Preparation method and application of catalyst for activating persulfate by using modified manganese slag

By using calcium oxide to activate electrolytic manganese slag to form a catalyst, the problem of high treatment costs of electrolytic manganese slag and dye wastewater is solved, and the effect of efficient degradation of organic pollutants is achieved, which is suitable for industrial applications.

CN118767939AActive Publication Date: 2024-10-15GUANGXI UNIV FOR NATITIES
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410731841.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-15
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

The existing technology has the problems of high cost, high energy consumption, and difficulty in industrial application when treating electrolytic manganese slag and dye wastewater. In addition, existing methods use explosive chemicals or high-cost oxidants, making it difficult to detoxify electrolytic manganese slag. processing and resource utilization.

Method used

Using calcium oxide as the oxidant, the electrolytic manganese slag is dried, ground, mixed and reacted with calcium oxide to form a modified electrolytic manganese slag catalyst, which is used to activate persulfate to generate highly oxidative active free radicals, degrade organic pollutants, and achieve Removal of high concentration organic wastewater.

Benefits of technology

It realizes high-value resource utilization of electrolytic manganese slag, reduces pollutant treatment costs, improves degradation efficiency, is simple to operate, low in cost, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004880432580000091
    Figure BDA0004880432580000091
  • Figure BDA0004880432580000101
    Figure BDA0004880432580000101
  • Figure BDA0004880432580000102
    Figure BDA0004880432580000102
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a modified manganese residue activated persulfate catalyst, and the preparation method of the catalyst comprises the following steps: step 1, drying, grinding and grinding a taken electrolytic manganese residue sample into uniform powder, and sieving with a 100-mesh sieve to prepare original electrolytic manganese residue powder; 2, mixing the original electrolytic manganese residue powder with deionized water, and stirring to obtain a uniformly mixed electrolytic manganese residue suspension; 3, calcium oxide is added into the electrolytic manganese residue turbid liquid, stirring reaction is carried out, and fully-reacted mixed liquid is obtained; 4, carrying out suction filtration on the mixed solution, washing until the solution is neutral, and drying; and 5, grinding and sieving with a 100-mesh sieve to prepare the modified electrolytic manganese residue catalyst. The modified electrolytic manganese residue catalyst is used for activating persulfate, full degradation of azo dyes represented by acid orange in a water body is achieved, the degradation rate is high, the preparation method is simple, the production cost is low, and industrial application and popularization are facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of environmental engineering and material science, and specifically relates to a catalyst preparation method for activating persulfate with modified manganese slag and application thereof. Background Art

[0002] Electrolytic manganese slag (EMR) is the main solid waste generated in the production process of electrolytic manganese metal. Its output is huge and growing. China alone produces more than 150 million tons of EMR each year. The main component of electrolytic manganese slag is acidic solid waste obtained by the reaction of manganese ore powder and sulfuric acid. The particle size is usually less than 80μm, the water content is high, and it contains a large amount of manganese, ammonia, and heavy metals such as copper, lead, nickel, and zinc. At present, due to technical limitations, landfill / dam stacking is the most common EMR disposal method, which not only occupies land resources, but also poses a serious threat to the environment. A large amount of accumulated electrolytic manganese slag will not only cause a large amount of waste of industrial raw materials, but also occupy a large amount of land resources during the stacking process. The dissolved harmful substances will also pollute the surrounding soil environment, water environment, etc., bringing serious potential harm to the ecological environment of the surrounding areas. Therefore, how to achieve the harmless treatment and disposal of electrolytic manganese slag and how to reuse EMR to realize resource utilization have become industry problems that the electrolytic manganese metal industry urgently needs to solve. Although a variety of treatment technologies have been proposed, such as water leaching, acid leaching, and alkali treatment, there are still deficiencies and problems in terms of adsorption performance and cost. Therefore, it is urgent to explore the harmless and resourceful utilization of electrolytic manganese slag.

[0003] Dye wastewater refers to wastewater containing pollutants such as dyes, auxiliaries, salts, and organic matter generated during the dyeing process. These dyes are difficult to degrade, have high chroma, and are highly polluting, and can easily cause great harm to the human body and the environment. At present, there have been many studies using biochar as a treatment agent for dye wastewater, but they all have problems such as difficulty in solid-liquid separation and low treatment efficiency. The advanced oxidation technology of sulfate radicals produced by activated persulfate has strong oxidizing properties, and it is feasible to use it to remove high-concentration organic wastewater. At the same time, EMR is rich in metal ions such as iron and manganese. It can activate persulfate without further adding transition metals, produce sulfate radicals, and oxidize and degrade high-concentration organic wastewater. It has certain potential and can be used as an adsorbent or to prepare catalysts for the degradation and removal of pollutants, which can achieve "waste treatment with waste".

[0004] Therefore, the application of persulfate activated by electrolytic manganese slag in high-concentration organic wastewater can not only realize the resource utilization of electrolytic manganese slag, reduce the company's stacking and treatment costs, and reduce ecological pollution, but also broaden the application path of "green and low-carbon" high-concentration organic wastewater.

[0005] At present, there have been many research reports on the preparation of manganese slag-based catalysts and their application in organic wastewater, but these methods still have some problems.

[0006] For example, Chinese patent application No. 202311025981.0 discloses a method for preparing a manganese slag-based catalyst and its application, wherein potassium permanganate, manganese slag and potassium persulfate are reacted to prepare a modified electrolytic manganese slag, and the removal rates of rhodamine B and antibiotics are above 98% and 70%, respectively. Although this method has a good removal effect on rhodamine B, potassium permanganate is an explosive drug, which is dangerous and has a high cost, and may not be able to be transformed into results, resulting in a large-scale industrial application.

[0007] For example, Chinese patent application No. 202311748945.7 discloses a method and application of preparing a denitrification catalyst by activating and calcining electrolytic manganese slag with oxalic acid. The method adds oxalic acid to the electrolytic manganese slag and then calcines it. The removal rate of nitrogen oxides can reach more than 50%. However, this method requires calcination at a temperature of 450 to 550°C, which is relatively costly.

[0008] For example, Chinese patent application No. 201611215237.7 discloses a method for efficient resource utilization of electrolytic manganese slag, which uses an alkali melting-hydrothermal synthesis method to obtain a zeolite product for use as a water treatment adsorbent. The alkali melting temperature used in this method is between 450 and 600°C, which has the problem of high cost and energy consumption.

[0009] For example, Chinese patent application No. 201910679732.0 discloses a method for preparing high-adsorption zeolite by microwave alkali melting activation of electrolytic manganese slag, which uses manganese slag, electrolytic manganese anolyte, and sodium hydroxide to heat at 400-600°C under microwave, and the prepared zeolite can be used as a water treatment adsorbent. However, this method uses microwave alkali melting, which has high energy consumption and high cost, and is difficult to achieve industrial application. Summary of the invention

[0010] The object of the present invention is to provide a catalyst preparation method and application of modified manganese slag activated persulfate in view of the deficiencies in the prior art. The present invention uses calcium oxide as an oxidant, which is cheaper than the cost of potassium permanganate used in the prior art, and calcium oxide (or quicklime) is the most convenient and simple method for washing manganese slag to remove ammonia nitrogen. While removing residual ammonia nitrogen in manganese slag, persulfate can also be activated to produce free radicals with high oxidation activity to degrade organic pollutants, resulting in a synergistic effect of "killing two birds with one stone". In addition, the organic wastewater targeted by this system has a broad spectrum, not a single organic wastewater, and therefore has a better promotion effect.

[0011] In order to achieve the above object, the present invention adopts the following technical solutions:

[0012] A method for preparing a catalyst for activating persulfate by modified manganese slag comprises the following steps:

[0013] Step 1: First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and then ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag powder;

[0014] Step 2, mixing the original electrolytic manganese slag powder obtained in the previous step with deionized water in a certain proportion, and stirring on a magnetic stirrer to obtain a uniformly mixed electrolytic manganese slag suspension;

[0015] Step 3, adding a certain amount of calcium oxide to the above-mentioned uniformly mixed electrolytic manganese slag suspension, and continuing to stir the reaction with a magnetic stirrer to obtain a fully reacted mixed solution;

[0016] Step 4: Filter the mixed solution obtained above and rinse it with deionized water until the solution is neutral, and dry the obtained solid in a drying oven at 75°C;

[0017] Step 5: Grind the dried solid with an agate mortar and pass it through a 100-mesh sieve to prepare a modified electrolytic manganese slag catalyst.

[0018] In the present invention, the main raw material is electrolytic manganese slag, which contains iron, aluminum, silicon, and trace manganese; and the metal elements contained in the electrolytic manganese slag can be metal elements that activate persulfate, so it can become a high-efficiency catalyst for persulfate. The preparation method of the present invention includes drying and grinding in step one, mixing reaction in steps two and three, and washing and drying in steps four and five, which is simple to operate and has low cost.

[0019] The purpose of drying and grinding in step 1 of the present invention is to use electrolytic manganese slag powder as raw material, so as to achieve mechanical activation of electrolytic manganese slag and provide more surface active sites; the mixing and stirring in step 2 is to dissolve part of manganese ions in the original electrolytic manganese slag into the solution, so as to facilitate the reaction with calcium oxide in the next step; calcium oxide is added to the suspension in step 3, and magnetic stirring is adopted to increase the reaction between calcium oxide and manganese ions, and at the same time, calcium oxide combines with water to release heat, which can also increase the reaction rate; after the reaction in step 3, on the one hand, the formation of the internal pore structure of the electrolytic manganese slag powder can be achieved, the specific surface area of ​​the modified electrolytic manganese slag catalyst is increased, and the increase of active sites of the modified electrolytic manganese slag catalyst is achieved; on the other hand, the stable loading of active species iron and manganese can effectively activate persulfate to produce strong oxidizing sulfate radicals (SO4-·), thereby effectively degrading organic pollutants.

[0020] The present invention further illustrates that in step 1, the electrolytic manganese slag sample is dried in an oven at 60-85° C. for 24-72 hours to remove the retained moisture in the electrolytic manganese slag and then ground into small pieces using an agate mortar.

[0021] The present invention further illustrates that in step 2, the solid-liquid ratio (kg:L) of the original electrolytic manganese slag powder and deionized water is 0.1-0.5; and the stirring time of the electrolytic manganese slag suspension is 0.25-12h.

[0022] The present invention further illustrates that in step three, the addition ratio (kg:kg) of the calcium oxide and the original electrolytic manganese slag is 0.1 to 0.6; and the stirring reaction time is 0.25 to 12 hours.

[0023] The present invention also provides a modified electrolytic manganese slag catalyst prepared by the above-mentioned preparation method.

[0024] The present invention also provides an application of the modified electrolytic manganese slag catalyst in a persulfate activation system, which is used for degrading organic dyes or antibiotic wastewater in water.

[0025] The application of the modified electrolytic manganese slag catalyst in the persulfate activation system is further described. The specific application is: persulfate is added to a water body containing acid orange azo dyes to obtain a mixed solution, and then the modified electrolytic manganese slag catalyst is added, and a magnetic stirrer is used to mix and stir the reaction for 2 to 3 hours to complete the degradation of the azo dyes in the water body.

[0026] The application further illustrates that in the water body containing acid orange azo dyes, the added amount of the persulfate is 0.5-2 mmol / L; and the added amount of the modified electrolytic manganese slag catalyst is 0.25-2.00 g / L.

[0027] The application further illustrates that the concentration of acid orange in the water of the acid orange azo dye is 10 to 100 mg / L.

[0028] The application of the modified electrolytic manganese slag catalyst in the persulfate activation system further illustrates that the pH value of the organic dye or antibiotic wastewater ranges from 3 to 11; during the degradation reaction, the degradation reaction temperature is 5 to 40° C., and the degradation reaction time is 5 to 30 min.

[0029] Advantages of the present invention:

[0030] 1. The modified manganese slag activated persulfate catalyst preparation method of the present invention comprises step 1 of drying and grinding, steps 2 and 3 of mixing reaction, and steps 4 and 5 of washing and drying, which is simple to operate and has low cost.

[0031] 2. The modified electrolytic manganese slag catalyst of the present invention can efficiently activate persulfate to generate free radicals with high oxidation ability, is simple to operate, and has strong feasibility, thereby improving the efficiency of degrading organic pollutants.

[0032] 3. The modified electrolytic manganese slag catalyst of the present invention has good chemical stability, relatively fast preparation speed, good degradation effect, and can significantly reduce the cost of pollutant treatment.

[0033] 4. The modified electrolytic manganese slag catalyst of the present invention has electrolytic manganese slag as its main raw material, which can realize high-value resource utilization of electrolytic manganese slag and solve the pollution problem caused by the stacking of electrolytic manganese slag.

[0034] 5. The modified electrolytic manganese slag catalyst of the present invention uses calcium oxide as a modifier, which is commercially available, does not need to be made by oneself, does not need secondary processing, has low cost, is harmless and non-toxic, and has strong usability.

[0035] 6. The modified electrolytic manganese slag catalyst of the present invention uses calcium oxide as a modifier to increase the hardness of the modified electrolytic manganese slag, making it possible to directly granulate the manganese slag and providing a basis for subsequent industrial applications.

[0036] 7. The modified electrolytic manganese slag catalyst of the present invention is used to activate persulfate to degrade organic pollutants. It not only has high catalytic activity, which makes the pollutant degradation efficiency high, but also can realize the high-value resource utilization of electrolytic manganese slag solid waste. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 The SEM images of the original unmodified electrolytic manganese slag and the modified electrolytic manganese slag catalyst of Example 3 of the present invention;

[0038] Figure 2 is the standard curve of AO7 solution concentration;

[0039] Figure 3 It is a curve diagram showing the change in removal rate of Acid Orange 7 (AO7) by the modified electrolytic manganese slag catalyst of Examples 1-9 and Comparative Examples 1-2;

[0040] Figure 4 It is the variation curve of the removal rate of acid orange 7 (AO7) in different systems;

[0041] Figure 5 It is a curve diagram showing the change of the removal rate of acid orange 7 (AO7) by the modified electrolytic manganese slag catalyst of Example 3 due to common anions;

[0042] Figure 6 It is a curve diagram showing the change of the removal rate of acid orange 7 (AO7) by the modified electrolytic manganese slag catalyst of Example 3 with humic acid;

[0043] Figure 7 The figure is a curve diagram showing the change of the removal rate of Acid Orange 7 (AO7) by the modified electrolytic manganese slag catalyst of Example 3 at different pH values;

[0044] Figure 8This is a curve chart showing the change in removal rate of other pollutants by the modified electrolytic manganese slag catalyst in Example 3. DETAILED DESCRIPTION

[0045] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] In the examples of the present invention, unless otherwise specified, all raw material components are commercially available products well known to those skilled in the art; in the examples of the present invention, unless otherwise specified, the technical means used are conventional means well known to those skilled in the art.

[0047] Example 1

[0048] A method for preparing a catalyst for activating persulfate by modified manganese slag comprises the following steps:

[0049] S1. First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag powder;

[0050] S2, 5g of the original electrolytic manganese slag powder obtained in the previous step was mixed with 15mL of deionized water, and stirred on a magnetic stirrer for 30min to obtain a uniformly mixed electrolytic manganese slag suspension;

[0051] S3, adding 2g of calcium oxide to the above-mentioned uniformly mixed electrolytic manganese slag suspension, and continuing to stir the reaction with a magnetic stirrer for 60min to obtain a fully reacted mixed solution;

[0052] S4, the mixed solution obtained above is filtered and rinsed with deionized water until the solution is neutral, and the obtained solid is placed in a drying oven at 75°C for drying;

[0053] S5. Grind the dried solid with an agate mortar and pass it through a 100-mesh sieve to prepare a modified electrolytic manganese slag catalyst.

[0054] Example 2

[0055] A method for preparing a catalyst for activating persulfate by modified manganese slag comprises the following steps:

[0056] S1. First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag powder;

[0057] S2, 5g of the original electrolytic manganese slag powder obtained in the previous step was mixed with 20mL of deionized water, and stirred on a magnetic stirrer for 30min to obtain a uniformly mixed electrolytic manganese slag suspension;

[0058] S3, adding 2g of calcium oxide to the above-mentioned uniformly mixed electrolytic manganese slag suspension, and continuing to stir the reaction with a magnetic stirrer for 60min to obtain a fully reacted mixed solution;

[0059] S4, the mixed solution obtained above is filtered and rinsed with deionized water until the solution is neutral, and the obtained solid is placed in a drying oven at 75°C for drying;

[0060] S5. Grind the dried solid with an agate mortar and pass it through a 100-mesh sieve to prepare a modified electrolytic manganese slag catalyst.

[0061] Example 3

[0062] A method for preparing a catalyst for activating persulfate by modified manganese slag comprises the following steps:

[0063] S1. First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag powder;

[0064] S2, 5g of the original electrolytic manganese slag powder obtained in the previous step was mixed with 25mL of deionized water, and stirred on a magnetic stirrer for 30min to obtain a uniformly mixed electrolytic manganese slag suspension;

[0065] S3, adding 2g of calcium oxide to the above-mentioned uniformly mixed electrolytic manganese slag suspension, and continuing to stir the reaction with a magnetic stirrer for 60min to obtain a fully reacted mixed solution;

[0066] S4, the mixed solution obtained above is filtered and rinsed with deionized water until the solution is neutral, and the obtained solid is placed in a drying oven at 75°C for drying;

[0067] S5. Grind the dried solid with an agate mortar and pass it through a 100-mesh sieve to prepare a modified electrolytic manganese slag catalyst.

[0068] like Figure 1 As shown in the figure, a is the original electrolytic manganese slag powder obtained in Example S1, and b is the modified electrolytic manganese slag catalyst obtained in this example. Figure 1 It can be seen that compared with the original electrolytic manganese slag, a network nanostructure appears in the modified electrolytic manganese slag, which makes it have a larger specific surface area, thereby providing more active sites for the catalyst reaction and making it have higher catalytic reaction activity.

[0069] Example 4

[0070] A method for preparing a catalyst for activating persulfate by modified manganese slag comprises the following steps:

[0071] S1. First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag powder;

[0072] S2, 5g of the original electrolytic manganese slag powder obtained in the previous step was mixed with 25mL of deionized water, and stirred on a magnetic stirrer for 30min to obtain a uniformly mixed electrolytic manganese slag suspension;

[0073] S3, adding 0.5g of calcium oxide to the above-mentioned uniformly mixed electrolytic manganese slag suspension, and continuing to stir the reaction with a magnetic stirrer for 60min to obtain a fully reacted mixed solution;

[0074] S4, the mixed solution obtained above is filtered and rinsed with deionized water until the solution is neutral, and the obtained solid is placed in a drying oven at 75°C for drying;

[0075] S5. Grind the dried solid with an agate mortar and pass it through a 100-mesh sieve to prepare a modified electrolytic manganese slag catalyst.

[0076] Example 5

[0077] A method for preparing a catalyst for activating persulfate by modified manganese slag comprises the following steps:

[0078] S1. First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag powder;

[0079] S2, 5g of the original electrolytic manganese slag powder obtained in the previous step was mixed with 25mL of deionized water, and stirred on a magnetic stirrer for 30min to obtain a uniformly mixed electrolytic manganese slag suspension;

[0080] S3, adding 1g of calcium oxide to the above-mentioned uniformly mixed electrolytic manganese slag suspension, and continuing to stir the reaction with a magnetic stirrer for 60min to obtain a fully reacted mixed solution;

[0081] S4, the mixed solution obtained above is filtered and rinsed with deionized water until the solution is neutral, and the obtained solid is placed in a drying oven at 75°C for drying;

[0082] S5. Grind the dried solid with an agate mortar and pass it through a 100-mesh sieve to prepare a modified electrolytic manganese slag catalyst.

[0083] Example 6

[0084] A method for preparing a catalyst for activating persulfate by modified manganese slag comprises the following steps:

[0085] S1. First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag powder;

[0086] S2, 5g of the original electrolytic manganese slag powder obtained in the previous step was mixed with 25mL of deionized water, and stirred on a magnetic stirrer for 30min to obtain a uniformly mixed electrolytic manganese slag suspension;

[0087] S3, adding 3g of calcium oxide to the above-mentioned uniformly mixed electrolytic manganese slag suspension, and continuing to stir the reaction with a magnetic stirrer for 60min to obtain a fully reacted mixed solution;

[0088] S4, the mixed solution obtained above is filtered and rinsed with deionized water until the solution is neutral, and the obtained solid is placed in a drying oven at 75°C for drying;

[0089] S5. Grind the dried solid with an agate mortar and pass it through a 100-mesh sieve to prepare a modified electrolytic manganese slag catalyst.

[0090] Example 7

[0091] A method for preparing a catalyst for activating persulfate by modified manganese slag comprises the following steps:

[0092] S1. First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag powder;

[0093] S2, 5g of the original electrolytic manganese slag powder obtained in the previous step was mixed with 25mL of deionized water, and stirred on a magnetic stirrer for 30min to obtain a uniformly mixed electrolytic manganese slag suspension;

[0094] S3, adding 2g of calcium oxide to the above-mentioned uniformly mixed electrolytic manganese slag suspension, and continuing to stir the reaction with a magnetic stirrer for 15min to obtain a fully reacted mixed solution;

[0095] S4, the mixed solution obtained above is filtered and rinsed with deionized water until the solution is neutral, and the obtained solid is placed in a drying oven at 75°C for drying;

[0096] S5. Grind the dried solid with an agate mortar and pass it through a 100-mesh sieve to prepare a modified electrolytic manganese slag catalyst.

[0097] Example 8

[0098] A method for preparing a catalyst for activating persulfate by modified manganese slag comprises the following steps:

[0099] S1. First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag powder;

[0100] S2, 5g of the original electrolytic manganese slag powder obtained in the previous step was mixed with 25mL of deionized water, and stirred on a magnetic stirrer for 30min to obtain a uniformly mixed electrolytic manganese slag suspension;

[0101] S3, adding 2g of calcium oxide to the above-mentioned uniformly mixed electrolytic manganese slag suspension, and continuing to stir the reaction with a magnetic stirrer for 30min to obtain a fully reacted mixed solution;

[0102] S4, the mixed solution obtained above is filtered and rinsed with deionized water until the solution is neutral, and the obtained solid is placed in a drying oven at 75°C for drying;

[0103] S5. Grind the dried solid with an agate mortar and pass it through a 100-mesh sieve to prepare a modified electrolytic manganese slag catalyst.

[0104] Example 9

[0105] A method for preparing a catalyst for activating persulfate by modified manganese slag comprises the following steps:

[0106] S1. First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag powder;

[0107] S2, 5g of the original electrolytic manganese slag powder obtained in the previous step was mixed with 25mL of deionized water, and stirred on a magnetic stirrer for 30min to obtain a uniformly mixed electrolytic manganese slag suspension;

[0108] S3, adding 2g of calcium oxide to the above-mentioned uniformly mixed electrolytic manganese slag suspension, and continuing to stir the reaction with a magnetic stirrer for 90min to obtain a fully reacted mixed solution;

[0109] S4, the mixed solution obtained above is filtered and rinsed with deionized water until the solution is neutral, and the obtained solid is placed in a drying oven at 75°C for drying;

[0110] S5. Grind the dried solid with an agate mortar and pass it through a 100-mesh sieve to prepare a modified electrolytic manganese slag catalyst.

[0111] Comparative Example 1

[0112] The preparation method of the electrolytic manganese slag of this comparative example 1 is:

[0113] S1. First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag.

[0114] Comparative Example 2

[0115] The preparation method of the electrolytic manganese slag of this comparative example 2 is:

[0116] S1. First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag.

[0117] S2, 5g of the original electrolytic manganese slag powder obtained in the previous step was mixed with 25mL of deionized water, and stirred on a magnetic stirrer for 30min to obtain a uniformly mixed electrolytic manganese slag suspension;

[0118] S3, the suspension obtained above is filtered and rinsed with deionized water until the solution is neutral, and the obtained solid is placed in a drying oven at 75°C for drying;

[0119] S4. Grind the dried solid with an agate mortar and pass it through a 100-mesh sieve to prepare a modified electrolytic manganese slag catalyst.

[0120] In order to further illustrate the effect of the present invention, the modified electrolytic manganese slag catalysts prepared in Examples 1-7 and Comparative Examples 1-2 are specifically tested below.

[0121] Application Example 1

[0122] Several portions of Acid Orange 7 (AO7) solution were prepared, wherein the concentration of AO7 was 40 mg / L. The modified electrolytic manganese slag catalysts prepared in the above-mentioned Examples 1-7 and Comparative Examples 1-2 were taken, wherein the concentration of the modified electrolytic manganese slag catalyst was 0.3 g / L, and added to the acid orange 7 (AO7) solution and placed on a magnetic stirrer, reacted for 30 min to reach adsorption and desorption equilibrium, and potassium persulfate (PMS) was added at ambient temperature, wherein the concentration of PMS was 1 mmol / L, and 3 mL of sample was taken at different time intervals (0, 5, 10, 15, 20, 300 min), filtered with a cellulose acetate filter, and then mixed with 1 mL of MeOH for storage. The concentration of the sample was determined at the absorption peak of 483 nm using a UV-visible spectrophotometer, and all experiments were repeated three times to take the average value to reduce experimental errors and ensure accuracy.

[0123] It is worth noting that the persulfate in the present invention includes but is not limited to sodium persulfate, potassium persulfate, ammonium persulfate and the like.

[0124] The degradation effect was determined by UV-visible spectrophotometer, and the AO7 concentration standard curve was drawn as follows:

[0125] Prepare AO7 solution with a concentration of 40 mg / L, dilute it to 1, 2, 5, 10, 15 and 20 mg / L, and finally obtain AO7 solutions with concentrations of 1, 2, 5, 10, 15, 20 and 40 mg / L. Use a UV-visible spectrophotometer to measure the absorbance of AO7 solutions of different concentrations at the absorption peak of 483 nm. Perform a linear fit between the measured absorbance and the concentration of AO7 solution to obtain the following: Figure 2 The standard curve of AO7 solution concentration is shown.

[0126] The degradation efficiency of AO7 is calculated according to the following formula 2.1:

[0127] E=(C0–C) / C0×100%

[0128] Wherein C0 represents the initial concentration of AO7 (mg / L), C represents the measured concentration of AO7 (mg / L), and E represents the degradation efficiency of AO7 (%).

[0129] The removal rates (%) of AO7 by each group of modified electrolytic manganese slag catalysts are shown in Table 1 and Figure 3 As shown:

[0130] Table 1

[0131]

[0132] As shown in Table 1 and Figure 3 The test results show that the modification time and the amount of calcium oxide used have a great influence on the final AO7 degradation results, as follows:

[0133] (1) In Examples 1-3, as the ratio (g:mL) of the original electrolytic manganese slag to deionized water decreases, the ability of the modified electrolytic manganese slag to catalyze the degradation of AO7 by PMS gradually increases. Considering the actual situation, the optimal ratio is selected as 1:5.

[0134] (2) Compared with Example 3, in Examples 4-6, as the ratio of calcium oxide to original electrolytic manganese slag increases, the ability of the modified electrolytic manganese slag to catalyze PMS to degrade AO7 gradually increases. From the perspective of economy, the optimal dosage ratio (g:g) of the modified electrolytic manganese slag to calcium oxide to original electrolytic manganese slag is 2:5.

[0135] (3) Compared with Example 3, in Examples 7-9, as the reaction time increases, the ability of the modified electrolytic manganese slag to catalyze PMS to degrade AO7 gradually increases. Considering the time cost, the reaction time of the modified electrolytic manganese slag is 60 min.

[0136] Application Example 2

[0137] Prepare 3 portions of AO7 solution, wherein the concentration of AO7 is 40 mg / L. Take 2 portions of the modified electrolytic manganese slag catalyst added in the above Example 3 and add them to the AO7 solution respectively, and place them on a magnetic stirrer, wherein the concentration of the modified electrolytic manganese slag catalyst is 0.3 g / L, and react for 30 minutes to reach adsorption and desorption equilibrium, wherein one bottle is added with PMS at ambient temperature, wherein the concentration of PMS is 1 mmol / L, and no PMS is added to the control sample. Take the remaining bottle of AO7 solution, do not add the modified electrolytic manganese slag, only add PMS at ambient temperature, wherein the concentration of PMS is 1 mmol / L, and other conditions remain unchanged.

[0138] 3 mL of sample was taken at different time intervals (0, 5, 10, 15, 20, 300 min), filtered through a cellulose acetate filter, and then mixed with 1 mL of MeOH for storage. The concentration of the sample was determined at the absorption peak of 483 nm using a UV-visible spectrophotometer. All experiments were repeated three times and the average value was taken to reduce experimental errors and ensure accuracy.

[0139] The removal rates (%) of AO7 by different systems are shown in Table 2 and Figure 4 As shown:

[0140] Table 2

[0141]

[0142] As shown in Table 2 and Figure 4 As shown, the degradation ability of AO7 by adding only PMS or modified electrolytic manganese slag system is very low, but the degradation ability of AO7 by modified electrolytic manganese slag / PMS system is greatly improved. It can be said that the modified electrolytic manganese slag catalyst prepared by the present invention can efficiently activate PMS and greatly improve the ability to degrade AO7.

[0143] Application Example 3

[0144] Prepare several portions of AO7 solution, wherein the concentration of AO7 is 40 mg / L. Take the modified electrolytic manganese slag catalyst of Example 3 above and add them to the AO7 solution respectively, and place it on a magnetic stirrer, wherein the concentration of the modified electrolytic manganese slag catalyst is 0.3 g / L, react for 30 minutes to reach adsorption and desorption equilibrium, add PMS at ambient temperature, wherein the concentration of PMS is 1 mmol / L, add chloride ions, nitrate ions, sulfate ions and bicarbonate ions to the solution respectively, wherein the ion concentration is 20 mg / L, and take a group of blank samples without adding anions.

[0145] 3 mL of sample was taken at different time intervals (0, 5, 10, 15, 20, 300 min), filtered through a cellulose acetate filter, and then mixed with 1 mL of MeOH for storage. The concentration of the sample was determined at the absorption peak of 483 nm using a UV-visible spectrophotometer. All experiments were repeated three times and the average value was taken to reduce experimental errors and ensure accuracy.

[0146] The removal rates (%) of AO7 by the modified electrolytic manganese slag catalyst of Example 3 with different common anions are shown in Table 3 and Figure 5 As shown:

[0147] Table 3

[0148]

[0149]

[0150] As shown in Table 3 and Figure 5 As shown in the figure, the effects of different common anions on the ability of modified electrolytic manganese slag to catalyze the degradation of AO7 by PMS. - The degradation of AO7 was promoted by excessive Cl - It reacts with oxidative active substances to generate HOCl or Cl in the system, thereby increasing the degradation rate of AO7; NO3 - It has almost no effect on the degradation of AO7; SO4 2- It has a certain inhibitory effect on the degradation of AO7, but the average degradation efficiency can still reach 99.3%. This may be because when the initial sulfate ion concentration is high, the decomposition of PMS into sulfate ions is inhibited, thereby reducing the generation of oxidative active substances, thereby reducing the decomposition rate of AO7 to a certain extent; HCO3 - It has a certain inhibitory effect on the degradation of AO7, HCO3 - It is possible that PMS can be competitively adsorbed with AO7 on the surface of the modified electrolytic manganese slag. This competitive adsorption reduces the contact opportunity between AO7 and manganese slag, thereby reducing the degradation efficiency of PMS on AO7. However, the modified electrolytic manganese slag catalyst prepared by the present invention still has good performance and is capable of practical application.

[0151] Application Example 4

[0152] Prepare several portions of AO7 solution, wherein the concentration of AO7 is 40 mg / L. Take the modified electrolytic manganese slag catalyst of Example 3 above and add them to the AO7 solution respectively, and place it on a magnetic stirrer, wherein the concentration of the modified electrolytic manganese slag catalyst is 0.3 g / L, react for 30 minutes to achieve adsorption and desorption equilibrium, add PMS at ambient temperature, wherein the concentration of PMS is 1 mmol / L, add humic acid to the solution, and the concentrations are 5, 10 and 20 mg / L respectively, and no humic acid is added to the blank sample.

[0153] 3 mL of sample was taken at different time intervals (0, 5, 10, 15, 20, 300 min), filtered through a cellulose acetate filter, and then mixed with 1 mL of MeOH for storage. The concentration of the sample was determined at the absorption peak of 483 nm using a UV-visible spectrophotometer. All experiments were repeated three times and the average value was taken to reduce experimental errors and ensure accuracy.

[0154] The removal rate (%) of AO7 by humic acid on the modified electrolytic manganese slag catalyst of Example 3 is shown in Table 4 and Figure 6 As shown:

[0155] Table 4

[0156]

[0157] As shown in Table 4 and Figure 6 As shown, the effect of different concentrations of humic acid on the ability of modified electrolytic manganese slag to catalyze the degradation of AO7 by PMS. Under the conditions of humic acid concentrations of 5.0 mg / L, 10.0 mg / L, and 20.0 mg / L, the degradation efficiency of AO7 was 88.62%, 85.01%, and 84.75%, respectively. Compared with the condition without HA, the degradation efficiency of AO7 was reduced by 7.3%, which may be because humic acid reacted with the oxidative active substances in the reaction system, thereby inhibiting the degradation efficiency of AO7. However, it can be found that even when the humic acid concentration was 20.0 mg / L, the degradation efficiency of AO7 was still as high as 84.8%. Therefore, humic acid has a certain effect on the ability of modified electrolytic manganese slag to catalyze the degradation of AO7 by PMS, but the modified electrolytic manganese slag catalyst still has the prospect of application in complex water bodies.

[0158] Application Example 5

[0159] Prepare several portions of AO7 solution, wherein the concentration of AO7 is 40.0 mg / L. Take the modified electrolytic manganese slag catalyst of Example 3 above and add it to the AO7 solution respectively, and place it on a magnetic stirrer, wherein the concentration of the modified electrolytic manganese slag catalyst is 0.3 g / L, react for 30 minutes to achieve adsorption and desorption equilibrium, add PMS at ambient temperature, wherein the concentration of PMS is 1 mmol / L, and adjust the solution pH to 4, 5, 6, 7, 8, 9 and 10, wherein the pH of the blank sample is not adjusted.

[0160] 3 mL of sample was taken at different time intervals (0, 5, 10, 15, 20, 300 min), filtered through a cellulose acetate filter, and then mixed with 1 mL of MeOH for storage. The concentration of the sample was determined at the absorption peak of 483 nm using a UV-visible spectrophotometer. All experiments were repeated three times and the average value was taken to reduce experimental errors and ensure accuracy.

[0161] The removal rate (%) of AO7 by the modified electrolytic manganese slag catalyst of Example 3 at different pH values ​​is shown in Table 5 and Figure 7 As shown:

[0162] Table 5

[0163]

[0164] As shown in Table 5 and Figure 7 As shown, the effect of different pH values ​​on the ability of modified electrolytic manganese slag to catalyze PMS degradation of AO7. It can be seen that pH has little effect on the modified electrolytic manganese slag catalyst prepared by the present invention, and the modified electrolytic manganese slag catalyst still has the prospect of application in complex water bodies.

[0165] Application Example 6

[0166] Prepare several solutions, including AO7 solution, methyl orange solution, rhodamine B solution, tetracycline hydrochloride solution and oxytetracycline hydrochloride solution, wherein the concentration of AO7 solution is 40 mg / L, and the concentration of other pollutant solutions is 20 mg / L; take the modified electrolytic manganese slag catalyst of Example 3 above and add them to the above solutions respectively, and place them on a magnetic stirrer, wherein the concentration of the modified electrolytic manganese slag catalyst is 0.3 g / L, react for 30 minutes to reach adsorption and desorption equilibrium, and add potassium permonosulfate (PMS) at ambient temperature, wherein the concentration of PMS is 1 mmol / L.

[0167] 3 mL of sample was taken at different time intervals (0, 5, 10, 15, 20, 300 min), filtered through a cellulose acetate filter, and then mixed with 1 mL of MeOH for storage. The concentration of the sample was determined at the absorption peak of 483 nm using a UV-visible spectrophotometer. All experiments were repeated three times and the average value was taken to reduce experimental errors and ensure accuracy.

[0168] The removal rate (%) of other pollutants by the modified electrolytic manganese slag catalyst of Example 3 is shown in Table 6 and Figure 8 As shown:

[0169] Table 6

[0170]

[0171] As shown in Table 6 and Figure 8 As shown, the ability of the modified electrolytic manganese slag to catalyze PMS to degrade other pollutants. It can be seen that the modified electrolytic manganese slag catalyst prepared by the present invention still has a high removal effect on other organic pollutants, and the modified electrolytic manganese slag catalyst still has a high application prospect.

[0172] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0173] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A method for preparing a catalyst for activating persulfate by modified manganese slag, characterized in that: The following steps are involved: Step 1: First, the retrieved electrolytic manganese slag sample is placed in an oven for drying, then ground with an agate mortar, and then ground into uniform powder with a high-speed grinder, and passed through a 100-mesh sieve to prepare the original electrolytic manganese slag powder; Step 2, mixing the original electrolytic manganese slag powder obtained in the previous step with deionized water, and stirring on a magnetic stirrer to obtain a uniformly mixed electrolytic manganese slag suspension; Step 3, adding calcium oxide to the above-mentioned uniformly mixed electrolytic manganese slag suspension, and continuing to stir the reaction with a magnetic stirrer to obtain a fully reacted mixed solution; Step 4: Filter the mixed solution obtained above and rinse it with deionized water until the solution is neutral, and dry the obtained solid in a drying oven at 75°C; Step 5: Grind the dried solid with an agate mortar and pass it through a 100-mesh sieve to prepare a modified electrolytic manganese slag catalyst.

2. The method for preparing a catalyst for activating persulfate by modified manganese slag according to claim 1, characterized in that: In step 1, the electrolytic manganese slag sample is dried in an oven at 60-85° C. for 24-72 hours to remove the remaining moisture in the electrolytic manganese slag and then ground into small pieces using an agate mortar.

3. The method for preparing a catalyst for activating persulfate by modified manganese slag according to claim 1, characterized in that: In step 2, the solid-liquid ratio (kg: L) of the original electrolytic manganese slag powder and deionized water is 0.1 to 0.5; the stirring time of the electrolytic manganese slag suspension is 0.25 to 12 hours.

4. The method for preparing a catalyst for activating persulfate by modified manganese slag according to claim 1, characterized in that: In step 3, the addition ratio of calcium oxide to original electrolytic manganese slag powder (kg:kg) is 0.1-0.6; the stirring reaction time is 0.25-12h.

5. A modified electrolytic manganese slag catalyst prepared by the preparation method according to any one of claims 1 to 4.

6. Use of the modified electrolytic manganese slag catalyst as claimed in claim 5 in a persulfate activation system for degrading organic dyes or antibiotic wastewater in water.

7. The use of the modified electrolytic manganese slag catalyst in a persulfate activation system according to claim 6, characterized in that: Specifically, persulfate is added to water containing acid orange azo dyes to obtain a mixed solution, and then a modified electrolytic manganese slag catalyst is added, and a magnetic stirrer is used to mix and stir the reaction for 2 to 3 hours to complete the degradation of the azo dyes in the water.

8. The use of the modified electrolytic manganese slag catalyst in a persulfate activation system according to claim 7, characterized in that: In the water body containing acid orange azo dyes, the added amount of the persulfate is 0.5-2 mmol / L; the added amount of the modified electrolytic manganese slag catalyst is 0.25-2.00 g / L.

9. The use of the modified electrolytic manganese slag catalyst in a persulfate activation system according to claim 8, characterized in that: The concentration of acid orange in the water containing the acid orange azo dye is 10-100 mg / L.

10. The use of the modified electrolytic manganese slag catalyst in a persulfate activation system according to claim 6, characterized in that: The pH value of the organic dye or antibiotic wastewater ranges from 3 to 11; during the degradation reaction, the degradation reaction temperature is 5 to 40° C., and the degradation reaction time is 5 to 30 min.

Citation Information

Patent Citations

  • Method for treating sulfite-containing wastewater

    CN102030436A

  • Method for treating organic wastewater difficult to degrade by preparing ozone catalyst through modifying carrier

    CN105540819A

  • Manganese dioxide and sulfite system and preparation method and application thereof

    CN109336212A

  • Application of modified manganese sand to catalysis of degradation of organic wastewater by hydrogen peroxide

    CN109759079A