Zn-Fe / MMT catalyst and preparation method and application thereof

Through the preparation of Zn-Fe/MMT catalyst, modified montmorillonite is used to carry metal Zn and Fe, which solves the problem of low yield in the direct conversion of CH4 and CO2 into acetic acid, improves catalytic activity and selectivity, and achieves high efficiency. The effect of converting methane and carbon dioxide into acetic acid.

CN118767922APending Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310375841.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing technology, the reaction yield of direct conversion of CH4 and CO2 into acetic acid is low and thermodynamically unfavorable. There are problems such as activation of methane C-H bonds and low efficiency of C-C coupling of CH4 and CO2.

Method used

Zn-Fe/MMT catalyst is used to modify montmorillonite to load metal Zn and Fe. The catalyst is prepared by acidifying montmorillonite with gluconic acid and coordination chelation method to improve catalytic activity and selectivity and promote the C-H bonding of methane and carbon dioxide. C-O bond activation.

Benefits of technology

It significantly improves the yield and catalytic activity of converting methane and carbon dioxide into acetic acid, lowers the reaction energy barrier, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004171097600000081
    Figure BDA0004171097600000081
Patent Text Reader

Abstract

The invention provides a Zn-Fe / MMT catalyst as well as a preparation method and application thereof. The Zn-Fe / MMT catalyst prepared by the invention comprises modified montmorillonite, metal Zn and metal Fe. The prepared Zn-Fe / MMT catalyst has good catalytic activity and selectivity in the reaction of directly synthesizing acetic acid from methane and carbon dioxide, and the synergistic effect of Zn and Fe is beneficial to activation of C-H bonds of methane and C-O of CO2 in the process of preparing acetic acid from methane and carbon dioxide; and meanwhile, the high-oxygen-density MMT is beneficial to improving the dispersity and the loading capacity of Zn and Fe, so that the yield of preparing acetic acid from methane and carbon dioxide is improved. The Zn-Fe / MMT catalyst is prepared by adopting a coordination chelation method, the atom utilization rate is increased, and the preparation method is simple and suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to a Zn-Fe / MMT catalyst and a preparation method and application thereof. Background Art

[0002] CH4 and CO2 are the main greenhouse gases in the atmosphere. Excessive greenhouse gases in the atmosphere have caused an increasingly serious global warming problem and have attracted widespread attention from countries around the world. Therefore, converting CH4 and CO2 into high value-added products and reducing the content of CH4 and CO2 in the air have always been hot issues for researchers. At present, the processes for converting CH4 and CO2 into high value-added products can be divided into indirect conversion and direct conversion. Indirect conversion is to first reform to prepare synthesis gas, and then catalytically convert the synthesis gas into alcohols, hydrocarbons and other chemicals. This process often consumes a lot of energy and has high production costs. The direct conversion process avoids the high-pressure and high-temperature reaction requirements required for reforming CH4 and CO2 to produce synthesis gas, greatly shortening the reaction process route. The direct conversion of CH4 and CO2 into acetic acid meets the requirements of atom-economic reactions and is a reaction commonly used in direct conversion processes.

[0003] However, both CH4 and CO2 are very stable compounds, and the direct conversion of CH4 and CO2 into acetic acid is a thermodynamically unfavorable reaction. Among them, the CH bond activation of methane and the CC coupling of CH4 and CO2 are the key to the direct conversion of CH4 and CO2 into acetic acid. Previous studies have found that the transition metal Zn has a good activation effect on the CH of CH4, because the dissociative adsorption of CH4 on Zn is thermodynamically favorable and can significantly reduce the reaction energy barrier. However, the reaction of CH4 and CO2 to synthesize acetic acid in the prior art still has the problem of low yield of acetic acid. Summary of the invention

[0004] In order to solve the above problems in the prior art, the present invention proposes a Zn-Fe / MMT catalyst and a preparation method and application thereof.

[0005] In a first aspect, the present invention provides a Zn-Fe / MMT catalyst, comprising modified montmorillonite (MMT) and metal Zn and metal Fe supported on the modified montmorillonite.

[0006] As a specific embodiment of the present invention, the mass fraction of metal Zn in the modified montmorillonite is 0.002% to 0.5%; and / or the mass fraction of metal Fe in the modified montmorillonite is 0.002% to 3%.

[0007] As a specific embodiment of the present invention, the molar ratio of metal Zn to metal Fe is (1-10):1.

[0008] As a specific embodiment of the present invention, the modified montmorillonite is montmorillonite acidified with gluconic acid, and the added amount of gluconic acid is 2.0 wt% to 20 wt% of the mass of the montmorillonite.

[0009] Preferably, the montmorillonite is any one of sodium montmorillonite, calcium montmorillonite and magnesium montmorillonite, with a particle size of 0.2 to 1 μm and a specific surface area of ​​400 to 750 m 2 / g.

[0010] In a second aspect, the present invention provides a method for preparing a Zn-Fe / MMT catalyst, comprising:

[0011] Step 1, dispersing montmorillonite in a gluconic acid aqueous solution, stirring, filtering, and drying to obtain modified montmorillonite;

[0012] Step 2, preparing a solution A containing zinc salt, iron salt and catechol; preferably, in the process of preparing solution A, the concentration of zinc salt is 0.001-0.4 mol / L, the concentration of iron salt used is 0.001-0.1 mol / L, the concentration of catechol is 10%-20%, and the modified montmorillonite is dispersed in water to obtain a dispersion B; the solution A is contacted with the dispersion B for reaction, and the volume of the added solution A is 4%-6% of the volume of the dispersion B; after washing, drying and calcining, a Zn-Fe / MMT catalyst is obtained.

[0013] As a specific embodiment of the present invention, the calcination is carried out under an inert atmosphere, preferably nitrogen, the calcination temperature is 400-600° C., the heating rate is 1-10° C. / min, and the calcination time is 0.5-5 h.

[0014] As a specific embodiment of the present invention, the stirring time in step 1 is 2 to 4 hours, and the drying time is 4 to 7 days;

[0015] As a specific embodiment of the present invention, in step 2, the zinc salt aqueous solution and the iron salt aqueous solution are respectively added to the catechol aqueous solution, and stirred at room temperature for 20 to 60 minutes to prepare solution A;

[0016] As a specific embodiment of the present invention, modified montmorillonite is dispersed in water and stirred at room temperature for 12 to 24 hours to prepare dispersion B; preferably, the mass of montmorillonite in dispersion B is 2 wt % to 4 wt %.

[0017] As a specific embodiment of the present invention, solution A is added dropwise to dispersion B at a dropping speed of 10 to 20 mL / min, and stirred at room temperature for 5 to 12 hours.

[0018] As a specific embodiment of the present invention, the zinc salt is any one of zinc nitrate, zinc chloride and zinc sulfate.

[0019] As a specific embodiment of the present invention, the iron salt is any one of iron nitrate, iron chloride and iron sulfate.

[0020] As a specific embodiment of the present invention, the concentration of gluconic acid is 0.08 mol / L to 1.2 mol / L.

[0021] In a third aspect, the present invention provides a catalyst prepared by the preparation method provided by the second aspect of the present invention.

[0022] In a fourth aspect, the present invention provides a use of the Zn—Fe / MMT catalyst according to the first aspect or a third party's Zn—Fe / MMT catalyst in a process for synthesizing acetic acid from carbon dioxide and methane.

[0023] In a fifth aspect, the present invention provides a method for synthesizing acetic acid from methane and carbon dioxide.

[0024] As a specific embodiment of the present invention, the process of synthesizing acetic acid from methane and carbon dioxide uses CH4 and CO2 as raw materials, adopts the Zn-Fe / MMT catalyst of the first aspect of the present invention or the Zn-Fe / MMT catalyst prepared by the preparation method of the second aspect, and reacts in a fixed bed reactor. The reaction starts with nitrogen pretreatment at 150-200°C for 1-2h, and then the reaction gas is switched to CH4 and CO2, the volume ratio of CH4 to CO2 is 1: (1-10), and the volume space velocity is 360-1200h ~1 , the reaction temperature is 400-600°C, and the reaction pressure is 0.1-5.0MPa.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The Zn-Fe / MMT catalyst prepared by the present invention has good catalytic activity and selectivity in the direct synthesis of acetic acid from methane and carbon dioxide. The synergistic effect of Zn and Fe is beneficial to the activation of the CH bond of methane and the CO of CO2 in the process of preparing acetic acid from methane and carbon dioxide. At the same time, the MMT with high oxygen density helps to improve the dispersibility and loading amount of Zn and Fe, thereby improving the yield of preparing acetic acid from methane and carbon dioxide.

[0027] The invention adopts the coordination chelation method to prepare the Zn-Fe / MMT catalyst, thereby improving the atomic utilization rate, and the preparation method is simple and suitable for large-scale production. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with specific embodiments, but they do not constitute any limitation to the present invention.

[0029] In the examples, the reaction process was tested by an online gas chromatograph (Younglin Instruments, Acme 6000 series) equipped with FID and TCD.

[0030] Methane conversion rate = (moles of methane converted ÷ moles of methane flowing through the fixed bed reactor) × 100%;

[0031] The number of moles of methane converted = the number of moles of methane flowing through the fixed bed reactor - the number of moles of methane in the product;

[0032] Space-time yield of acetic acid = mass of acetic acid / (mass of catalyst × reaction time).

[0033] Example 1

[0034] Step 1: Preparation of modified montmorillonite:

[0035] Take 2g of the particle size of 0.5μm and the specific surface area of ​​600m 2 / g of sodium montmorillonite was dispersed in 15mL of 0.1mol / L gluconic acid aqueous solution, stirred at room temperature for 2h, filtered and vacuum dried for 4 days to obtain modified montmorillonite (abbreviated as "MMT");

[0036] Step 2: Preparation of Zn-Fe / MMT catalyst:

[0037] 1 mL of 0.001 mol / L Zn(NO3)2 aqueous solution and 1 mL of 0.001 mol / L Fe(NO3)3 aqueous solution were added to 0.5 mL of 15% catechol aqueous solution, stirred for 20 min, and prepared as solution A; 1 g of MMT was dispersed in 50 mL of deionized water, stirred for 12 h, and prepared as dispersion B; solution A was added dropwise to dispersion B at 10 mL / min, stirred for 5 h, then washed, dried, and ground to obtain powder. The powder was placed in a tubular furnace, heated to 400 ° C at a heating rate of 5 ° C / min under a nitrogen atmosphere, maintained for 5 h, and then rapidly cooled to room temperature to obtain a Zn-Fe / MMT catalyst, denoted as CAT-1.

[0038] The catalytic performance of the prepared catalyst was evaluated, and the specific steps were as follows:

[0039] 0.4 g of catalyst was weighed and loaded into a quartz reactor. It was pretreated with nitrogen at 200 °C for 1 h. The reaction temperature was raised to 450 °C. The volumetric space velocity of methane and carbon dioxide was 600 h-1. -1 The volume ratio of raw gas CH4:CO2 is 1:3. The evaluation results are shown in Table 1.

[0040] Example 2

[0041] Step 1: Preparation of modified montmorillonite:

[0042] Take 2g of the particle size of 0.5μm and the specific surface area of ​​600m 2 / g of sodium montmorillonite was dispersed in 10mL of 0.1mol / L gluconic acid aqueous solution, stirred at room temperature for 2h, filtered and vacuum dried for 4 days;

[0043] Step 2: Preparation of Zn-Fe / MMT catalyst:

[0044] 1mL 0.001mol / L Zn(NO3)2·6H2O solution and 1mL 0.001mol / L Fe(NO3)3·9H2O solution were added to 0.5mL 15% catechol aqueous solution, stirred for 60min, and prepared as solution A; 1g MMT was dispersed in 50mL deionized water, stirred for 12h, and prepared as dispersion B; solution A was added dropwise to dispersion B at 10mL / min, stirred for 12h, then washed, dried, and ground to obtain powder. The powder was placed in a tubular furnace, heated to 400℃ at a heating rate of 10℃ / min under a nitrogen atmosphere, maintained for 5h, and then quickly cooled to room temperature to obtain a Zn-Fe / MMT catalyst, denoted as CAT-2.

[0045] The catalytic performance of the prepared catalyst was evaluated, and the specific steps were as follows:

[0046] 0.4 g of catalyst was weighed and loaded into a quartz reactor. It was pretreated with nitrogen at 200 °C for 1 h. The reaction temperature was raised to 400 °C. The volumetric space velocity of methane and carbon dioxide was 360 h -1 The volume ratio of raw gas CH4:CO2 is 1:1. The evaluation results are shown in Table 1.

[0047] Example 3

[0048] Step 1: Preparation of modified montmorillonite:

[0049] Take 2g of the particle size of 0.5μm and the specific surface area of ​​600m 2 / g of sodium montmorillonite was dispersed in 15mL of 0.09mol / L gluconic acid aqueous solution, stirred at room temperature for 2h, filtered and vacuum dried for 4 days;

[0050] Step 2: Preparation of Zn-Fe / MMT catalyst:

[0051] 1mL 0.001mol / L ZnCl2 solution and 1mL 0.001mol / L FeCl3 solution were added to 0.5mL 15% catechol aqueous solution, stirred for 20min, and prepared as solution A; 1g MMT was dispersed in 50mL deionized water, stirred for 24h, and prepared as dispersion B; solution A was added dropwise to dispersion B at 20mL / min, stirred for 5h, then washed, dried, and ground to obtain powder. The powder was placed in a tubular furnace, heated to 600℃ at a heating rate of 1℃ / min under a nitrogen atmosphere, maintained for 5h, and then quickly cooled to room temperature to obtain a Zn-Fe / MMT catalyst, recorded as CAT-3.

[0052] The catalytic performance of the prepared catalyst was evaluated, and the specific steps were as follows:

[0053] 0.4 g of catalyst was weighed and loaded into a quartz reactor. It was pretreated with nitrogen at 200 °C for 1 h. The reaction temperature was raised to 600 °C. The volume space velocity of methane and carbon dioxide was 100 h -1 The volume ratio of raw gas CH4:CO2 is 1:1. The evaluation results are shown in Table 1.

[0054] Example 4

[0055] Step 1: Preparation of modified montmorillonite:

[0056] Take 2.5g of the particle size of 0.8μm and the specific surface area of ​​500m 2 / g of calcium-based montmorillonite was dispersed in 8mL of 0.3mol / L gluconic acid aqueous solution, stirred at room temperature for 2h, filtered and vacuum dried for 4 days;

[0057] Step 2: Preparation of Zn-Fe / MMT catalyst:

[0058] 1mL 0.04mol / L ZnSO4 solution and 1mL 0.008mol / L Fe2(SO4)3 solution were added to 0.5mL 15% catechol aqueous solution, stirred for 60min, and prepared as solution A; 1g MMT was dispersed in 50mL deionized water, stirred for 12h, and prepared as dispersion B; solution A was added dropwise to dispersion B at 20mL / min, stirred for 12h, then washed, dried, and ground to obtain powder. The powder was placed in a tubular furnace, heated to 400℃ at a heating rate of 1℃ / min under a nitrogen atmosphere, maintained for 5h, and then rapidly cooled to room temperature to obtain a Zn-Fe / MMT catalyst, recorded as CAT-4.

[0059] The catalytic performance of the prepared catalyst was evaluated, and the specific steps were as follows:

[0060] 0.4 g of catalyst was weighed and loaded into a quartz reactor. It was pretreated with nitrogen at 200 °C for 1 h. The reaction temperature was raised to 400 °C. The volumetric space velocity of methane and carbon dioxide was 360 h -1 The volume ratio of raw gas CH4:CO2 is 1:1. The evaluation results are shown in Table 1.

[0061] Example 5

[0062] Step 1: Preparation of modified montmorillonite:

[0063] Take 5g of the particle size of 0.8μm and the specific surface area of ​​500m 2 / g of calcium-based montmorillonite was dispersed in 10mL of 0.5mol / L gluconic acid aqueous solution, stirred at room temperature for 2h, filtered and vacuum dried for 4 days;

[0064] Step 2: Preparation of Zn-Fe / MMT catalyst:

[0065] 1mL 0.01mol / L Zn(NO3)2·6H2O solution and 1mL 0.008mol / L Fe2(SO4)3 solution were added to 0.5mL 15% catechol aqueous solution, stirred for 20min, and prepared as solution A; 1g MMT was dispersed in 50mL deionized water, stirred for 24h, and prepared as dispersion B; solution A was added dropwise to dispersion B at 10mL / min, stirred for 12h, then washed, dried, and ground to obtain powder. The powder was placed in a tubular furnace, heated to 600℃ at a heating rate of 10℃ / min under a nitrogen atmosphere, maintained for 0.5h, and then quickly cooled to room temperature to obtain a Zn-Fe / MMT catalyst, recorded as CAT-5.

[0066] The catalytic performance of the prepared catalyst was evaluated, and the specific steps were as follows:

[0067] 0.4 g of catalyst was weighed and loaded into a quartz reactor. It was pretreated with nitrogen at 200 °C for 1 h. The reaction temperature was raised to 600 °C. The volume space velocity of methane and carbon dioxide was 1000 h-1. -1 The volume ratio of raw gas CH4:CO2 is 1:10. The evaluation results are shown in Table 1.

[0068] Example 6

[0069] Step 1: Preparation of modified montmorillonite:

[0070] Take 3g of the particle size of 0.6μm and the specific surface area of ​​650m 2 / g magnesium-based montmorillonite was dispersed in 25mL of 0.09mol / L gluconic acid aqueous solution, stirred at room temperature for 2h, filtered and vacuum dried for 4 days;

[0071] Step 2: Preparation of Zn-Fe / MMT catalyst:

[0072] 1mL 0.01mol / L ZnCl2 solution and 1mL 0.001mol / L Fe(NO3)3·9H2O solution were added to 0.5mL 15% catechol aqueous solution, stirred for 60min, and prepared as solution A; 1g MMT was dispersed in 50mL deionized water, stirred for 12h, and prepared as dispersion B; solution A was added dropwise to dispersion B at 20mL / min, stirred for 5h, then washed, dried, and ground to obtain powder. The powder was placed in a tubular furnace, heated to 400℃ at a heating rate of 10℃ / min under a nitrogen atmosphere, maintained for 0.5h, and then quickly cooled to room temperature to obtain a Zn-Fe / MMT catalyst, recorded as CAT-6.

[0073] The catalytic performance of the prepared catalyst was evaluated, and the specific steps were as follows:

[0074] 0.4 g of catalyst was weighed and loaded into a quartz reactor. It was pretreated with nitrogen at 200 °C for 1 h. The reaction temperature was raised to 400 °C. The volume space velocity of methane and carbon dioxide was 1000 h-1. -1 The volume ratio of raw gas CH4:CO2 is 1:10. The evaluation results are shown in Table 1.

[0075] Example 7

[0076] Step 1: Preparation of modified montmorillonite:

[0077] Take 5g of the particle size of 0.6μm and the specific surface area of ​​650m 2 / g magnesium-based montmorillonite was dispersed in 5mL of 1mol / L gluconic acid aqueous solution, stirred at room temperature for 2h, filtered and vacuum dried for 4 days;

[0078] Step 2: Preparation of Zn-Fe / MMT catalyst:

[0079] 1mL 0.005mol / L ZnSO4 solution and 1mL 0.001mol / L FeCl3 solution were added to 0.5mL 15% catechol aqueous solution, stirred for 20min, and prepared as solution A; 1g MMT was dispersed in 50mL deionized water, stirred for 24h, and prepared as dispersion B; solution A was added dropwise to dispersion B at 10mL / min, stirred for 5h, then washed, dried, and ground to obtain powder. The powder was placed in a tubular furnace, heated to 600℃ at a heating rate of 1℃ / min under a nitrogen atmosphere, maintained for 0.5h, and then quickly cooled to room temperature to obtain a Zn-Fe / MMT catalyst, recorded as CAT-7.

[0080] The catalytic performance of the prepared catalyst was evaluated, and the specific steps were as follows:

[0081] 0.4 g of catalyst was weighed and loaded into a quartz reactor. It was pretreated with nitrogen at 200 °C for 1 h. The reaction temperature was raised to 400 °C. The volume space velocity of methane and carbon dioxide was 1000 h-1. -1 The volume ratio of raw gas CH4:CO2 is 1:10. The evaluation results are shown in Table 1.

[0082] Comparative Example 1

[0083] The difference between Comparative Example 1 and Example 1 is that no Zn(NO3)2 aqueous solution is added during the preparation of the catalyst in step 2, and the prepared catalyst is recorded as CAT-8. The catalyst prepared in Comparative Example 1 was evaluated for performance using the same catalytic performance evaluation method as in Example 1. The evaluation results are shown in Table 1.

[0084] Comparative Example 2

[0085] The difference between Comparative Example 2 and Example 1 is that no Fe(NO3)3 aqueous solution is added during the preparation of the catalyst in step 2, and the prepared catalyst is recorded as CAT-9. The catalyst prepared in Comparative Example 2 was evaluated for performance using the same catalytic performance evaluation method as in Example 1. The evaluation results are shown in Table 1.

[0086] Comparative Example 3

[0087] The difference between Comparative Example 3 and Example 1 is that the sodium-montmorillonite powder is directly used to prepare the catalyst without the modification step of step 1, and the prepared catalyst is recorded as CAT-10. The catalyst prepared in Comparative Example 3 is evaluated for performance using the same catalytic performance evaluation method as Example 1. The evaluation results are shown in Table 1.

[0088] Reference Example 1

[0089] The catalyst prepared by Rabie, AM, etc. is denoted as Cu-K + -ZSM-5, referenced by Rabie, AM; Betiha, MA; Park, SE

[0090] Table 1 Performance of Zn-Fe / MMT catalyst for direct synthesis of acetic acid from CH4 and CO2

[0091]

[0092] As can be seen from Table 1, the Zn-Fe / MMT catalyst has excellent catalytic performance for the direct synthesis of acetic acid from CH4 and CO2, with a maximum methane conversion rate of 7.8% and an acetic acid space-time yield of 1.58 mmol / (g·h). The catalyst prepared in Comparative Example 1 does not contain metal Zn, and the maximum methane conversion rate is 1.2%, and the acetic acid space-time yield is 0.20 mmol / (g·h); the catalyst prepared in Comparative Example 2 does not contain metal Fe, and the maximum methane conversion rate is 2.5%, and the acetic acid space-time yield is 0.41 mmol / (g·h); the catalyst prepared in Comparative Example 3 without modifying montmorillonite has a maximum methane conversion rate of 3.1%, and an acetic acid space-time yield of 0.60 mmol / (g·h).

[0093] In summary, the Zn-Fe / MMT catalyst prepared by the present invention can reduce the reaction energy barrier of synthesizing acetic acid from CH4 and CO2, and improve the methane conversion rate and the space-time yield of acetic acid.

[0094] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.

Claims

1. A Zn-Fe / MMT catalyst, characterized in that: The invention comprises modified montmorillonite and metal Zn and metal Fe loaded on the modified montmorillonite.

2. The catalyst according to claim 1, characterized in that The mass fraction of metal Zn in the modified montmorillonite is 0.002% to 0.5%; and / or the mass fraction of metal Fe in the modified montmorillonite is 0.002% to 3%.

3. The catalyst according to claim 1 or 2, characterized in that The molar ratio of the metal Zn to the metal Fe is (1-10):

1.

4. The catalyst according to any one of claims 1 to 3, characterized in that The modified montmorillonite is montmorillonite acidified with gluconic acid, and the amount of gluconic acid added is 2.0wt% to 20wt% of the mass of the montmorillonite; preferably, the montmorillonite is any one of sodium montmorillonite, calcium montmorillonite, and magnesium montmorillonite, with a particle size of 0.2 to 1 μm and a specific surface area of ​​400 to 750 m 2 / g.

5. A method for preparing a Zn-Fe / MMT catalyst, characterized in that: include: Step 1, dispersing montmorillonite in a gluconic acid aqueous solution, stirring, filtering, and drying to obtain modified montmorillonite; Step 2, preparing a solution A containing zinc salt, iron salt and catechol; preferably, in the process of preparing solution A, the concentration of zinc salt is 0.001-0.4 mol / L, the concentration of iron salt used is 0.001-0.1 mol / L, the concentration of catechol is 10%-20%, and the modified montmorillonite is dispersed in water to obtain a dispersion B; the solution A is contacted with the dispersion B for reaction, and the volume of the added solution A is 4%-6% of the volume of the dispersion B; after washing, drying and calcining, a Zn-Fe / MMT catalyst is obtained.

6. The method according to claim 5, characterized in that The calcination conditions in step 2 include: the calcination is carried out in an inert atmosphere, preferably a nitrogen atmosphere; and / or the calcination temperature is 400-600° C.; and / or the heating rate is 1-10° C. / min; and / or the calcination time is 0.5-5 h.

7. The method according to claim 5 or 6, characterized in that: In step 1, the stirring time is 2 to 4 hours and the drying time is 4 to 7 days; And / or, the method for preparing solution A in step 2 comprises: adding a zinc salt aqueous solution and an iron salt aqueous solution to a catechol aqueous solution, and stirring, preferably stirring at room temperature for 20 to 60 minutes; and / or, dispersing the modified montmorillonite in water to obtain dispersion B in step 2 comprises: dispersing the modified montmorillonite in water, and stirring at room temperature for 12 to 24 hours, preferably, the mass of montmorillonite in dispersion B is 2wt% to 4wt%; and / or, contacting solution A with dispersion B comprises: dropping solution A into dispersion B at a dropping speed of 10 to 20 mL / min, and stirring at room temperature for 5 to 12 hours.

8. The method according to any one of claims 5 to 7, characterized in that: The zinc salt is any one of zinc nitrate, zinc chloride and zinc sulfate; and / or the iron salt is any one of iron nitrate, iron chloride and iron sulfate.

9. The method according to any one of claims 5 to 8, characterized in that: The concentration of the gluconic acid is 0.08 mol / L to 1.2 mol / L.

10. A catalyst prepared by the preparation method according to any one of claims 5 to 9.

11. Use of the catalyst according to any one of claims 1 to 4 or the catalyst according to claim 10 in a process for synthesizing acetic acid from methane and carbon dioxide.

12. A method for synthesizing acetic acid from methane and carbon dioxide, characterized in that: With CH4 and CO2 as raw materials, the catalyst according to any one of claims 1 to 4 or the catalyst according to claim 10 is used to react in a fixed bed reactor; preferably, the reaction starts with nitrogen pretreatment at 150-200°C for 1-2h, and then the reaction gas is switched to CH4 and CO2, the volume ratio of CH4 to CO2 is 1: (1-10), and the volume space velocity is 360-1200h -1 , the reaction temperature is 400-600°C, and the reaction pressure is 0.1-5.0MPa.

Citation Information

Patent Citations

  • Preparation method of supported metal catalyst

    CN105562116A

  • Device for directly synthesizing C1-C4 alcohol by CH4 / CO2 at low temperature and synthesis method thereof

    CN109603707A

  • Supported MCM-41 catalyst as well as preparation method and application thereof

    CN114797948A

  • Modified montmorillonite-loaded ruthenium-based catalyst as well as preparation method and application thereof

    CN114832820A

  • Preparation method of HZSM-5 loaded solid superacid catalyst

    CN115430438A

Cited By

  • Process for preparing acetic acid through series connection of anaerobic fermentation and fixed bed thermocatalysis

    CN120423944A

  • Process for preparing acetic acid by anaerobic fermentation coupled with fixed bed thermal catalysis in series

    CN120423944B