Preparation method and application of mesoporous Ni-coated SiO2 methane dry reforming catalyst
By using inverse microemulsion and post-treatment methods in methane dry reforming catalysts to prepare mesoporous Ni@SiO2 catalysts, the problems of poor activity and stability of catalysts at high space velocities in the existing technology have been solved, and efficient and stable methane production has been achieved. and carbon dioxide conversion.
Patent Information
- Application Number
- CN202410871973.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-15
AI Technical Summary
Existing methane dry reforming nickel-based catalysts have poor activity under high space velocity conditions, low single-pass conversion rates of methane and carbon dioxide, the catalyst is prone to sintering, carbon deposition, poor stability, and short service life.
The mesoporous Ni@SiO2 catalyst is prepared using reverse microemulsion and post-treatment methods. Ni nanoparticles are encapsulated inside the mesoporous SiO2. By adjusting the raw material ratio and conditions during the synthesis process, the specific surface area of the catalyst and the dispersion of active centers are increased. , enhance anti-agglomeration and anti-carbon deposition properties.
The performance of the methane dry reforming reaction is significantly improved. The single-pass conversion rate of methane and CO2 conversion rate of the catalyst can reach more than 90% and 95% at high space velocity. There was no significant decline in the 50-hour performance test, and the stability and The reactivity is significantly improved.
Smart Images

Figure CN118767918A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of energy utilization and environmental technology, relates to a preparation method and application of a catalyst, and specifically relates to a preparation method and application of a mesoporous Ni@SiO2 methane dry reforming catalyst. Background Art
[0002] Methane and carbon dioxide are greenhouse gases with the largest emission. Through methane dry reforming technology, methane and carbon dioxide are converted into synthesis gas or hydrogen, which is of great significance to the environment and energy. However, the molecular structures of methane and carbon dioxide are very stable and difficult to activate, and catalytic conversion is required under high temperature conditions. Publication No. CN106268822A discloses a M-SiO2 (M=Ni or NiCo) catalyst and its preparation method and application in methane carbon dioxide reforming reaction, using a microemulsion method and a catalyst prepared by hydrogen reduction treatment, but the space velocity applicable to the catalyst is only 600-18000 ml per gram per hour, and the conversion rate of methane and carbon dioxide is relatively low. At present, methane dry reforming nickel-based catalysts have poor activity under high space velocity conditions, low per-pass conversion of methane and carbon dioxide, easy sintering of the catalyst, easy carbon deposition, poor stability, short service life and other problems. Therefore, developing Ni-based methane dry reforming catalysts with high specific surface area, high dispersion of active centers, resistance to sintering and resistance to carbon deposition, and achieving efficient and stable conversion of methane and carbon dioxide at high space velocity has become a difficulty that must be solved in current research. Summary of the invention
[0003] In order to overcome the technical problems of poor activity, low methane and carbon dioxide single-pass conversion rate and short life of existing methane dry reforming Ni-based catalysts under high space velocity conditions, the present invention proposes a mesoporous Ni@SiO2 methane dry reforming catalyst and its preparation method and application. The synthesis of a mesoporous Ni@SiO2 methane dry reforming catalyst material is achieved by using a reverse microemulsion and post-treatment method, and the material is used as a new nanocatalyst for methane dry reforming reactions. Compared with traditional catalysts, the catalyst has a high specific surface area, highly dispersed active centers, excellent reaction activity under high space velocity, and anti-agglomeration and anti-carbon deposition characteristics.
[0004] To achieve the above object, the technical solution of the present invention is implemented as follows:
[0005] A mesoporous Ni@SiO2 methane dry reforming catalyst, wherein the mesoporous Ni@SiO2 catalyst is Ni nanoparticles encapsulated inside the mesoporous SiO2, and the specific surface area of the catalyst is 70-900m 2 / g, the mass percentage of Ni is 1-6%, the Ni particle size is 4-8nm, and the pore size of mesoporous SiO2 is 2-5nm.
[0006] A method for preparing a mesoporous Ni@SiO2 methane dry reforming catalyst, comprising the following steps:
[0007] (1) mixing a Ni source aqueous solution, an alkane solvent, a nonionic surfactant and a reducing agent, and then adding ammonia water and tetraethyl orthosilicate to obtain a mixed solution;
[0008] (2) stirring the mixed solution obtained in step (1) to react, centrifuging, washing, drying and calcining to obtain a solid powder;
[0009] (3) dispersing the solid powder obtained in step (2) in water, adding a cationic surfactant and an alkaline inorganic salt to obtain an aqueous solution, stirring the reaction, and obtaining a mesoporous Ni@SiO2 methane dry reforming catalyst after centrifugation, washing, drying, calcining and hydrogen reduction.
[0010] In the step (1), the Ni source in the Ni source aqueous solution is NiNO3 or NiCl2; the alkane solvent is n-hexane, n-octane or cyclohexane; the non-ionic surfactant is any one of Lutensol AO5, Brij L4 and Brij O10; and the reducing agent is any one of NaBH4, LiBH4, KBH4 and LiAlH4.
[0011] In the step (1), the concentration of the Ni source aqueous solution is 0.1-2 mol / L; the volume ratio of the alkane solvent to the Ni source aqueous solution is (10-52):1; the concentration of the non-ionic surfactant in the mixed solution is 0.1-0.5 mol / L; the molar ratio of the reducing agent to the Ni source is (3-7):1; and the molar ratio of tetraethyl orthosilicate to the Ni source is (20-100):1.
[0012] The calcination temperature in step (2) is 500-900° C. and the calcination time is 3-12 hours.
[0013] In step (3), the cationic surfactant is C 12 TAB, C 14 TAB, C 16 TAB and C 18 Any one of TAB; Any one of the basic inorganic salts Na2CO3, K2CO3, CH3COONa and CH3COOK.
[0014] In the step (3), (3.0-13.0) g of solid powder is added to each liter of water; the concentration of the cationic surfactant in the aqueous solution is 1-5 mmol / L, and the concentration of the alkaline inorganic salt in the aqueous solution is 0.1-0.3 mol / L; the reaction temperature in the step (3) is 35-90° C. and the reaction time is 4-8 hours.
[0015] In the step (3), the calcination temperature is 400-800°C and the time is 3-12 hours; the hydrogen reduction temperature is 700-800°C and the time is 2-5 hours.
[0016] The above-mentioned mesoporous Ni@SiO2 methane dry reforming catalyst is used in the methane carbon dioxide reforming reaction.
[0017] The above-mentioned mesoporous Ni@SiO2 methane dry reforming catalyst is used in the methane carbon dioxide reforming reaction at a reaction temperature of 700-800°C and a space velocity of 18000-54000 ml / (g cat ·h), CH4 and CO2 molar ratio is 0.8-1.2. When the temperature is 750℃, the space velocity is 54000ml / (gcat·h) and CH4 / CO2=1.0, the CH4 conversion rate is greater than 80%, and the CO2 conversion rate is ≥90%.
[0018] The beneficial effects produced by the present invention are:
[0019] 1. The present invention adopts the method of reverse microemulsion and post-treatment to realize the synthesis of a mesoporous Ni@SiO2 methane dry reforming catalyst material, and uses the material as a new nanocatalyst for the reaction of methane dry reforming. Compared with traditional catalysts, the catalyst has a high specific surface area, highly dispersed active centers, excellent reaction activity at high space velocity, and anti-agglomeration and anti-carbon deposition characteristics. The catalyst Ni nanoparticles of the present invention are encapsulated inside the mesoporous SiO2, and the specific surface area of the catalyst can be as high as 900m 2 / g, the particle size, dispersion, specific surface area and pore structure of the catalyst active center can be controlled by adjusting the raw material ratio and synthesis conditions during the synthesis process, which is beneficial to improving the methane dry reforming reaction activity and catalyst stability.
[0020] 2. The catalyst of the present invention can significantly improve the performance of methane dry reforming reaction. At a temperature of 750°C, a space velocity of 54000ml / (gcat·h) and a CH4 / CO2 of 1.054000ml / (gcat·h), the catalyst can significantly improve the performance of methane dry reforming reaction. cat ·h), the methane single-pass conversion rate can reach more than 90%, and the CO2 conversion rate can reach more than 95%. The catalyst did not show obvious performance degradation in the 50-hour performance test. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 The electron microscope photographs of the mesoporous Ni@SiO2 methane dry reforming catalyst in Example 1 of the present invention at different magnifications.
[0023] Figure 2 The electron microscope photographs of the mesoporous Ni@SiO2 methane dry reforming catalyst of Example 2 of the present invention at different magnifications.
[0024] Figure 3 The electron microscope photographs of the mesoporous Ni@SiO2 methane dry reforming catalyst of Example 3 of the present invention at different magnifications.
[0025] Figure 4 This is the N2 adsorption-desorption curve of the mesoporous Ni@SiO2 methane dry reforming catalyst in Example 2 of the present invention.
[0026] Figure 5 This is a pore size distribution diagram of the mesoporous Ni@SiO2 methane dry reforming catalyst in Example 2 of the present invention.
[0027] Figure 6 These are the stability test data of the mesoporous Ni@SiO2 methane dry reforming catalyst in Example 2 of the present invention. DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] The preparation method of the mesoporous Ni@SiO2 methane dry reforming catalyst of this embodiment comprises the following steps:
[0031] 150 mL of cyclohexane and 50 mmol of Lutensol AO5 were weighed into a 250 mL round-bottom flask, and then 3 mL of a 0.5 mol / L nickel chloride solution was added, stirred until transparent, and 6 mmol of NaBH4 was added, and stirred for 6 hours; 3 mL of ammonia water and 100 mmol of tetraethyl orthosilicate were added, and stirred for 4 hours; the solid was collected by centrifugation, ultrasonically dispersed in acetone and ethanol solutions, and centrifuged and washed 3 times to separate the solid product; the solid product was dried at 80 ° C for 8 hours, and then calcined at 600 ° C in a muffle furnace for 5 hours to obtain a solid powder; 1 g of the above solid powder was taken, ultrasonically dispersed in 180 mL of deionized water, and then 0.2 g of C 16TAB, stirred for 1 hour; then added 3.5g of anhydrous Na2CO3, reacted at 35°C for 6 hours under stirring; collected the solid, ultrasonically dispersed it in water and ethanol solution, centrifuged and washed 3 times to separate the solid product; dried the solid product at 80°C for 8 hours, then calcined it at 600°C in a muffle furnace for 5 hours to obtain a solid powder, and reduced the solid powder with 10% H2 / N2 mixed gas at 700°C for 5 hours to obtain catalyst 1#.
[0032] Example 2
[0033] The preparation method of the mesoporous Ni@SiO2 methane dry reforming catalyst of this embodiment comprises the following steps:
[0034] 80 mL of cyclohexane and 15 mmol of Brij L4 were placed in a 150 mL round-bottom flask, followed by the addition of 2 mL of a 0.25 mol / L nickel chloride solution, stirring until transparent, adding 2.5 mmol of NaBH4, stirring for 6 hours; adding 1.0 mL of ammonia water and 30 mmol of ethyl orthosilicate, stirring for 4 hours; collecting the solid by centrifugation, ultrasonically dispersing it in acetone and ethanol solutions, centrifugally washing it 3 times, and separating the solid product; drying the solid product at 80 ° C for 8 hours, and then calcining it at 550 ° C in a muffle furnace for 5 hours to obtain a solid powder; taking 0.8 g of the above solid powder, ultrasonically dispersing it in 150 mL of deionized water, and then adding 0.18 g of C 16 TAB, stirred for 1 hour; then added 3.0g of anhydrous Na2CO3, reacted at 70°C for 6 hours under stirring; collected the solid, ultrasonically dispersed it in water and ethanol solution, centrifuged and washed 3 times to separate the solid product; dried the solid product at 80°C for 8 hours, then calcined it at 550°C in a muffle furnace for 5 hours to obtain a solid powder, and reduced the solid powder with 10% H2 / N2 mixed gas at 700°C for 5 hours to obtain catalyst 2#.
[0035] Example 3
[0036] The preparation method of the mesoporous Ni@SiO2 methane dry reforming catalyst of this embodiment comprises the following steps:
[0037] 130 mL of cyclohexane and 30 mmol of Brij L4 were placed in a 150 mL round-bottom flask, followed by the addition of 2.5 mL of a 0.3 mol / L nickel chloride solution, stirring until transparent, adding 5 mmol of NaBH4, stirring for 6 hours; adding 1.5 mL of ammonia water and 50 mmol of ethyl orthosilicate, stirring for 4 hours; collecting the solid by centrifugation, ultrasonically dispersing it in acetone and ethanol solutions, centrifugally washing it 3 times, and separating the solid product; drying the solid product at 80 ° C for 8 hours, and then calcining it at 600 ° C in a muffle furnace for 5 hours to obtain a solid powder; taking 0.8 g of the above solid powder, ultrasonically dispersing it in 150 mL of deionized water, and then adding 0.18 g of C 18 TAB, stirred for 1 hour; then added 3.0g of anhydrous Na2CO3, reacted at 90°C for 6 hours under stirring; collected the solid, ultrasonically dispersed it in water and ethanol solution, centrifuged and washed 3 times to separate the solid product; dried the solid product at 80°C for 8 hours, then calcined it at 600°C in a muffle furnace for 5 hours to obtain a solid powder, and reduced the solid powder with 10% H2 / N2 mixed gas at 700°C for 5 hours to obtain catalyst 3#.
[0038] Depend on Figure 1 , Figure 2 and Figure 3 As shown in Table 1, the Ni@SiO2 catalysts prepared in Examples 1-3 can encapsulate Ni nanoparticles inside SiO2, the Ni mass percentage is between 4-6%, the Ni particle size is between 6-8nm, and the Ni dispersion can reach 19%.
[0039] Table 1. Ni mass percentage, Ni particle size and dispersion data of the prepared mesoporous Ni@SiO2 methane dry reforming catalyst.
[0040] catalyst Ni mass percentage Ni particle size Ni dispersion Example 1 4.1% 6.3nm 11% Example 2 5.3% 7.4nm 16% Example 3 5.8% 6.5nm 19%
[0041] Example 4
[0042] The preparation method of the mesoporous Ni@SiO2 methane dry reforming catalyst of this embodiment comprises the following steps:
[0043] 130 mL of cyclohexane and 14.3 mmol of Brij L4 were placed in a 150 mL round-bottom flask, followed by the addition of 13 mL of a 0.1 mol / L nickel chloride solution, stirring until transparent, adding 3.6 mmol of NaBH4, stirring for 6 hours; adding 1.5 mL of ammonia water and 26 mmol of ethyl orthosilicate, stirring for 4 hours; collecting the solid by centrifugation, ultrasonically dispersing it in acetone and ethanol solutions, centrifugally washing it 3 times, and separating the solid product; drying the solid product at 80 ° C for 8 hours, and then calcining it at 500 ° C for 12 hours in a muffle furnace to obtain a solid powder; taking 2 g of the above solid powder, ultrasonically dispersing it in 150 mL of deionized water, and then adding 0.055 g of C 16 TAB, stirred for 1 hour; then added 1.59g of anhydrous Na2CO3, reacted at 90°C for 4 hours under stirring; collected the solid, ultrasonically dispersed it in water and ethanol solution, centrifuged and washed 3 times to separate the solid product; dried the solid product at 80°C for 8 hours, then calcined it at 800°C in a muffle furnace for 3 hours to obtain a solid powder, and reduced the solid powder with 10% H2 / N2 mixed gas at 800°C for 2 hours to obtain a catalyst.
[0044] Example 5
[0045] The preparation method of the mesoporous Ni@SiO2 methane dry reforming catalyst of this embodiment comprises the following steps:
[0046] 52 mL of cyclohexane and 26.5 mmol of Brij L4 were placed in a 150 mL round-bottom flask, followed by the addition of 1 mL of a 2 mol / L nickel chloride solution, stirring until transparent, adding 6 mmol of NaBH4, and stirring for 6 hours; 1.5 mL of ammonia water and 100 mmol of tetraethyl orthosilicate were added, and stirring was performed for 4 hours; the solid was collected by centrifugation, ultrasonically dispersed in acetone and ethanol solutions, and centrifuged and washed 3 times to separate the solid product; the solid product was dried at 80 ° C for 8 hours, and then calcined at 900 ° C for 3 hours in a muffle furnace to obtain a solid powder; 0.5 g of the above solid powder was taken, ultrasonically dispersed in 150 mL of deionized water, and then 0.275 g of C 16 TAB, stirred for 1 hour; then added 4.77g of anhydrous Na2CO3, reacted at 35°C under stirring conditions for 8 hours; collected the solid, ultrasonically dispersed it in water and ethanol solutions, centrifuged and washed 3 times, and separated to obtain a solid product; the solid product was dried at 80°C for 8 hours, and then calcined at 400°C in a muffle furnace for 12 hours to obtain a solid powder, and the solid powder was reduced with a 10% H2 / N2 mixed gas at 700°C for 5 hours to obtain a catalyst.
[0047] Example 6
[0048] The preparation method of the mesoporous Ni@SiO2 methane dry reforming catalyst of this embodiment comprises the following steps:
[0049] 130 mL of cyclohexane and 30 mmol of Brij L4 were placed in a 150 mL round-bottom flask, followed by the addition of 2.5 mL of a 0.4 mol / L nickel chloride solution, stirring until transparent, adding 5 mmol of NaBH4, stirring for 6 hours; adding 1.5 mL of ammonia water and 100 mmol of tetraethyl orthosilicate, stirring for 4 hours; collecting the solid by centrifugation, ultrasonically dispersing it in acetone and ethanol solutions, centrifugally washing it 3 times, and separating the solid product; drying the solid product at 80 ° C for 8 hours, and then calcining it at 700 ° C in a muffle furnace for 4 hours to obtain a solid powder; taking 0.8 g of the above solid powder, ultrasonically dispersing it in 150 mL of deionized water, and then adding 0.11 g of C 16 TAB, stirred for 1 hour; then added 3.18g of anhydrous Na2CO3, reacted at 90°C for 6 hours under stirring conditions; collected the solid, ultrasonically dispersed it in water and ethanol solutions, centrifuged and washed it 3 times, and separated the solid product; dried the solid product at 80°C for 8 hours, and then calcined it at 600°C in a muffle furnace for 5 hours to obtain a solid powder, and reduced the solid powder with 10% H2 / N2 mixed gas at 700°C for 5 hours to obtain a catalyst.
[0050] Example 7
[0051] The preparation method of the mesoporous Ni@SiO2 methane dry reforming catalyst of this embodiment comprises the following steps:
[0052] 80 mL of cyclohexane and 15 mmol of Brij O10 were placed in a 150 mL round-bottom flask, followed by the addition of 2 mL of a 0.25 mol / L nickel chloride solution, stirring until transparent, adding 2.5 mmol of LiAlH4, stirring for 6 hours; adding 1.0 mL of ammonia water and 30 mmol of tetraethyl orthosilicate, stirring for 4 hours; collecting the solid by centrifugation, ultrasonically dispersing it in acetone and ethanol solutions, centrifugally washing it 3 times, and separating the solid product; drying the solid product at 80 ° C for 8 hours, and then calcining it at 550 ° C in a muffle furnace for 5 hours to obtain a solid powder; taking 0.8 g of the above solid powder, ultrasonically dispersing it in 150 mL of deionized water, and then adding 0.18 g of C 14 TAB, stirred for 1 hour; then added 3.0g of anhydrous K2CO3, reacted at 70°C for 6 hours under stirring; collected the solid, ultrasonically dispersed it in water and ethanol solution, centrifuged and washed 3 times to separate the solid product; dried the solid product at 80°C for 8 hours, then calcined it at 550°C in a muffle furnace for 5 hours to obtain a solid powder, and reduced the solid powder with 10% H2 / N2 mixed gas at 700°C for 5 hours to obtain a catalyst.
[0053] Comparative Example 1
[0054] The preparation method of the Ni / SiO2 methane dry reforming catalyst of this comparative example comprises the following steps:
[0055] 4.0g of commercial SiO2 carrier was purchased and calcined at 750℃ for 3h to remove impurities in the carrier. Then 2.4g of Ni(NO3)2·6H2O was prepared into 1mol / L nickel nitrate solution and impregnated on the treated SiO2 carrier. After impregnation, it was dried at 80℃ for 12h. Finally, it was calcined at 700℃ for 6h to obtain Ni / SiO2 catalyst 4#.
[0056] Comparative Example 2
[0057] The preparation method of the Ni@SiO2 methane dry reforming catalyst of this comparative example is different from that of Example 2 in that it is not treated with a cationic surfactant. The specific steps are as follows:
[0058] 80 mL of cyclohexane and 15 mmol of Brij L4 were measured in a 150 mL round-bottom flask, followed by the addition of 2 mL of a 0.25 mol / L nickel chloride solution, stirring until transparent, adding 2.5 mmol of NaBH4, and stirring for 6 hours; adding 1.0 mL of ammonia water and 30 mmol of tetraethyl orthosilicate, and stirring for 4 hours; collecting the solid by centrifugation, ultrasonically dispersing it in acetone and ethanol solutions, and washing it by centrifugation for 3 times to separate the solid product; drying the solid product at 80°C for 8 hours, and then calcining it at 550°C in a muffle furnace for 5 hours to obtain a solid powder; reducing the solid powder with a 10% H2 / N2 mixed gas at 700°C for 5 hours to obtain catalyst 5#.
[0059] Application Examples
[0060] The catalysts prepared in Examples 1-3 and Comparative Examples 1-2 were used in a methane carbon dioxide reforming reaction, and their catalytic performance was tested. The specific test steps and results are as follows.
[0061] Test steps: Weigh 100g of catalysts 1-5# respectively, mix them with 100mg of quartz sand and load them into a fixed bed reactor for methane dry reforming reaction. The reaction conditions are: temperature 750℃, space velocity 54000ml / (g cat ·h), CH4 / CO2=1.0, the tail gas was analyzed by gas chromatography, and the analysis results are listed in Table 2.
[0062] Figure 4 and Figure 5 They are the N2 adsorption-desorption curve and pore size distribution diagram of the specific surface test results of the catalyst prepared in Example 2. Figure 4 and Figure 5It can be seen that the Ni@SiO2 catalyst prepared in Example 2 has a high specific surface area of 900m 2 / g, and the average pore size is about 3.2nm.
[0063] The methane dry reforming reaction performance evaluation data of the catalysts prepared in Examples 1-3 and Comparative Examples 1-2 are shown in Table 2. It can be seen that the Ni@SiO2 catalyst prepared in Example 2 has a methane dry reforming reaction performance of 750°C and 54000ml / (g cat ·h), the CH4 single-pass conversion rate can reach 91%, and the CO2 conversion rate can reach up to 96%, and the catalyst has no obvious performance degradation in the 50h performance test ( Figure 6 ).
[0064] Table 2. Evaluation data of methane dry reforming reaction performance of catalysts prepared in Examples 1-3 and Comparative Examples 1-2
[0065] catalyst <![CDATA[Air speed (h -1 )]]> <![CDATA[CH4 conversion rate (%)]]> <![CDATA[CO2 conversion rate (%)]]> Example 1 54000 82 90 Example 2 54000 91 96 Example 3 54000 86 92 Comparative Example 1 54000 19 23 Comparative Example 2 54000 18 42
[0066] From the above, it can be seen that the catalyst has good dispersion of active centers, high specific surface area, and especially high processing capacity and stability, and has good prospects in industrial applications.
[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A mesoporous Ni@SiO 2 Preparation method of methane dry reforming catalyst, It is characterized in that Here are the steps: (1) After mixing a Ni source aqueous solution, an alkane solvent, a nonionic surfactant and a reducing agent, ammonia water and tetraethyl orthosilicate are added to obtain a mixed solution; (2) stirring the mixed solution obtained in step (1) to react, centrifuging, washing, drying and calcining to obtain a solid powder; (3) dispersing the solid powder obtained in step (2) in water, adding a cationic surfactant and an alkaline inorganic salt to obtain an aqueous solution, stirring the reaction, and obtaining mesoporous Ni@SiO after centrifugation, washing, drying, roasting and hydrogen reduction. 2 Methane dry reforming catalyst.
2. The mesoporous Ni@SiO according to claim 1 2 Preparation method of methane dry reforming catalyst, It is characterized in that The Ni source in the Ni source aqueous solution in step (1) is NiNO 3 or NiCl 2 ; The alkane solvent is n-hexane, n-octane or cyclohexane; the nonionic surfactant is any one of Lutensol AO5, Brij L4 and Brij O10; the reducing agent is NaBH 4 , LiBH 4 KBH 4 and LiAlH 4 Any one of .
3. The mesoporous Ni@SiO according to claim 2 2 Preparation method of methane dry reforming catalyst, It is characterized in that In the step (1), the concentration of the Ni source aqueous solution is 0.1-2 mol / L; the volume ratio of the alkane solvent to the Ni source aqueous solution is (10-52):1; the concentration of the non-ionic surfactant in the mixed solution is 0.1-0.5 mol / L; the molar ratio of the reducing agent to the Ni source is (3-7):1; and the molar ratio of tetraethyl orthosilicate to the Ni source is (20-100):
1.
4. The mesoporous Ni@SiO according to claim 2 2 Preparation method of methane dry reforming catalyst, It is characterized in that The calcination temperature in step (2) is 500-900°C and the calcination time is 3-12 h.
5. The mesoporous Ni@SiO according to claim 2 2 Preparation method of methane dry reforming catalyst, It is characterized in that The cationic surfactant in step (3) is C 12 TAB, C 14 TAB, C 16 TAB and C 18 Any one of TAB; basic inorganic salt Na 2 CO 3 , K 2 CO 3 , CH 3 COONa and CH 3 Any of COOK.
6. The mesoporous Ni@SiO according to claim 2 2 Preparation method of methane dry reforming catalyst, It is characterized in that In the step (3), (3.0-13.0) g of solid powder is added to each liter of water; the concentration of the cationic surfactant in the aqueous solution is 1-5 mmol / L, and the concentration of the alkaline inorganic salt in the aqueous solution is 0.1-0.3 mol / L; the reaction temperature in the step (3) is 35-90° C. and the reaction time is 4-8 h.
7. The mesoporous Ni@SiO according to claim 2 2 Preparation method of methane dry reforming catalyst, It is characterized in that In the step (3), the calcination temperature is 400-800°C and the time is 3-12 h; the hydrogen reduction temperature is 700-800°C and the time is 2-5 h.
8. Mesoporous Ni@SiO prepared by the preparation method according to any one of claims 1 to 7 2 Methane dry reforming catalyst, It is characterized in that The mesoporous Ni@SiO 2 Methane dry reforming catalyst is Ni nanoparticles encapsulated in mesoporous SiO 2 Internally, the catalyst has a specific surface area of 70-900 m 2 / g, the mass percentage of Ni is 1-6%, the Ni particle size is 4-8 nm, and the mesoporous SiO 2 The pore size is 2-5 nm.
9. The mesoporous Ni@SiO according to claim 8 2 Application of methane dry reforming catalyst in methane carbon dioxide reforming reaction.
10. The use according to claim 9, It is characterized in that In the methane carbon dioxide reforming reaction, when the temperature is 750°C, the space velocity is 54000 ml / (gcat·h) and CH 4 / CO 2 =1.0, CH 4 The conversion rate is greater than 80%, CO 2 Conversion rate ≥90%.
Citation Information
Patent Citations
Preparation method of anti-carbon accumulation and anti-sintering methane dry reforming Ni-based catalyst
CN105964261A
M-SiO2 catalyst and preparation method thereof, and application of M-SiO2 catalyst to methane reforming with carbon dioxide
CN106268822A
PROCESS FOR THE PREPARATION OF Ni-CeMgAl2O4 CATALYST FOR DRY REFORMING OF METHANE WITH CARBON DIOXIDE
US20160001269A1
Cited By
Sulfur-resistant methane dry reforming catalyst as well as preparation method and application thereof
CN120515442A
An anti-sulfur methanation dry reforming catalyst, a preparation method and application thereof
CN120515442B