Preparation method and application of bimetallic catalyst based on membrane pore confinement
The bimetallic catalyst is prepared by carrying out a redox reaction in the membrane pores, which solves the problems of easy shedding of the catalyst and complicated process, achieves the effect of efficient degradation of micro-pollutants, simplifies the process and reduces the cost.
Patent Information
- Application Number
- CN202410755859.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
AI Technical Summary
Existing catalytic membrane preparation methods have problems such as easy shedding of catalysts, uneven distribution, complex processes, high energy consumption and high cost. In particular, the degradation efficiency of micro-pollutants is not high in water treatment.
By controlling the concentration ratio of the reducing agent and the oxidizing agent in the membrane pores, diffusion and infiltration under normal pressure are carried out to carry out the redox reaction, and the bimetallic catalyst is prepared, avoiding high-temperature calcination, simplifying the process and improving the stability and activity of the catalyst.
The catalyst achieves high-efficiency degradation of micro-pollutants, with a degradation rate of more than 90%. The process is simple and low-cost, making it suitable for industrial production.
Smart Images

Figure CN118767940A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of membrane catalysis in water treatment, and in particular to a preparation method and application of a bimetallic catalyst based on membrane pore confinement. Background Art
[0003] The membrane provides a fixed place for the growth and catalytic oxidation of the catalyst, and the unique pore structure of the membrane pores reduces the agglomeration of the catalyst to a certain extent. The membrane, as a carrier of the catalyst, does not require a cumbersome catalyst separation / recovery process. More importantly, the diversified structure of the membrane pores provides a rich loading place and reaction site for the catalyst, thereby further accelerating the degradation process of pollutants. At present, the preparation of catalytic membranes is mainly to introduce catalysts into the membrane by means of surface loading, blending and in-situ reaction. The catalyst loaded on the membrane surface is generally filtered by vacuum filtration to the surface of the base membrane to form a catalytic layer. The catalytic membrane prepared by this method has the disadvantages of easy falling off, leakage and uneven distribution of the catalyst. The blending method mainly involves uniformly mixing the catalyst into the precursor solution of the organic membrane material, and then fixing the catalyst in the membrane or on the membrane surface by surface coating or immersion phase conversion method. Patent CN112121648A discloses a method for preparing a casting solution by blending a nanocatalyst and PVDF, and then preparing a polyvinylidene fluoride mixed matrix membrane by a phase separation method. However, the catalytic membrane prepared by the blending method has the disadvantages of uneven catalyst distribution, easy clogging of active sites and limited catalytic activity. The in-situ growth method filters or coats the precursor solution to fill the membrane pores with the reaction solution, and then performs multiple injections or high-temperature calcination and other post-treatments to make the catalyst grow in situ in the membrane. The preparation process is generally more complicated, often requiring long-term high temperatures, high energy consumption, and consumption of multiple organic solvents, and the cost is high. Patent CN105597558 discloses a catalytic nanofiltration membrane prepared by in-situ growth of a single metal oxide. The degradation rate of the catalytic nanofiltration membrane for pollutants can reach more than 80%. Its preparation process uses multiple injections of reaction reagents to prepare the catalyst, which takes a long time and has a complex reaction process.
[0004] The present invention aims at the deficiencies of the current technology, uses membrane pores as reactors, and controls the concentration ratio of reducing agent and oxidizing agent to diffuse and penetrate into the membrane pores at normal pressure respectively, and then prepares a bimetallic catalyst through redox reaction. The preparation method of the catalyst is simple and easy, does not require high-temperature calcination, has strong operability, is easy to industrialize, and the prepared catalyst has a high degradation efficiency for micropollutants in water bodies. Summary of the invention
[0005] The present invention provides a method for preparing a bimetallic catalyst under membrane pore confinement conditions, which is easy to operate, simple in process, and does not require special equipment, instruments, and operating means. The developed catalyst does not contain any precious metals, has low cost, is environmentally friendly, has no secondary pollution, has high catalytic activity, and has strong stability. It is applied to the treatment of micro-polluted water bodies, has a strong ability to degrade pollutants, and is easy to promote and apply.
[0006] 1. A method for preparing a bimetallic catalyst based on pore confinement, characterized in that it comprises the steps of:
[0007] (1) preparing a reducing agent solution A and an oxidizing agent solution B of a certain concentration, wherein the concentrations of the two solutions are controlled to be 0.05 mol / L to 1.0 mol / L, wherein the molar concentration ratio of solution A to solution B is 1:1 to 10:1;
[0008] (2) pre-treating the porous membrane by first soaking it in a 95% ethanol solution for 30 min, and then rinsing and soaking it in deionized water;
[0009] (3) The pretreated porous membrane is first immersed in solution A, and solution A is diffused and infiltrated into the membrane pores by oscillating in a constant temperature water bath for 60 minutes. Then the membrane is taken out and the membrane surface is rinsed with deionized water to remove the residual solution A on the membrane surface. Then the membrane is immersed in solution B, and the reaction temperature of solution B is controlled at 60-90°C for 2-12 hours. Then the prepared catalytic membrane is cooled to room temperature and stored in deionized water.
[0010] Preferably, in step (1), the reducing metal salt solution mainly comprises: Fe 2+ 、Co 2+ , Mn 2+ and Ce 3+ Metal salt solutions such as potassium permanganate and potassium ferrate.
[0011] The pore size of the porous membrane in step (2) ranges from 0.01 μm to 10 μm, with a preferred range of 0.01 μm to 1 μm. The porous membrane material mainly refers to polymer ultrafiltration / microfiltration membranes such as polyvinylidene fluoride, polyethersulfone, polypropylene, polyacrylonitrile, and inorganic ceramic ultrafiltration / microfiltration membrane materials, and the membrane pores are preferably honeycomb pores and sponge pores.
[0012] The two solutions participating in the redox reaction in step (3) refer to one of the reducing agent solutions and one of the oxidizing agent solutions capable of generating a bimetallic catalyst in claim 2.
[0013] In order to improve the reaction efficiency of the catalyst in step (3), ultrasound can be used to assist the diffusion of the solution.
[0014] In the present invention, the reducing agent solution first diffuses and fills the membrane pores, and then the oxidant begins to diffuse. During the diffusion process, the reducing agent contacts the membrane pores and undergoes a redox reaction to form a preliminary catalyst nucleus, which is then matured and grown by controlling the hydrothermal conditions. Due to the effect of spatial confinement, the grown catalyst is basically round particles and anchored in the membrane pores.
[0015] The bimetallic catalyst prepared by the present invention can be used in advanced oxidation water treatment technology to activate persulfate (PMS) to degrade micropollutants in water, and in the presence of low concentrations of PMS, it has a high degradation effect on most pollutants, with a degradation rate of more than 90%. The degradable micropollutants mainly include phenols, dyes, antibiotics and other pollutants in water.
[0016] Compared with the prior art, the present invention has the advantages of:
[0017] (1) The catalyst preparation reaction process of the present invention does not require complicated processes and reagents, and the process is simple and easy. The oxidant undergoes a redox reaction with the reductant during the diffusion process, and bimetallic catalyst particles are generated in the membrane pore confinement environment.
[0018] (2) The catalytic membrane prepared by the present invention has both filtering and catalytic functions. The catalyst in the membrane is confined to the nanoscale space, which can effectively improve the selectivity and activity of the catalyst, increase the contact probability of the generated free radicals with the pollutants, and enhance the catalytic degradation rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] FIG1 is a cross-sectional SEM image of the original PVDF membrane and the iron-manganese bimetallic PVDF catalyst membrane in Example 1 (the particles in the circle are the synthesized catalyst);
[0021] Figure 2 The comparison of the catalytic degradation effects of different target pollutants by the iron-manganese bimetallic PVDF catalytic membrane in Example 1 (operating conditions: [RhB] = [AO7] = [BPA] = [SMX] = 20 μM, pH = 3.6, PMS = 0.5 mM); DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0025] The characterization methods used in the following embodiments mainly include:
[0026] The cross-sectional morphology of the membrane was measured by scanning electron microscopy (SEM, Germany, ZEISS Sigma 300).
[0027] The present invention uses membrane catalyst to catalyze and degrade dye pollutants in water: rhodamine B (RhB), orange yellow G (AO7), phenolic substances: bisphenol A (BPA) and antibiotics: sulfamethoxazole (SMX) to prove its application effect. The specific experimental process is as follows: under room temperature, the prepared catalytic membrane is placed in a circulating filtration device, 20 μM of target pollutants and 0.5 mM of PMS are added to the feed liquid, and the pH value of the feed liquid is adjusted with sulfuric acid (H2SO4) and sodium hydroxide (NaOH). After adjusting to an appropriate pH, a peristaltic pump is turned on to circulate the solution through the membrane at a pressure of 0.1 MPa, and then the permeate flows back to the feed liquid to keep the volume constant. 3 mL of the solution is taken out regularly, and quenched with 10 mM of disodium ethylenediaminetetraacetic acid (EDTA) at the same time, and detected and analyzed at a wavelength of 554 nm (RhB) or 484 nm (AO7) using an ultraviolet spectrophotometer (T6 type, Beijing Puxi Company). BPA and SMX were detected using a Tianmei liquid chromatograph equipped with a Diamonsil C18 analytical column.
[0028] The pollutant removal rate is calculated by the following formula:
[0029]
[0030] Where C (mol / L) and C0 (mol / L) are the final concentration and initial concentration of the pollutant, respectively.
[0031] The raw materials and reagents used in the following examples and comparative examples are all commercially available products.
[0032] Example 1
[0033] Using polyvinylidene fluoride PVDF membrane (pore size 0.22μm) as the membrane support, the PVDF membrane was first soaked in 95% ethanol solution for 30min to remove impurities, and then rinsed and soaked with deionized water to replace the ethanol solution in the membrane pores. Then two metal reaction solutions were prepared, in which the metal ion salt solution with reduction reaction was ferrous sulfate heptahydrate solution (0.3mM), and the oxidant solution with oxidation effect was potassium permanganate solution (0.1mM), and the ratio was controlled to be 3:1. Then the PVDF membrane was soaked in 30ml ferrous sulfate heptahydrate solution for 1h, and the ferrous ions were allowed to penetrate into the membrane pores by free diffusion through constant temperature water bath oscillation. When the membrane was saturated, the membrane was taken out, the membrane surface was rinsed with deionized water several times, and then soaked in 30ml potassium permanganate solution, and the reaction temperature of the potassium permanganate solution was increased. The hydrothermal reaction was carried out at 75℃ for 4h, and the iron-manganese bimetallic catalyst was embedded in situ through the redox reaction of potassium permanganate and ferrous sulfate metal salt. Finally, the hydrothermal membrane was left to cool, taken out and rinsed several times with deionized water, and finally stored in deionized water for subsequent testing.
[0034] Finally, the cross-sectional SEM images of the original PVDF membrane and the iron-manganese bimetallic PVDF catalytic membrane are shown in Figure 1. Scanning electron microscopy (SEM) shows that compared with the original PVDF membrane (Figure 1(a)), the iron-manganese bimetallic PVDF catalytic membrane (Figure 1(b)) has obvious spherical catalysts, which proves the successful preparation of the iron-manganese bimetallic catalyst and the feasibility of the method. With 20μM RhB, AO7, BPA and SMX as the target pollutants, under the condition of adding a small amount of PMS (0.5mM), the effect is as follows Figure 2 As shown, the membrane catalyst can achieve efficient purification of RhB, AO7 and BPA within 25 minutes, with removal rates greater than 90%, and a degradation rate of SMX of 40%, indicating that the bimetallic catalyst has efficient degradation effect and special selectivity.
[0035] Example 2
[0036] Compared with Example 1, this example replaces the heptahydrate ferrous sulfate solution with a hexahydrate cobalt nitrate solution, replaces the catalyst support material with a polyacrylonitrile PAN membrane (pore size 0.01 μm), and uses an ultrasonic assisted diffusion reaction. Other reaction conditions and steps remain unchanged, and finally a catalytic membrane of a cobalt-manganese bimetallic catalyst is obtained. Taking 20 μM RhB as the target pollutant, under the condition of adding a small amount of PMS (0.5 mM), the effect can be seen from Table 1 that the removal rate of RhB can reach 93.8% within 25 minutes.
[0037] Example 3
[0038] Using polyethersulfone PES membrane (pore size 1 μm) as the membrane support, the PES membrane was first soaked in 95% ethanol solution for 30 minutes to remove impurities, and then rinsed and soaked with deionized water to replace the ethanol solution in the membrane pores. Then two metal reaction solutions were prepared, in which the metal ion salt solution with a reducing reaction was manganese chloride tetrahydrate (0.1 mM), and the oxidant solution with an oxidizing effect was potassium ferrate solution (0.1 mM), and the ratio was controlled to be 1:1. PES was first soaked in 30ml of tetrahydrate manganese chloride solution for 1h, and then oscillated in a constant temperature water bath to allow manganese ions to penetrate into the membrane pores through free diffusion. When the membrane was saturated, the membrane was taken out, and the membrane surface was washed several times with deionized water. Then it was soaked in 30ml of potassium ferrate solution, and the reaction temperature of the potassium ferrate solution was increased. The hydrothermal reaction was carried out at 80℃ for 4h. The manganese-iron bimetallic catalyst was embedded in situ through the redox reaction of potassium ferrate and manganese chloride metal salt. Finally, the hydrothermal membrane was left to cool, taken out and rinsed with deionized water several times, and finally stored in deionized water. With 20μM RhB as the target pollutant, its catalytic performance was tested under the condition of adding a small amount of PMS (0.5mM). The effect can be seen from Table 1 that the removal rate of RhB can reach 78.7% within 25min.
[0039] Example 4
[0040] A ceramic ultrafiltration membrane (composition = ZrO2 and TiO2; thickness = 2.5 mm; diameter = 4.7 cm; pore size 0.10 μm) was used as the membrane support. The ceramic membrane was first ultrasonically cleaned with ethanol and deionized water for 30 minutes, and then rinsed and soaked with deionized water. Then two metal reaction solutions were prepared, in which the metal ion salt solution with a reducing reaction was cerium nitrate hexahydrate (0.4 mM), and the oxidant solution with an oxidizing effect was potassium permanganate solution (0.1 mM), and the ratio was controlled to be 4:1. The ceramic ultrafiltration membrane was first soaked in 100ml of hexahydrate cerium nitrate solution for 1h, and ultrasonic assisted diffusion reaction was used to make cerium ions penetrate into the membrane pores through ultrasonic diffusion. When the membrane was saturated, the membrane was taken out, the membrane surface was washed several times with deionized water, and then it was soaked in 100ml of potassium permanganate solution, and the reaction temperature of the potassium permanganate solution was increased. The hydrothermal reaction was carried out at 90℃ for 12h, and the cerium-manganese bimetallic catalyst was embedded in situ through the redox reaction of potassium permanganate and cerium nitrate metal salt. Finally, the hydrothermal membrane was allowed to stand and cool to room temperature, taken out and rinsed with deionized water several times, and placed in a vacuum oven to dry before use. Taking 20μM RhB as the target pollutant, under the condition of adding a small amount of PMS (0.5mM), the effect can be seen from Table 1 that the removal rate of RhB can reach 95.5% within 25min.
[0041] Comparative Example 1
[0042] Compared with Example 1, the concentration of ferrous sulfate heptahydrate solution was increased to 1M, and the concentration ratio of ferrous sulfate heptahydrate solution to potassium permanganate solution was adjusted to 10:1, and other reaction conditions and steps remained unchanged, as a comparison. Taking 20 μM RhB as the target pollutant, under the condition of adding a small amount of PMS (0.5 mM), the effect can be seen from Table 1 that the removal rate of RhB can reach 97.2% within 25 minutes.
[0043] Comparative Example 2
[0044] Compared with Example 1, this example reduces the concentration of potassium permanganate solution to 0.05M, and adjusts the concentration ratio of potassium permanganate solution to 6:1, and other reaction conditions and steps remain unchanged, as a comparison. Taking 20μM RhB as the target pollutant, under the condition of adding a small amount of PMS (0.5mM), the effect can be seen from Table 1 that the removal rate of RhB can reach 82.7% within 25min.
[0045] Comparative Example 3
[0046] Compared with Example 1, the hydrothermal temperature was raised to 90°C, the hydrothermal time was extended to 12h, and the other reaction conditions and steps were kept unchanged for comparison. Taking 20μM RhB as the target pollutant, under the condition of adding a small amount of PMS (0.5mM), the effect can be seen from Table 1 that the removal rate of RhB can reach 95.6% within 25min.
[0047] Comparative Example 4
[0048] Compared with Example 1, the hydrothermal temperature in this example was reduced to 60°C, the hydrothermal time was shortened to 2h, and the other reaction conditions and steps remained unchanged, for comparison. Taking 20μM RhB as the target pollutant, under the condition of adding a small amount of PMS (0.5mM), the effect can be seen from Table 1 that the removal rate of RhB within 25min is 65.3%.
[0049] Comparative Example 5
[0050] Compared with Example 1, the pore size of the polyvinylidene fluoride PVDF membrane supporting the catalyst was changed from 0.22 μm to 0.10 μm, and the other reaction conditions and steps remained unchanged for comparison. Taking 20 μM RhB as the target pollutant, under the condition of adding a small amount of PMS (0.5 mM), the effect can be seen from Table 1 that the removal rate of RhB can reach 94.8% within 25 minutes.
[0051] Comparative Example 6
[0052] Compared with Example 1, the supporting material of the catalyst generation, polyvinylidene fluoride PVDF membrane (pore size 0.22 μm), was changed to polypropylene PP membrane (pore size 0.22 μm), and other reaction conditions and steps remained unchanged, for comparison. Taking 20 μM RhB as the target pollutant, under the condition of adding a small amount of PMS (0.5 mM), the effect can be seen from Table 1 that the removal rate of RhB can reach 92.7% within 25 minutes.
[0053] Table 1 is a comparison table of the degradation of dye RhB by different membrane catalysts in Examples 1-4 and Comparative Examples 1-6 (operating conditions: [RhB] = 20 μM, pH = 3.6, PMS = 0.5 mM);
[0054] Table 1
[0055] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.
Claims
1. A method for preparing a bimetallic catalyst based on membrane pore confinement, characterized in that: Includes steps: (1) preparing a reducing agent solution A and an oxidizing agent solution B of a certain concentration, wherein the concentrations of the two solutions are controlled to be 0.05 mol / L to 1.0 mol / L, wherein the molar concentration ratio of solution A to solution B is 1:1 to 10:1; (2) pre-treating the porous membrane by first soaking it in a 95% ethanol solution for 30 min, and then rinsing and soaking it in deionized water; (3) The pretreated porous membrane is first immersed in solution A, and solution A is diffused and infiltrated into the membrane pores by oscillating in a constant temperature water bath for 60 minutes. Then the membrane is taken out and the membrane surface is rinsed with deionized water to remove the residual solution A on the membrane surface. Then the membrane is immersed in solution B, and the reaction temperature of solution B is controlled at 60-90°C for 2-12 hours. Then the prepared catalytic membrane is cooled to room temperature and stored in deionized water.
2. The preparation method according to claim 1, characterized in that: The reducing metal salt solution in step (1) mainly includes: Fe 2+ 、Co 2+ , Mn 2+ and Ce 3+ Metal salt solutions such as potassium permanganate and potassium ferrate.
3. The preparation method according to claim 1, characterized in that: The pore size of the porous membrane in step (2) ranges from 0.01 μm to 10 μm, with a preferred range of 0.01 μm to 1 μm. The porous membrane material mainly refers to polymer ultrafiltration / microfiltration membranes such as polyvinylidene fluoride, polyethersulfone, polypropylene, polyacrylonitrile, and inorganic ceramic ultrafiltration / microfiltration membrane materials, and the membrane pores are preferably honeycomb pores and sponge pores.
4. The preparation method according to claim 1, characterized in that: The two solutions participating in the redox reaction in step (3) refer to one of the reducing agent solutions and one of the oxidizing agent solutions capable of generating a bimetallic catalyst in claim 2.
5. The preparation method according to claim 1, characterized in that: In order to improve the reaction efficiency of the catalyst in step (3), ultrasound can be used to assist the diffusion of the solution.
6. The bimetallic catalyst prepared by the preparation method according to claim 1 can be used in advanced oxidation water treatment technology to activate persulfate (PMS) to degrade micropollutants in water, and in the presence of low concentration of PMS, it has a high degradation effect on most pollutants, and the degradation rate can reach more than 90%.
7. The degradable micropollutants according to claim 6 mainly include pollutants such as phenols, dyes and antibiotics in water.
Citation Information
Patent Citations
Method for modifying water treatment inorganic catalytic membrane
CN103495345A
Non-stoichiometric iron-manganese oxide heterogeneous Fenton-like catalyst and preparation method and application thereof
CN111054380A
Preparation method and application of ferromanganese layered bimetal hydroxide catalyst
CN111215091A
Method for synchronously adsorbing, degrading and removing arsanilic acid in water by activating persulfate with cerium-manganese bimetallic catalyst
CN113880220A