Ag-based deoxidation catalyst as well as preparation method and application thereof

By controlling the content and proportion of the active phase on the surface of the AgxO catalyst, an efficient Ag-based deoxygenation catalyst is constructed, which solves the problems of low deoxidation rate and high hydrogen demand of existing deoxygenation catalysts, and achieves high-efficiency, low-cost deep oxygen removal effects.

CN118767912APending Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310376044.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The deoxygenation rate of existing deoxygenation catalysts is not high, or a relatively high proportion of hydrogen is required to achieve deep deoxidation. Furthermore, the cost of precious metal catalysts is high and the deep deoxygenation efficiency is low.

Method used

By controlling the content and proportion of the AgxO (Ag/AgO/Ag2O) catalyst surface active phase, an efficient catalyst surface active phase is constructed to improve oxygen adsorption and activation capabilities. Ag-based deoxygenation catalysts are used, including catalyst carrier, active component Ag, AgO, Ag2O and additives are prepared through impregnation and roasting reduction processes to reduce reaction pressure and hydrogen demand.

Benefits of technology

It achieves high H2 activation capacity and O2 adsorption-activation capacity, reduces operating costs, improves deoxygenation efficiency, and can deeply remove extremely low trace oxygen especially under low hydrogen conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767912A_ABST
    Figure CN118767912A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of catalyst preparation, and discloses an Ag-based deoxidation catalyst as well as a preparation method and application thereof. The Ag-based deoxidation catalyst comprises a catalyst carrier, active components and an auxiliary agent, the active components and the auxiliary agent are attached to the catalyst carrier, and the active components comprise at least two of Ag, AgO and Ag2O. According to the technical scheme, by effectively controlling the content, the type and the proportion of AgxO (Ag / AgO / Ag2O) on the surface of the catalyst, the effective number of active phases on the surface of the Ag-based catalyst is efficiently constructed, adsorption and activation of oxygen are promoted, and meanwhile the deoxidation efficiency of the catalyst is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst preparation, and in particular to an Ag-based deoxidation catalyst and a preparation method and application thereof. Background Art

[0002] Catalytic oxidation reaction is one of the most common chemical reactions in the chemical production process. The incomplete reaction of raw materials (low-carbon hydrocarbons) and oxidants (air, oxygen, ozone, etc.) causes a large amount of oxidants to be enriched in the recycling of raw materials, which in turn leads to a great risk of explosion in the chemical production process. The "Petrochemical Combustible Gas Emission System Design Specification" stipulates that combustible gases with an oxygen content greater than 2% (v%) should not be discharged into the plant's combustible gas emission system, so the efficient treatment of oxygen in oxygen-containing tail gas has become a key issue that needs to be solved urgently.

[0003] At present, inert gas dilution emission has become the main method of oxygen treatment, which not only increases operating costs (large amounts of nitrogen consumption), but also pollutes the environment with VOCs emissions. In recent years, catalytic oxidation has been widely studied due to its great advantages in economy, environmental protection, and energy saving; however, the high price of precious metal catalysts and the low efficiency of deep deoxygenation still exist. Therefore, the development of metal catalysts with high catalytic oxidation activity has received extensive attention from researchers.

[0004] Patent application CN111905729A discloses an organic hydrocarbon deoxygenation catalyst and a preparation method thereof, which is used for removing ethylene and extremely trace oxygen (≦1000ppm) in ethylene. The deoxygenation catalyst requires a higher hydrogen content (6000ppm) during use, and the remaining hydrogen causes waste. The deoxygenation efficiency is low (1ppm) at a lower temperature (100°C).

[0005] Patent application CN106378144B discloses a manganese-based deoxidizer with cerium-based oxide as carrier, its preparation method and application. The catalyst is composed of active components, carrier and binder, wherein the active components are Cu and MnO, accounting for 35%-75% of the total weight of the catalyst; the carrier is CeO2 or CeO2-MOx composite oxide, accounting for 20%-50% of the total weight of the catalyst. Under a pressure of 0.4MPa, ethylene gas with a very small amount of oxygen 1000ppm O2 is introduced to carry out a deoxidation experiment.

[0006] Patent application CN100513367C discloses a deoxidation catalyst with MnO / Mn3O4 as active components, and adding active promoters alkaline earth metal oxides and aluminum oxide. The deoxidation catalyst can remove 1-2000ppm of low-content oxygen in propylene, ethylene, etc. Under a reaction pressure of 0.4MPa, the deoxidation catalyst has a very small amount of oxygen of 1000ppm O2, and the tail oxygen after deoxidation is less than 1ppm.

[0007] In the preparation of deoxygenation metal catalysts, the currently reported removal of extremely low trace oxygen content (1000 ppm) per unit time requires a higher proportion of hydrogen to achieve deep removal of oxygen. Summary of the invention

[0008] The purpose of the present invention is to overcome the problem that the deoxidation rate of the deoxidation catalyst in the prior art is not high, or that a high proportion of hydrogen is required to achieve deep deoxidation, and to provide an Ag-based deoxidation catalyst and its preparation method and application. x The content, type and ratio of Ag / AgO / Ag2O can effectively construct the effective number of active phases on the surface of Ag-based catalysts, promote the adsorption and activation of oxygen, and thus improve the deoxygenation efficiency of the catalyst.

[0009] In order to achieve the above objectives, the present invention provides an Ag-based deoxidation catalyst, comprising a catalyst carrier and active components and additives attached to the catalyst carrier, wherein the active components are at least two of Ag, AgO and Ag2O.

[0010] Preferably, relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal element is 1-10 parts by weight, preferably 3-5 parts by weight; the content of the auxiliary agent in terms of metal element is 0.5-3 parts by weight, preferably 1-2 parts by weight.

[0011] Preferably, the active component is a combination of Ag and AgO, and the molar ratio of Ag to AgO is 1:1.5-2.5; or

[0012] The active component is a combination of AgO and Ag2O, and the molar ratio of AgO to Ag2O is 1:1.2-3; or

[0013] The active component is a combination of Ag and Ag2O, and the molar ratio of Ag to Ag2O is 1:1.8-3; or

[0014] The active component is a combination of Ag, AgO and Ag2O, and the molar ratio of Ag, AgO and Ag2O is 1:(1.1-1.5):(0.5-0.8).

[0015] Preferably, the catalyst carrier is at least one of SiO2, Al2O3 and molecular sieve.

[0016] Preferably, the auxiliary agent is at least one of NaNO3, Mg(NO3)2, Zr(NO3)4, KNO3 and Cu(NO3)2.

[0017] The second aspect of the present invention provides a method for preparing the above-mentioned Ag-based deoxidation catalyst, which comprises: adhering a Ag component precursor and an auxiliary agent to a catalyst carrier, and then calcining and reducing.

[0018] Preferably, the process of attaching the Ag component precursor and the auxiliary agent to the catalyst carrier is carried out by impregnation.

[0019] Preferably, the impregnation is carried out by equal volume impregnation, excess impregnation or stepwise impregnation.

[0020] Preferably, the Ag component precursor is AgNO3.

[0021] Preferably, the calcination conditions include: temperature of 300-500° C. and time of 3-8 h.

[0022] Preferably, the reducing atmosphere is H2, a combination of H2 and CO, or a mixed atmosphere with different hydrogen concentrations.

[0023] Preferably, the reduction conditions include: catalyst heating rate of 2-15°C / min, reduction temperature of 100-500°C, and reduction time of 1-12h.

[0024] The third aspect of the present invention provides the use of the above-mentioned Ag-based deoxygenation catalyst in the deoxygenation process of olefin gas containing oxygen.

[0025] According to the technical solution of the present invention, by effectively controlling the Ag on the catalyst surface x The content, type and ratio of Ag / AgO / Ag2O can effectively construct the effective number of active phases on the surface of Ag-based catalysts, promote the adsorption and activation of oxygen, and thus improve the deoxygenation efficiency of the catalyst.

[0026] Compared with the prior art, the technical solution of the present invention has the following advantages:

[0027] (1) The Ag-based deoxidation catalyst has high H2 activation ability and O2 adsorption-activation ability;

[0028] (2) The Ag-based deoxidation catalyst has the advantages of low reaction pressure and low required hydrogen content;

[0029] (3) Compared with other precious metal catalyst (Pt, Pd) deoxidation technologies, metal Ag-based deoxidation catalysts greatly reduce operating costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Schematic diagram of the Ag-based deoxidation catalyst of the present invention. DETAILED DESCRIPTION

[0031] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0032] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0033] In the present invention, unless otherwise specified, the concentration "%" of a gas refers to "volume %"; the "space velocity" refers to "volume space velocity"; and the pressure refers to absolute pressure.

[0034] like Figure 1 As shown, the Ag-based deoxidation catalyst of the present invention includes a catalyst carrier and active components and additives attached to the catalyst carrier, wherein the active components are at least two of Ag, AgO and Ag2O.

[0035] In the Ag-based deoxidation catalyst of the present invention, the content of the active component in terms of metal elements can be 1-10 parts by weight, preferably 3-5 parts by weight, relative to 100 parts by weight of the catalyst carrier; the content of the auxiliary agent in terms of metal elements can be 0.5-3 parts by weight, preferably 1-2 parts by weight.

[0036] According to the Ag-based deoxidation catalyst of the present invention, in some embodiments, the active component is a combination of Ag and AgO, and the molar ratio of Ag to AgO is 1:1.5-2.5, preferably 1:1.8-2.3.

[0037] According to the Ag-based deoxygenation catalyst of the present invention, in other embodiments, the active component is a combination of AgO and Ag2O, and the molar ratio of AgO to Ag2O is 1:1.2-3, preferably 1:1.3-2.7, and more preferably 1:1.6-2.5.

[0038] According to the Ag-based deoxidation catalyst of the present invention, in other embodiments, the active component is a combination of Ag and Ag2O, and the molar ratio of Ag to Ag2O is 1:1.8-3, preferably 1:2.1-2.5.

[0039] According to the Ag-based deoxygenation catalyst of the present invention, in other embodiments, the active component is a combination of Ag, AgO and Ag2O, and the molar ratio of Ag, AgO and Ag2O is 1:(1.1-1.5):(0.5-0.8), preferably 1:(1.2-1.4):(0.6-0.7).

[0040] In the Ag-based deoxidation catalyst of the present invention, the catalyst carrier can be a conventional carrier in the art. In a preferred embodiment, the catalyst carrier is at least one of SiO2, Al2O3 and molecular sieve. In the present invention, the molecular sieve can specifically be at least one of a pure silicon molecular sieve carrier, an H-ZSM-5 molecular sieve carrier, an MCM-22 molecular sieve carrier and a Y-type molecular sieve carrier.

[0041] In the Ag-based deoxidation catalyst of the present invention, the auxiliary agent may be a water-soluble sodium salt, magnesium salt, zirconium salt, potassium salt and copper salt. In a preferred embodiment, the auxiliary agent is at least one of NaNO3, Mg(NO3)2, Zr(NO3)4, KNO3 and Cu(NO3)2.

[0042] According to some embodiments of the present invention, the Ag-based deoxygenation catalyst includes a catalyst carrier and an active component and an auxiliary agent attached to the catalyst carrier, wherein the active component is at least two of Ag, AgO and Ag2O; relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal elements can be 1-10 parts by weight, and the content of the auxiliary agent in terms of metal elements can be 0.5-3 parts by weight; the catalyst carrier is at least one of SiO2, Al2O3 and molecular sieve, and the auxiliary agent is at least one of NaNO3, Mg(NO3)2, Zr(NO3)4, KNO3 and Cu(NO3)2.

[0043] According to some other embodiments of the present invention, the Ag-based deoxygenation catalyst includes a catalyst carrier and an active component and an auxiliary agent attached to the catalyst carrier, wherein the active component is at least two of Ag, AgO and Ag2O; relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal elements can be 3-5 parts by weight, and the content of the auxiliary agent in terms of metal elements can be 1-2 parts by weight; the catalyst carrier is at least one of SiO2, Al2O3 and molecular sieve, and the auxiliary agent is at least one of NaNO3, Mg(NO3)2, Zr(NO3)4, KNO3 and Cu(NO3)2.

[0044] According to some other embodiments of the present invention, the Ag-based deoxygenation catalyst includes a catalyst carrier and an active component and an auxiliary agent attached to the catalyst carrier, wherein the active component is a combination of Ag and AgO, and the molar ratio of Ag to AgO is 1:1.5-2.5; relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal elements can be 3-5 parts by weight, and the content of the auxiliary agent in terms of metal elements can be 1-2 parts by weight; the catalyst carrier is at least one of SiO2, Al2O3 and molecular sieve, and the auxiliary agent is at least one of NaNO3, Mg(NO3)2, Zr(NO3)4, KNO3 and Cu(NO3)2.

[0045] According to some other embodiments of the present invention, the Ag-based deoxidation catalyst includes a catalyst carrier and an active component and an auxiliary agent attached to the catalyst carrier, wherein the active component is a combination of AgO and Ag2O, and the molar ratio of AgO to Ag2O is 1:1.2-3; relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal elements can be 3-5 parts by weight, and the content of the auxiliary agent in terms of metal elements can be 1-2 parts by weight; the catalyst carrier is at least one of SiO2, Al2O3 and molecular sieve, and the auxiliary agent is at least one of NaNO3, Mg(NO3)2, Zr(NO3)4, KNO3 and Cu(NO3)2.

[0046] According to some other embodiments of the present invention, the Ag-based deoxygenation catalyst includes a catalyst carrier and an active component and an auxiliary agent attached to the catalyst carrier, wherein the active component is a combination of Ag and Ag2O, and the molar ratio of Ag to Ag2O is 1:1.8-3; relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal elements can be 3-5 parts by weight, and the content of the auxiliary agent in terms of metal elements can be 1-2 parts by weight; the catalyst carrier is at least one of SiO2, Al2O3 and molecular sieve, and the auxiliary agent is at least one of NaNO3, Mg(NO3)2, Zr(NO3)4, KNO3 and Cu(NO3)2.

[0047] According to some other embodiments of the present invention, the Ag-based deoxygenation catalyst includes a catalyst carrier and an active component and an auxiliary agent attached to the catalyst carrier, wherein the active component is a combination of Ag, AgO and Ag2O, and the molar ratio of Ag, AgO and Ag2O is 1:(1.1-1.5):(0.5-0.8); relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal elements can be 3-5 parts by weight, and the content of the auxiliary agent in terms of metal elements can be 1-2 parts by weight; the catalyst carrier is at least one of SiO2, Al2O3 and molecular sieve, and the auxiliary agent is at least one of NaNO3, Mg(NO3)2, Zr(NO3)4, KNO3 and Cu(NO3)2.

[0048] According to some other embodiments of the present invention, the Ag-based deoxygenation catalyst includes a catalyst carrier and an active component and an auxiliary agent attached to the catalyst carrier, wherein the active component is a combination of Ag and AgO, and the molar ratio of Ag to AgO is 1:1.5-2.5; relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal elements can be 3-5 parts by weight, and the content of the auxiliary agent in terms of metal elements can be 1-2 parts by weight; the catalyst carrier is a SiO2 carrier, and the auxiliary agent is NaNO3.

[0049] According to some other embodiments of the present invention, the Ag-based deoxidation catalyst includes a catalyst carrier and an active component and an auxiliary agent attached to the catalyst carrier, wherein the active component is a combination of AgO and Ag2O, and the molar ratio of AgO to Ag2O is 1:1.2-3; relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal elements can be 3-5 parts by weight, and the content of the auxiliary agent in terms of metal elements can be 1-2 parts by weight; the catalyst carrier is an Al2O3 carrier, and the auxiliary agent is Mg(NO3)2.

[0050] According to some other embodiments of the present invention, the Ag-based deoxygenation catalyst includes a catalyst carrier and an active component and an auxiliary agent attached to the catalyst carrier, wherein the active component is a combination of Ag and Ag2O, and the molar ratio of Ag to Ag2O is 1:1.8-3; relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal elements can be 3-5 parts by weight, and the content of the auxiliary agent in terms of metal elements can be 1-2 parts by weight; the catalyst carrier is a molecular sieve carrier, and the auxiliary agent is Zr(NO3)4.

[0051] According to some other embodiments of the present invention, the Ag-based deoxygenation catalyst includes a catalyst carrier and an active component and an auxiliary agent attached to the catalyst carrier, wherein the active component is a combination of AgO and Ag2O, and the molar ratio of AgO to Ag2O is 1:1.2-3; relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal elements can be 3-5 parts by weight, and the content of the auxiliary agent in terms of metal elements can be 1-2 parts by weight; the catalyst carrier is a molecular sieve carrier, and the auxiliary agent is KNO3.

[0052] According to some other embodiments of the present invention, the Ag-based deoxygenation catalyst includes a catalyst carrier and an active component and an auxiliary agent attached to the catalyst carrier, wherein the active component is a combination of AgO and Ag2O, and the molar ratio of AgO to Ag2O is 1:1.2-3; relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal elements can be 3-5 parts by weight, and the content of the auxiliary agent in terms of metal elements can be 1-2 parts by weight; the catalyst carrier is a molecular sieve carrier, and the auxiliary agent is Cu(NO3)2.

[0053] According to some other embodiments of the present invention, the Ag-based deoxygenation catalyst includes a catalyst carrier and an active component and an auxiliary agent attached to the catalyst carrier, wherein the active component is a combination of Ag, AgO and Ag2O, and the molar ratio of Ag, AgO and Ag2O is 1:(1.1-1.5):(0.5-0.8); relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal elements can be 3-5 parts by weight, and the content of the auxiliary agent in terms of metal elements can be 1-2 parts by weight; the catalyst carrier is a molecular sieve carrier, and the auxiliary agent is KNO3.

[0054] The preparation method of the Ag-based deoxidation catalyst may include: attaching an Ag component precursor and an auxiliary agent to a catalyst carrier, and then performing calcination and reduction.

[0055] In the method of the present invention, the process of attaching the Ag component precursor and the auxiliary agent to the catalyst carrier can be implemented by impregnation, which can be equal volume impregnation, excess impregnation or step-by-step impregnation.

[0056] In a specific embodiment, the process of attaching the Ag component precursor and the auxiliary agent to the catalyst carrier is: immersing the catalyst carrier in a solution containing the Ag component precursor and the auxiliary agent by equal volume impregnation or excess impregnation, and then drying.

[0057] In another specific embodiment, the process of attaching the Ag component precursor and the auxiliary agent to the catalyst carrier is: using a step-by-step impregnation method, first immersing the catalyst carrier in a solution containing the auxiliary agent, then immersing it in a solution containing the Ag component precursor after drying, and then drying.

[0058] In the present invention, the Ag component precursor is preferably AgNO3.

[0059] In the present invention, the auxiliary agent is preferably at least one of NaNO3, Mg(NO3)2, Zr(NO3)4, KNO3 and Cu(NO3)2.

[0060] In the present invention, the catalyst carrier is preferably at least one of SiO2, Al2O3 and molecular sieve.

[0061] In the method of the present invention, the calcination and reduction processes enable the prepared Ag-based deoxidation catalyst to contain at least two of Ag, AgO and Ag2O as active components.

[0062] Specifically, the calcination conditions include: temperature of 300-500° C. and time of 3-8 hours.

[0063] Specifically, the reducing atmosphere is H2, a combination of H2 and CO, or a mixed atmosphere of different hydrogen concentrations. In a specific embodiment, the reducing atmosphere is a mixed atmosphere of different H2 concentrations, and the formation of surface oxygen vacancies of the catalyst is efficiently controlled by regulating the reducing atmosphere. Specifically, the reducing atmosphere can be, for example, 5% H2 (N2 dilution), 10% H2 (N2 dilution), 15% H2 (N2 dilution), etc.

[0064] Specifically, the reduction conditions include: catalyst heating rate of 2-15°C / min, reduction temperature of 100-500°C, and reduction time of 1-12h.

[0065] In the method described in the present invention, the amounts of the Ag component precursor, the auxiliary agent and the catalyst carrier are such that in the prepared Ag-based deoxidation catalyst, the content of the active component in terms of metal element is 1-10 parts by weight, preferably 3-5 parts by weight, relative to 100 parts by weight of the catalyst carrier; the content of the auxiliary agent in terms of metal element is 0.5-3 parts by weight, preferably 1-2 parts by weight.

[0066] According to some embodiments of the present invention, the preparation method of the Ag-based deoxidation catalyst includes: using an equal volume impregnation or an excess impregnation method to immerse the catalyst carrier in a solution containing an Ag component precursor and an additive, followed by drying, and then calcining and reducing, wherein the calcination conditions include: a temperature of 300-500°C and a time of 3-8h; the reducing atmosphere is H2, a combination of H2 and CO, or a mixed atmosphere of different hydrogen concentrations; the reduction conditions include: a catalyst heating rate of 2-15°C / min, a reduction temperature of 100-500°C, and a reduction time of 1-12h.

[0067] According to other embodiments of the present invention, the preparation method of the Ag-based deoxidation catalyst includes: using a step-by-step impregnation method, first immersing the catalyst carrier in a solution containing an additive, and then immersing it in a solution containing an Ag component precursor after drying, and then drying, and then calcining and reducing, wherein the calcination conditions include: a temperature of 300-500°C and a time of 3-8h; the reducing atmosphere is a combination of H2, H2 and CO, or a mixed atmosphere of different hydrogen concentrations; the reduction conditions include: a catalyst heating rate of 2-15°C / min, a reduction temperature of 100-500°C, and a reduction time of 1-12h.

[0068] According to other embodiments of the present invention, the preparation method of the Ag-based deoxidation catalyst includes: using an equal volume impregnation method to impregnate a SiO2 carrier into a solution containing AgNO3 and NaNO3, followed by drying, and then calcining and reducing, wherein the calcination conditions include: a temperature of 300-500°C and a time of 3-8h; the reducing atmosphere is H2 or 5-15% H2 (N2 diluted); the reduction conditions include: a catalyst heating rate of 2-15°C / min, a reduction temperature of 100-500°C, and a reduction time of 1-12h.

[0069] According to other embodiments of the present invention, the preparation method of the Ag-based deoxidation catalyst includes: using an equal volume impregnation method to impregnate an Al2O3 carrier into a solution containing AgNO3 and Mg(NO3)2, followed by drying, and then calcining and reducing, wherein the calcination conditions include: a temperature of 300-500°C and a time of 3-8h; the reducing atmosphere is H2 or 5-15% H2 (N2 diluted); the reduction conditions include: a catalyst heating rate of 2-15°C / min, a reduction temperature of 100-500°C, and a reduction time of 1-12h.

[0070] According to other embodiments of the present invention, the preparation method of the Ag-based deoxygenation catalyst includes: using an over-impregnation method to impregnate a molecular sieve carrier into a solution containing AgNO3 and Zr(NO3)4, followed by drying, and then calcining and reducing, wherein the calcination conditions include: a temperature of 300-500°C and a time of 3-8h; the reducing atmosphere is H2 or 5-15% H2 (N2 diluted); the reduction conditions include: a catalyst heating rate of 2-15°C / min, a reduction temperature of 100-500°C, and a reduction time of 1-12h.

[0071] According to other embodiments of the present invention, the preparation method of the Ag-based deoxygenation catalyst includes: using an equal volume impregnation method to impregnate the molecular sieve carrier into a solution containing AgNO3 and KNO3, followed by drying, and then calcining and reducing, wherein the calcination conditions include: a temperature of 300-500°C and a time of 3-8h; the reducing atmosphere is H2 or 5-15% H2 (N2 diluted); the reduction conditions include: a catalyst heating rate of 2-15°C / min, a reduction temperature of 100-500°C, and a reduction time of 1-12h.

[0072] According to other embodiments of the present invention, the preparation method of the Ag-based deoxygenation catalyst includes: using an over-impregnation method to impregnate a molecular sieve carrier in a solution containing AgNO3 and Cu(NO3)2, followed by drying, and then calcining and reducing, wherein the calcination conditions include: a temperature of 300-500°C and a time of 3-8h; the reducing atmosphere is H2 or 5-15% H2 (N2 diluted); the reduction conditions include: a catalyst heating rate of 2-15°C / min, a reduction temperature of 100-500°C, and a reduction time of 1-12h.

[0073] According to other embodiments of the present invention, the preparation method of the Ag-based deoxygenation catalyst includes: using a step-by-step impregnation method, first impregnating the molecular sieve carrier in a KNO3 solution, drying it and then impregnating it in an AgNO3 solution, drying it, and then calcining and reducing it, wherein the calcination conditions include: a temperature of 300-500°C and a time of 3-8h; the reducing atmosphere is H2 or 5-15% H2 (N2 diluted); the reduction conditions include: a catalyst heating rate of 2-15°C / min, a reduction temperature of 100-500°C, and a reduction time of 1-12h.

[0074] The present invention also provides the use of the Ag-based deoxygenation catalyst in the deoxygenation process of olefin gas containing oxygen.

[0075] In specific applications, the Ag-based deoxygenation catalyst of the present invention can achieve the removal of extremely low trace oxygen (1000 ppm), and can achieve deep removal of oxygen at a relatively low proportion of hydrogen (such as less than 1 volume %, especially less than 0.5 volume %).

[0076] The following examples further illustrate the Ag-based deoxidation catalyst and its preparation method and application of the present invention. The examples are implemented based on the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following examples.

[0077] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, are all commercially available.

[0078] Example 1

[0079] (1) dissolving AgNO3 and NaNO3 in deionized water to obtain a solution containing AgNO3 and NaNO3;

[0080] (2) using an equal volume impregnation method, the SiO2 carrier is impregnated in the solution containing AgNO3 and NaNO3, then dried in the shade at room temperature for 12 hours, then dried at 120°C for 8 hours, and then calcined at 500°C for 4 hours to obtain a calcined product, wherein the weight ratio of AgNO3 (calculated as metal element), NaNO3 (calculated as metal element) and SiO2 carrier is 5:1:100;

[0081] (3) The calcined product is placed in a fixed bed reactor for reduction, and the reduction conditions are: temperature of 200° C., reducing atmosphere of pure H2, time of 8 h, pressure of 0.1 MPa, and heating rate of 3° C. / min, to obtain an Ag-based deoxygenation catalyst; in situ XPS detection shows that the active components in the Ag-based deoxygenation catalyst are Ag and AgO, and the molar ratio is 2.6:5;

[0082] (4) After the reduction is completed, the bed temperature of the fixed bed reactor is lowered to room temperature, and the catalyst bed is purged with nitrogen for 30 minutes;

[0083] (5) The feed gas is introduced into a fixed bed reactor for gas phase deoxygenation reaction, wherein the feed gas is composed of 99.25% ethylene, 0.25% oxygen and 0.5% hydrogen. The conditions for the deoxygenation reaction are: reaction space velocity 3000h -1 , reaction pressure is 0.2MPa, and reaction temperature is 100℃.

[0084] The oxygen content of the deoxygenated gas was detected and the deoxygenation rate was calculated. The results are shown in Table 1 below.

[0085] Example 2

[0086] (1) dissolving AgNO3 and Mg(NO3)2 in deionized water to obtain a solution containing AgNO3 and Mg(NO3)2;

[0087] (2) using an equal volume impregnation method, the Al2O3 carrier is impregnated in the solution containing AgNO3 and Mg(NO3)2, and then dried in the shade at room temperature for 12 hours, and then dried at 120°C for 10 hours, and then calcined at 400°C for 4 hours to obtain a calcined product, wherein the weight ratio of AgNO3 (calculated as metal element), Mg(NO3)2 (calculated as metal element) and Al2O3 carrier is 3:2:100;

[0088] (3) The calcined product is placed in a fixed bed reactor for reduction, and the reduction conditions are: temperature of 150° C., reducing atmosphere of 5% H2 (N2 diluted), time of 10 h, pressure of 0.1 MPa, and heating rate of 2° C. / min, to obtain an Ag-based deoxygenation catalyst; in-situ XPS detection shows that the active components in the Ag-based deoxygenation catalyst are AgO and Ag2O, and the molar ratio is 2.3:3;

[0089] (4) After the reduction is completed, the bed temperature of the fixed bed reactor is lowered to room temperature, and the catalyst bed is purged with nitrogen for 30 minutes;

[0090] (5) The feed gas is introduced into a fixed bed reactor for gas phase deoxygenation reaction, wherein the feed gas is composed of 99.25% ethylene, 0.25% oxygen and 0.5% hydrogen. The conditions for the deoxygenation reaction are: reaction space velocity 3000h -1 , reaction pressure is 0.25MPa, and reaction temperature is 100℃.

[0091] The oxygen content of the deoxygenated gas was detected and the deoxygenation rate was calculated. The results are shown in Table 1 below.

[0092] Example 3

[0093] (1) dissolving AgNO3 and Zr(NO3)4 in deionized water to obtain a solution containing AgNO3 and Zr(NO3)4;

[0094] (2) The pure silicon molecular sieve carrier is impregnated in the solution containing AgNO3 and Zr(NO3)4 by an over-impregnation method, and then dried in the shade at room temperature for 12 hours, and then dried at 100°C for 12 hours, and then calcined at 450°C for 4 hours to obtain a calcined product, wherein the weight ratio of AgNO3 (calculated as metal element), Zr(NO3)4 (calculated as metal element) and the molecular sieve carrier is 5:1.5:100;

[0095] (3) The calcined product is placed in a fixed bed reactor for reduction, and the reduction conditions are: temperature of 300° C., reducing atmosphere of 15% H2 (N2 diluted), time of 10 h, pressure of 0.1 MPa, and heating rate of 2° C. / min, to obtain an Ag-based deoxygenation catalyst; in-situ XPS detection shows that the active components in the Ag-based deoxygenation catalyst are Ag and Ag2O, and the molar ratio is 3:7;

[0096] (4) After the reduction is completed, the bed temperature of the fixed bed reactor is lowered to room temperature, and the catalyst bed is purged with nitrogen for 30 minutes;

[0097] (5) The feed gas is introduced into a fixed bed reactor for gas phase deoxygenation reaction, wherein the feed gas is composed of 99.25% ethylene, 0.25% oxygen and 0.5% hydrogen. The conditions for the deoxygenation reaction are: reaction space velocity 3000h -1 , reaction pressure is 0.25MPa, and reaction temperature is 100℃.

[0098] The oxygen content of the deoxygenated gas was detected and the deoxygenation rate was calculated. The results are shown in Table 1 below.

[0099] Example 4

[0100] (1) dissolving AgNO3 and KNO3 in deionized water to obtain a solution containing AgNO3 and KNO3;

[0101] (2) The H-ZSM-5 molecular sieve carrier is impregnated in the solution containing AgNO3 and KNO3 by equal volume impregnation, and then dried in the shade at room temperature for 12 hours, and then dried at 120°C for 12 hours, and then calcined at 450°C for 4 hours to obtain a calcined product, wherein the weight ratio of AgNO3 (calculated as metal element), KNO3 (calculated as metal element) and molecular sieve carrier is 4:1.5:100;

[0102] (3) The calcined product is placed in a fixed bed reactor for reduction, and the reduction conditions are: temperature of 300° C., reducing atmosphere of 5% H2 (N2 diluted), time of 10 h, pressure of 0.1 MPa, heating rate of 2° C. / min, to obtain an Ag-based deoxygenation catalyst; in-situ XPS detection shows that the active components in the Ag-based deoxygenation catalyst are AgO and Ag2O, and the molar ratio is 3:8;

[0103] (4) After the reduction is completed, the bed temperature of the fixed bed reactor is lowered to room temperature, and the catalyst bed is purged with nitrogen for 30 minutes;

[0104] (5) The feed gas is introduced into a fixed bed reactor for gas phase deoxygenation reaction, wherein the feed gas is composed of 99.25% ethylene, 0.25% oxygen and 0.5% hydrogen. The conditions for the deoxygenation reaction are: reaction space velocity 3000h -1 , reaction pressure is 0.3MPa, and reaction temperature is 100℃.

[0105] The oxygen content of the deoxygenated gas was detected and the deoxygenation rate was calculated. The results are shown in Table 1 below.

[0106] Example 5

[0107] (1) dissolving AgNO3 and Cu(NO3)2 in deionized water to obtain a solution containing AgNO3 and Cu(NO3)2;

[0108] (2) The Y-type molecular sieve carrier is impregnated in the solution containing AgNO3 and Cu(NO3)2 by an over-impregnation method, and then dried in the shade at room temperature for 12 hours, and then dried at 120°C for 12 hours, and then calcined at 450°C for 4 hours to obtain a calcined product, wherein the weight ratio of AgNO3 (calculated as metal element), Cu(NO3)2 (calculated as metal element) and the molecular sieve carrier is 4:2:100;

[0109] (3) The calcined product is placed in a fixed bed reactor for reduction, and the reduction conditions are: temperature of 300° C., reducing atmosphere of 10% H2 (diluted with N2), time of 10 h, pressure of 0.1 MPa, and heating rate of 2° C. / min, to obtain an Ag-based deoxygenation catalyst; in-situ XPS detection shows that the active components in the Ag-based deoxygenation catalyst are AgO and Ag2O, and the molar ratio is 3.5:6;

[0110] (4) After the reduction is completed, the bed temperature of the fixed bed reactor is lowered to room temperature, and the catalyst bed is purged with nitrogen for 30 minutes;

[0111] (5) The feed gas is introduced into a fixed bed reactor for gas phase deoxygenation reaction, wherein the feed gas is composed of 99.25% ethylene, 0.25% oxygen and 0.5% hydrogen. The conditions for the deoxygenation reaction are: reaction space velocity 3000h -1 , reaction pressure is 0.3MPa, and reaction temperature is 100℃.

[0112] The oxygen content of the deoxygenated gas was detected and the deoxygenation rate was calculated. The results are shown in Table 1 below.

[0113] Example 6

[0114] (1) dissolving KNO3 in deionized water to obtain a KNO3 solution; immersing a Y-type molecular sieve carrier in the KNO3 solution, and then drying in the shade at room temperature for 12 hours, and then drying at 120°C for 12 hours;

[0115] (2) dissolving AgNO3 in deionized water to obtain an AgNO3 solution; immersing the dried product of step (1) in the AgNO3 solution in a step-by-step impregnation manner, then drying in the shade at room temperature for 12 h, then drying at 120°C for 12 h, and then calcining at 450°C for 4 h to obtain a calcined product, wherein the weight ratio of AgNO3 (in terms of metal element), KNO3 (in terms of metal element) and molecular sieve carrier is 4:2:100;

[0116] (3) The calcined product is placed in a fixed bed reactor for reduction, and the reduction conditions are: temperature of 300° C., reducing atmosphere of 10% H2 (N2 diluted), time of 10 h, pressure of 0.1 MPa, and heating rate of 2° C. / min, to obtain an Ag-based deoxygenation catalyst; in-situ XPS detection shows that the active components in the Ag-based deoxygenation catalyst are Ag, AgO and Ag2O, and the molar ratio is 3:4:2;

[0117] (4) After the reduction is completed, the bed temperature of the fixed bed reactor is lowered to room temperature, and the catalyst bed is purged with nitrogen for 30 minutes;

[0118] (5) The feed gas is introduced into a fixed bed reactor for gas phase deoxygenation reaction, wherein the feed gas is composed of 99.25% ethylene, 0.25% oxygen and 0.5% hydrogen. The conditions for the deoxygenation reaction are: reaction space velocity 3000h -1 , reaction pressure is 0.3MPa, and reaction temperature is 100℃.

[0119] The oxygen content of the deoxygenated gas was detected and the deoxygenation rate was calculated. The results are shown in Table 1 below.

[0120] Example 7

[0121] (1) dissolving AgNO3 and KNO3 in deionized water to obtain a solution containing AgNO3 and KNO3;

[0122] (2) The Y-type molecular sieve carrier is impregnated in the solution containing AgNO3 and KNO3 by equal volume impregnation, and then dried in the shade at room temperature for 12 hours, and then dried at 120°C for 12 hours, and then calcined at 450°C for 4 hours to obtain a calcined product, wherein the weight ratio of AgNO3 (calculated as metal element), KNO3 (calculated as metal element) and the molecular sieve carrier is 4:2:100;

[0123] (3) The calcined product is placed in a fixed bed reactor for reduction, and the reduction conditions are: temperature of 300° C., reducing atmosphere of 10% H2 (N2 diluted), time of 10 h, pressure of 0.1 MPa, and heating rate of 2° C. / min, to obtain an Ag-based deoxygenation catalyst; in-situ XPS detection shows that the active components in the Ag-based deoxygenation catalyst are Ag, AgO and Ag2O, and the molar ratio is 1:1.2:0.6;

[0124] (4) After the reduction is completed, the bed temperature of the fixed bed reactor is lowered to room temperature, and the catalyst bed is purged with nitrogen for 30 minutes;

[0125] (5) The feed gas is introduced into a fixed bed reactor for gas phase deoxygenation reaction, wherein the feed gas is composed of 99.25% ethylene, 0.25% oxygen and 0.5% hydrogen. The conditions for the deoxygenation reaction are: reaction space velocity 3000h -1 , reaction pressure is 0.3MPa, and reaction temperature is 100℃.

[0126] The oxygen content of the deoxygenated gas was detected and the deoxygenation rate was calculated. The results are shown in Table 1 below.

[0127] Example 8

[0128] (1) dissolving AgNO3 and KNO3 in deionized water to obtain a solution containing AgNO3 and KNO3;

[0129] (2) The SiO2 carrier is impregnated in the solution containing AgNO3 and KNO3 by equal volume impregnation, and then dried in the shade at room temperature for 12 hours, and then dried at 120°C for 12 hours, and then calcined at 450°C for 4 hours to obtain a calcined product, wherein the weight ratio of AgNO3 (calculated as metal element), KNO3 (calculated as metal element) and SiO2 carrier is 4:1.5:100;

[0130] (3) The calcined product is placed in a fixed bed reactor for reduction, and the reduction conditions are: temperature of 300° C., reducing atmosphere of 5% H2 (N2 diluted), time of 10 h, pressure of 0.1 MPa, heating rate of 2° C. / min, to obtain an Ag-based deoxygenation catalyst; in-situ XPS detection shows that the active components in the Ag-based deoxygenation catalyst are AgO and Ag2O, and the molar ratio is 1:1.7;

[0131] (4) After the reduction is completed, the bed temperature of the fixed bed reactor is lowered to room temperature, and the catalyst bed is purged with nitrogen for 30 minutes;

[0132] (5) The feed gas is introduced into a fixed bed reactor for gas phase deoxygenation reaction, wherein the feed gas is composed of 99.25% ethylene, 0.25% oxygen and 0.5% hydrogen. The conditions for the deoxygenation reaction are: reaction space velocity 3000h -1 , reaction pressure is 0.3MPa, and reaction temperature is 100℃.

[0133] The oxygen content of the deoxygenated gas was detected and the deoxygenation rate was calculated. The results are shown in Table 1 below.

[0134] Example 9

[0135] (1) dissolving AgNO3 and Zr(NO3)4 in deionized water to obtain a solution containing AgNO3 and Zr(NO3)4;

[0136] (2) The Al2O3 carrier is impregnated in the solution containing AgNO3 and Zr(NO3)4 by an over-impregnation method, and then dried in the shade at room temperature for 12 hours, and then dried at 100°C for 12 hours, and then calcined at 450°C for 4 hours to obtain a calcined product, wherein the weight ratio of AgNO3 (calculated as metal element), Zr(NO3)4 (calculated as metal element) and Al2O3 carrier is 5:1.5:100;

[0137] (3) The calcined product is placed in a fixed bed reactor for reduction, and the reduction conditions are: temperature of 300° C., reducing atmosphere of 15% H2 (N2 diluted), time of 10 h, pressure of 0.1 MPa, heating rate of 2° C. / min, to obtain an Ag-based deoxygenation catalyst; in-situ XPS detection shows that the active components in the Ag-based deoxygenation catalyst are Ag and Ag2O, and the molar ratio is 1:2.1;

[0138] (4) After the reduction is completed, the bed temperature of the fixed bed reactor is lowered to room temperature, and the catalyst bed is purged with nitrogen for 30 minutes;

[0139] (5) The feed gas is introduced into a fixed bed reactor for gas phase deoxygenation reaction, wherein the feed gas is composed of 99.25% ethylene, 0.25% oxygen and 0.5% hydrogen. The conditions for the deoxygenation reaction are: reaction space velocity 3000h -1 , reaction pressure is 0.25MPa, and reaction temperature is 100℃.

[0140] The oxygen content of the deoxygenated gas was detected and the deoxygenation rate was calculated. The results are shown in Table 1 below.

[0141] Example 10

[0142] 1) dissolving AgNO3 and NaNO3 in deionized water to obtain a solution containing AgNO3 and NaNO3;

[0143] (2) using an equal volume impregnation method, the SiO2 carrier is impregnated in the solution containing AgNO3 and NaNO3, then dried in the shade at room temperature for 12 hours, then dried at 120°C for 8 hours, and then calcined at 500°C for 4 hours to obtain a calcined product, wherein the weight ratio of AgNO3 (calculated as metal element), NaNO3 (calculated as metal element) and SiO2 carrier is 5:1:100;

[0144] (3) The calcined product is placed in a fixed bed reactor for reduction, and the reduction conditions are: temperature of 250° C., reducing atmosphere of 15% H2 (N2 diluted), time of 8 h, pressure of 0.1 MPa, heating rate of 3° C. / min, to obtain an Ag-based deoxygenation catalyst; in-situ XPS detection shows that the active components in the Ag-based deoxygenation catalyst are Ag and AgO, and the molar ratio is 1:2.15;

[0145] (4) After the reduction is completed, the bed temperature of the fixed bed reactor is lowered to room temperature, and the catalyst bed is purged with nitrogen for 30 minutes;

[0146] (5) The feed gas is introduced into a fixed bed reactor for gas phase deoxygenation reaction, wherein the feed gas is composed of 99.25% ethylene, 0.25% oxygen and 0.5% hydrogen. The conditions for the deoxygenation reaction are: reaction space velocity 3000h -1 , reaction pressure is 0.2MPa, and reaction temperature is 100℃.

[0147] The oxygen content of the deoxygenated gas was detected and the deoxygenation rate was calculated. The results are shown in Table 1 below.

[0148] Comparative Example 1

[0149] (1) dissolving AgNO3 in deionized water to obtain an AgNO3 solution;

[0150] (2) The H-ZSM-5 molecular sieve carrier was impregnated in the AgNO3 solution by equal volume impregnation, and then dried in the shade at room temperature for 12 hours, and then dried at 120°C for 12 hours, and then calcined at 450°C for 4 hours to obtain a calcined product, wherein the weight ratio of AgNO3 (in terms of metal element) to the molecular sieve carrier was 4:100;

[0151] (3) The calcined product is placed in a fixed bed reactor for reduction under the following conditions: temperature of 300° C., reducing atmosphere of 5% H2 (diluted with N2), time of 10 h, pressure of 0.1 MPa, and heating rate of 2° C. / min, to obtain an Ag-based deoxygenation catalyst; in-situ XPS detection shows that the active component in the Ag-based deoxygenation catalyst is Ag2O;

[0152] (4) After the reduction is completed, the bed temperature of the fixed bed reactor is lowered to room temperature, and the catalyst bed is purged with nitrogen for 30 minutes;

[0153] (5) The feed gas is introduced into a fixed bed reactor for gas phase deoxygenation reaction, wherein the feed gas is composed of 99.25% ethylene, 0.25% oxygen and 0.5% hydrogen. The conditions for the deoxygenation reaction are: reaction space velocity 3000h -1 , reaction pressure is 0.3MPa, and reaction temperature is 100℃.

[0154] The oxygen content of the deoxygenated gas was detected and the deoxygenation rate was calculated. The results are shown in Table 1 below.

[0155] Table 1

[0156] serial number Oxygen content of raw gas / volume % Oxygen content after deoxidation / volume % Deoxidation rate / % Example 1 0.25 0.002 99.2 Example 2 0.25 0.001 99.6 Example 3 0.25 0.0005 99.8 Example 4 0.25 0.002 99.2 Example 5 0.25 0.001 99.6 Example 6 0.25 0.002 99.2 Example 7 0.25 0.003 98.8 Example 8 0.25 0.0025 99.0 Example 9 0.25 0.0032 98.7 Example 10 0.25 0.0036 98.6 Comparative Example 1 0.25 0.095 62.0

[0157] It can be seen from the results in Table 1 that in the gas phase deoxygenation reaction, the use of the Ag-based deoxygenation catalyst of the present invention can obtain a higher deoxygenation rate and a better deoxygenation effect.

[0158] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. An Ag-based deoxidation catalyst, characterized in that: It comprises a catalyst carrier and active components and additives attached to the catalyst carrier, wherein the active components are at least two of Ag, AgO and Ag2O.

2. The Ag-based deoxidation catalyst according to claim 1, characterized in that Relative to 100 parts by weight of the catalyst carrier, the content of the active component in terms of metal element is 1-10 parts by weight, preferably 3-5 parts by weight; the content of the auxiliary agent in terms of metal element is 0.5-3 parts by weight, preferably 1-2 parts by weight.

3. The Ag-based deoxidation catalyst according to claim 1 or 2, characterized in that: The active component is a combination of Ag and AgO, and the molar ratio of Ag to AgO is 1:1.5-2.5; or The active component is a combination of AgO and Ag2O, and the molar ratio of AgO to Ag2O is 1:1.2-3; or The active component is a combination of Ag and Ag2O, and the molar ratio of Ag to Ag2O is 1:1.8-3; or The active component is a combination of Ag, AgO and Ag2O, and the molar ratio of Ag, AgO and Ag2O is 1:(1.1-1.5):(0.5-0.8).

4. The Ag-based deoxidation catalyst according to any one of claims 1 to 3, characterized in that: The catalyst carrier is at least one of SiO2, Al2O3 and molecular sieve.

5. The Ag-based deoxidation catalyst according to any one of claims 1 to 3, characterized in that: The auxiliary agent is at least one of NaNO3, Mg(NO3)2, Zr(NO3)4, KNO3 and Cu(NO3)2.

6. A method for preparing the Ag-based deoxidation catalyst according to any one of claims 1 to 5, characterized in that: The method comprises: making a Ag component precursor and an auxiliary agent adhere to a catalyst carrier, and then performing calcination and reduction.

7. The method according to claim 6, characterized in that The process of attaching the Ag component precursor and the additive to the catalyst carrier is carried out by impregnation; Preferably, the impregnation is carried out by equal volume impregnation, excess impregnation or stepwise impregnation.

8. The method according to claim 6 or 7, characterized in that: The Ag component precursor is AgNO3.

9. The method according to claim 6, characterized in that The calcination conditions include: temperature of 300-500° C. and time of 3-8 hours.

10. The method according to claim 6, characterized in that The reducing atmosphere is H2, a combination of H2 and CO, or a mixed atmosphere with different hydrogen concentrations.

11. The method according to claim 6, characterized in that The reduction conditions include: catalyst heating rate of 2-15°C / min, reduction temperature of 100-500°C, and reduction time of 1-12h.

12. Use of the Ag-based deoxygenation catalyst according to any one of claims 1 to 5 in a deoxygenation process of an olefin gas containing oxygen.

Citation Information

Patent Citations

  • Deoxidation catalyst, preparation method thereof and method for removing oxygen in light olefin

    CN115707514A

  • Denitrification catalyst and denitrifying method using the same

    JP1996131829A

  • Silver and silver oxide catalysts for the oxidation of carbon monoxide in cigarette smoke

    US20050279372A1

  • Aldehyde decomposition catalyst

    WO2020110874A1