled at a higher speed for a longer time, and the resulting carrier particle size was still larger than that of Example 1.

[0078] 2) Preparation of catalyst:

[0079] Pour an appropriate amount of ethanol (10 ml of ethanol) into a petri dish, then pour in 2 mL of a 0.989 M ruthenium trichloride aqueous solution, stir thoroughly, and obtain an impregnation solution. Add 10 g of carrier 5 to the impregnation solution, and stir the mixture at 200 r / min for 6 h using a magnetic stirrer. After stirring, filter out the upper layer of liquid, and then use a high-voltage electric field with an intensity of 20 kV / cm to dry the residue for 8 h to obtain Ru / HfB for ammonia synthesis reaction. 2 Catalyst 5.

[0080] 3) Application of catalyst 5 in ammonia synthesis reaction:

[0081] 0.2 g of catalyst 5 was weighed and reacted in a continuous flow micro fixed bed reactor at a reaction pressure of 1 MPa, a temperature of 400 °C, and a mass space velocity of 60000 mL g -1 h -1 The ammonia synthesis performance was measured, and the amount of substance introduced was n(N 2 ):n(H 2 )=1:3N 2 and H 2At the beginning of the reaction, the ammonia synthesis rate of catalyst 5 was 22.2 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 5 was 21.2 mmol gcat -1 h -1 .

[0082] Comparative Example 2: No hot water treatment

[0083] Comparative Example 2 is used to illustrate the importance of hot water treatment when preparing the carrier by comparison with Example 1.

[0084] 1) Preparation of carrier:

[0085] Weigh 52.561g HfO 2 and 11.297 g of boron in a polyethylene bottle using ethanol (20 ml) and Si 3 N 4 The balls (4 pieces) were mixed and then dried by rotary evaporation to remove the ethanol. The dried powder mixture was pressed into a disc (about 10 mm in diameter and 10 mm thick). The disc was then placed in a graphite crucible and heated to 1600°C in a graphite element furnace at a heating rate of 10°C / min and maintained for 2 hours. After natural cooling, the cooled disc was placed in a ball mill at 400 r·min -1 The ruthenium-based catalyst HfB was obtained for the synthesis of ammonia at a speed of 4 h. 2 Carrier 6, the tested particle size is 2.75 μm. The carrier prepared in this comparative example was ball milled at a higher speed for a longer time, and the resulting carrier particle size was still larger than that of Example 1.

[0086] 2) Preparation of catalyst:

[0087] Pour an appropriate amount of 10 ml of ethanol into a petri dish, then pour in 2 mL of a 0.989 M ruthenium trichloride aqueous solution, stir thoroughly, and obtain an impregnation solution. Add 10 g of carrier 6 to the impregnation solution, and stir the mixture at 200 r / min for 6 h using a magnetic stirrer. After stirring, filter out the upper layer of liquid, and then use a high-voltage electric field drying device with an intensity of 20 kV / cm to dry the residue for 8 h to obtain Ru / HfB for ammonia synthesis reaction. 2 Catalyst 6. The amount of ruthenium loaded is 2% based on the mass of carrier 1.

[0088] 3) Application of Catalyst 6 in Ammonia Synthesis Reaction: 0.2 g of Catalyst 6 was weighed and the ammonia synthesis performance was measured in a continuous flow micro fixed bed reactor at a reaction pressure of 1 MPa, a temperature of 400 °C, and a mass space velocity of 60000 mL g-1 h-1. The amount of substance introduced was n(N 2):n(H 2 )=1:3N 2 and H 2 At the beginning of the reaction, the ammonia synthesis rate of catalyst 6 was 21.3 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 6 was 20.4 mmol gcat -1 h -1 .

[0089] Comparative Example 3: No high voltage electric field is used

[0090] Comparative Example 3 illustrates the importance of using a high voltage electric field to dry the catalyst when preparing it, by comparison with Example 1.

[0091] 1) Preparation of carrier:

[0092] Weigh 52.561g HfO 2 and 11.297 g of boron in a polyethylene bottle using 20 ml of ethanol and Si 3 N 4 The balls (4 pieces) were mixed and then dried by rotary evaporation to remove the ethanol. The dried powder mixture was pressed into a disc (about 10 mm in diameter and 10 mm thick). The disc was then placed in a graphite crucible and heated to 1600°C in a graphite element furnace at a heating rate of 10°C / min and maintained for 1 hour. The heat-treated disc was immersed in 80°C hot water for 60 minutes, and then the disc was placed in the graphite crucible again, heated to 1600°C and maintained for 1 hour. After natural cooling, the cooled disc was placed in a ball mill at 400r·min -1 The ruthenium-based catalyst HfB was obtained for the synthesis of ammonia at a speed of 4 h. 2 Carrier 7, tested particle size is 1.56 μm.

[0093] 2) Preparation of catalyst:

[0094] Pour 10 ml of ethanol into a petri dish, then pour in 2 mL of 0.989 M ruthenium trichloride aqueous solution, stir thoroughly, and obtain an impregnation solution. Add 10 g of carrier 7 to the above impregnation solution, and stir the mixture at 200 r / min for 6 h using a magnetic stirrer. After stirring, filter out the upper layer of liquid, and then use an oven at 120 ° C to dry the filter residue for 8 h. Obtain Ru / HfB for synthetic ammonia reaction 2 Catalyst 7. The amount of ruthenium loaded is 2% based on the mass of carrier 1.

[0095] 3) Application of catalyst 7 in ammonia synthesis reaction: 0.2 g of catalyst 7 was weighed and reacted in a continuous flow micro fixed bed reactor at a reaction pressure of 1 MPa, a temperature of 400 °C, and a mass space velocity of 60000 mL g -1 h -1 The ammonia synthesis performance was measured, and the amount of substance introduced was n(N 2 ):n(H 2 )=1:3N 2 and H 2 At the beginning of the reaction, the ammonia synthesis rate of catalyst 7 was 28.2 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 7 was 27.8 mmol gcat -1 h -1 .

[0096] Comparative Example 4: No ball milling was used in the preparation of the carrier

[0097] Comparative Example 4 illustrates the importance of ball milling when preparing a carrier by comparing it with Example 1.

[0098] A ruthenium-based catalyst for ammonia synthesis reaction and a preparation method and application thereof, comprising the following steps:

[0099] 1) Preparation of carrier:

[0100] Weigh 52.561g HfO 2 and 11.297 g of boron in a polyethylene bottle using 20 ml of ethanol and Si 3 N 4 The balls (4 pieces) were mixed and then dried by rotary evaporation to remove the ethanol. The dried powder mixture was pressed into a disc (about 10 mm in diameter and 10 mm thick). The disc was then placed in a graphite crucible and heated to 1600°C at a heating rate of 10°C / min in a graphite element furnace and kept for 1 hour. The heat-treated disc was immersed in 80°C hot water for 60 minutes, and then the disc was placed in a graphite crucible again, heated to 1600°C and kept for 1 hour, and then cooled naturally to obtain a ruthenium-based catalyst HfB for ammonia synthesis reaction. 2 Carrier 8, tested particle size is 1.65 μm.

[0101] 2) Preparation of catalyst:

[0102] Pour 10 ml of ethanol into a petri dish, then pour 2 mL of 0.989 M ruthenium trichloride aqueous solution, stir thoroughly, and obtain an impregnation solution. Add 10 g of carrier 8 to the impregnation solution, and stir the mixture at 200 r / min for 6 h using a magnetic stirrer. After stirring, filter out the upper layer of liquid, and then use a high-voltage electric field drying with an intensity of 20 kV / cm to dry the residue for 8 h to obtain Ru / HfB for ammonia synthesis reaction. 2 Catalyst 8. The loading amount of ruthenium is 2% based on the mass of carrier 1.

[0103] 3) Application of catalyst 8 in ammonia synthesis reaction:

[0104] 0.2 g of catalyst 8 was weighed and reacted in a continuous flow micro fixed bed reactor at a reaction pressure of 1 MPa, a temperature of 400 °C, and a mass space velocity of 60000 mL g -1 h -1 The ammonia synthesis performance was measured, and the amount of substance introduced was n(N 2 ):n(H 2 )=1:3N 2 and H 2 At the beginning of the reaction, the ammonia synthesis rate of catalyst 8 was 20.9 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 8 was 20 mmol gcat -1 h -1 .

[0105] Comparative Example 5: Graphite element furnace temperature is 1100°C

[0106] Comparative Example 5 is used to illustrate the importance of the final temperature of the graphite element furnace when preparing the carrier by comparing it with Example 1.

[0107] A ruthenium-based catalyst for ammonia synthesis reaction and a preparation method and application thereof, comprising the following steps:

[0108] 1) Preparation of carrier:

[0109] Weigh 52.561g HfO 2 and 11.297 g of boron in a polyethylene bottle using 20 ml of ethanol and Si 3 N 4The balls (4 pieces) were mixed and then dried by rotary evaporation to remove the ethanol. The dried powder mixture was dry-pressed into a disc (about 10 mm in diameter and 10 mm thick). The disc was then placed in a graphite crucible and heated to 1600°C in a graphite element furnace at a heating rate of 10°C / min and maintained for 1 hour. The heat-treated disc was immersed in 80°C hot water for 60 minutes, after which the disc was placed in a graphite crucible again, heated to 1100°C and maintained for 1 hour, and then cooled naturally. The cooled disc was placed in a ball mill and ground for 2 hours at a speed of 300r·min. -1 , and obtain the ruthenium-based catalyst HfB for the synthesis of ammonia 2 Carrier 9, tested particle size is 4.75 μm.

[0110] 2) Preparation of catalyst:

[0111] Pour 10 ml of ethanol into a petri dish, then pour 2 mL of 0.989 M ruthenium trichloride aqueous solution, stir thoroughly, and obtain an impregnation solution. Add 10 g of carrier 9 to the impregnation solution, and stir the mixture at 200 r / min for 6 h using a magnetic stirrer. After stirring, filter out the upper layer of liquid, and then use a high-voltage electric field drying device with an intensity of 20 kV / cm to dry the residue for 8 h to obtain Ru / HfB for ammonia synthesis reaction. 2 Catalyst 9. The ruthenium loading is 2% based on the mass of the carrier 1.

[0112] 3) Application of catalyst 9 in ammonia synthesis reaction:

[0113] 0.2 g of catalyst 9 was weighed and reacted in a continuous flow micro fixed bed reactor at a reaction pressure of 1 MPa, a temperature of 400 °C, and a mass space velocity of 60000 mL g -1 h -1 The ammonia synthesis performance was measured, and the amount of substance introduced was n(N 2 ):n(H 2 )=1:3N 2 and H 2 At the beginning of the reaction, the ammonia synthesis rate of catalyst 9 was 5.5 mmol gcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate of catalyst 9 was 2.5 mmol gcat -1 h -1 .

[0114] Comparative Example 6: Direct use of HfB 2 reaction

[0115] Weigh 0.2 g of HfB prepared in step 1) of Example 1 2The carrier 1 was used as a catalyst in a continuous flow micro fixed bed reactor at a reaction pressure of 1 MPa, a temperature of 400 °C, and a mass space velocity of 60000 mL g -1 h -1 The ammonia synthesis performance was measured, and the amount of substance introduced was n(N 2 ):n(H 2 )=1:3N 2 and H 2 In the initial stage of the reaction, HfB 2 The ammonia synthesis rate is 2.5mmolgcat -1 h -1 After 400 hours of reaction, the ammonia synthesis rate was 0.8 mmol gcat -1 h -1 .

[0116] The carrier and catalyst prepared in the above examples were subjected to XRD analysis, wherein the results of Example 1 are representative, and the results are as follows: Figure 1 As shown in the figure, the prepared HfB 2 There is no HfO in carrier 1 2 residual, and Ru was effectively loaded onto HfB 2 The catalyst prepared in the above embodiments of the present invention was imaged using a transmission electron microscope of the instrument model Tecnai G2 F30 S-Twin, wherein the results of Example 1 are representative, and the results are shown in FIG. Figure 2 ,in Figure 2 The left picture is bright field imaging, and the right picture is dark field imaging; combined Figure 1 The XRD patterns and Figure 2 As can be seen from the electron microscope images, both of them well confirm the final prepared HfB 2 There is no HfO in carrier 1 2 The residual also indicates that Ru is effectively loaded onto HfB 2 And the dispersion is very good; further from Figure 3 As shown in the energy spectrum, Ru in HfB 2 The dispersion on carrier 1 is very uniform.

[0117] The maximum activity and 400-hour activity results (expressed in terms of ammonia synthesis rate) of the catalysts in the above-mentioned embodiments and comparative examples during the application process are summarized in Figure 4 In. From Figure 4 It can be seen that the catalyst prepared by the method of the present invention has better catalytic activity and stability for ammonia synthesis.

[0118] It is easy to understand that the above embodiments are only examples for clear explanation and do not mean that the present invention is limited thereto. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from this are still within the protection scope of the present invention.

Claims

1. A method for preparing a ruthenium-based catalyst for ammonia synthesis reaction, characterized in that: The steps include: 1) The HfB2 carrier is prepared by a method comprising the following steps: 1a) mixing HfO2 and boron in a molar ratio of less than 0.3 and greater than 0, and pressing the obtained powder mixture to obtain a pressed product and subjecting it to a first heating reduction; 1b) then immersing the pressed product in hot water for treatment, and then taking out the pressed product and performing a second heating reduction; the temperature conditions of the first heating reduction and the second heating reduction are 1550-1700° C. respectively; 1c) grinding the pressed product after the treatment in step 1b) by ball milling to obtain the HfB2 carrier; 2) The HfB2 carrier obtained in step 1) is impregnated in an impregnation solution containing ruthenium ions, and then dried to obtain the ruthenium-based catalyst.

2. The preparation method according to claim 1, characterized in that: In step 2), the drying is performed using a high-voltage electric field drying technique. Preferably, the drying is performed at an electric field strength of 10 to 20 kV / cm.

3. The preparation method according to claim 1 or 2, characterized in that: In step 1a), the HfO2 and boron are mixed in the presence of ethanol and Si3N4 balls, and in step 1a), the powder mixture is dried before the pressing.

4. The preparation method according to claim 1 or 2, characterized in that: The time for the first heating reduction in step 1a) and the second heating reduction in step 1b) is 1-3 hours respectively.

5. The preparation method according to claim 4, characterized in that: In step 1a), when the first heating reduction is performed, the heating rate to 1550-1700° C. is 5-15° C. / min.

6. The preparation method according to claim 1 or 2, characterized in that: In step 1b), the treatment time in the hot water is 20 to 100 minutes; And / or, in step 1c), the rotation speed of the ball mill is 200-400 r / min, and the time is 2-4 h.

7. The preparation method according to claim 1 or 2, characterized in that: In step 2), based on the mass of the HfB2 carrier, the loading amount of ruthenium is 2 to 4 wt.%.

8. The preparation method according to claim 1 or 2, characterized in that: In step 2), the impregnation solution is a precursor aqueous solution of ruthenium ions; preferably, ethanol is also added to the impregnation solution; Preferably, the precursor of the ruthenium ion is selected from one or more of ruthenium acetylacetonate, ruthenium nitrosyl nitrate, ruthenium trichloride, and ruthenium acetate.

9. A ruthenium-based catalyst for ammonia synthesis reaction obtained by the preparation method according to any one of claims 1 to 8.

10. Use of the ruthenium-based catalyst according to claim 9 in an ammonia synthesis reaction, preferably, the ruthenium-based catalyst is used to catalyze the synthesis of ammonia from nitrogen and hydrogen.

Citation Information

Patent Citations

  • High-performance Ru-based synthetic ammonia catalyst as well as preparation method and application thereof

    CN114733551A

  • Ruthenium-based mild ammonia synthesis catalyst as well as preparation method and application thereof

    CN114789053A

  • High-temperature anti-sintering catalyst and synthesis method thereof

    CN112403461A

  • Preparation method of high-purity superfine hafnium boride powder and hafnium boride powder

    CN112919913A

  • Preparation method and application of nano-porous copper catalyst for acetylene hydrochlorination reaction

    CN113171773A