Preparation method and application of cobaltosic oxide loaded noble metal catalyst
By preparing Co3O4 supported precious metal catalysts and using alkaline precipitation and high-temperature calcination technology, the problem of insufficient performance of existing catalysts has been solved, and efficient catalytic oxidation of gaseous carbon-containing compounds has been achieved, especially at low temperatures to achieve high conversion rates and maintain stability.
Patent Information
- Application Number
- CN202310375421.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-04-10
AI Technical Summary
Existing catalysts have poor performance in catalytically oxidizing gaseous carbon-containing compounds. In particular, cobalt tetroxide has insufficient performance compared with precious metal catalysts, making it difficult to effectively degrade gaseous pollutants such as volatile organic compounds and methane.
By preparing Co3O4 loaded precious metal catalyst, alkaline reagent precipitation, solvothermal reaction and high temperature calcination methods are used to control the morphology and crystal structure of the carrier, combined with the H2O2 redox reaction, to drive the deposition of precious metals on the surface of the carrier to form a highly active and stable form. catalyst.
The catalytic oxidation performance is significantly improved. The precious metal catalyst supported by Co3O4 can achieve 100% methane conversion rate at low temperatures and maintain good stability at high temperatures, which is better than catalysts with high carrier crystallization.
Smart Images

Figure CN118767941A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of catalytic materials for oxidation and decomposition of gaseous carbon-containing compounds, and in particular relates to a preparation method of a cobalt tetraoxide-loaded noble metal catalyst and its application in catalytic oxidation of gaseous carbon-containing compounds. Background Art
[0002] Problems such as ozone pollution, greenhouse effect and indoor air pollution caused by gaseous pollutants such as VOCs (volatile organic compounds) and CH4 have gradually become prominent and gradually replaced the original air pollution problems, attracting widespread attention.
[0003] In addition to affecting the atmospheric environment, most VOCs also have serious biological toxicity. Long-term exposure to an environment polluted by VOCs is extremely harmful to the human body. For example, benzene compounds, which are widely used in industrial production processes, have long been certified as a Class I carcinogen by the International Agency for Research on Cancer (IARC) under the World Health Organization (WHO).
[0004] Methane is the most promising clean energy alternative and also a potential greenhouse gas. Compared with the greenhouse gas carbon dioxide (CO2) we are familiar with, the same amount of methane absorbs more infrared radiation than CO2, and its greenhouse effect is about 30 times that of CO2. The long-term accumulation of CH4 directly causes 16% of the greenhouse effect.
[0005] Strengthening the coordinated control of the above-mentioned gaseous pollution is the key to promoting the continuous improvement of my country's ambient air quality. Compared with other gaseous pollutant control technologies, catalytic oxidation technology can oxidize and decompose gaseous carbon-containing compounds such as CH4 and VOCs into CO2 and H2O at relatively low temperatures (200-600℃). It is considered to be one of the most effective technologies for solving air pollution problems, and therefore has received widespread attention and application.
[0006] As we all know, catalysts are the core materials of catalytic oxidation technology and play a key role in the catalytic oxidation degradation of gaseous pollutants. As an important industrial material, cobalt tetroxide (Co3O4) has a wide range of applications in energy storage, metallurgy and catalysis. + , 3 +Mainly) is conducive to its important role in the activation of gas-phase O2 and the breakage of organic compound CH, so it has a good catalytic oxidation function for the degradation of gaseous carbon-containing compounds. Although cobalt tetroxide has a wide range of applications in the catalytic oxidation degradation of gaseous carbon-containing compounds, its performance is slightly inferior to that of precious metal catalysts. In recent years, the research and development of precious metal catalysts based on cobalt oxide and their application in the field of environmental catalysis have continued to grow, which has made up for the shortcomings of related research to a certain extent. Summary of the invention
[0007] In order to improve the deficiencies of the prior art, the present invention provides a method for preparing a Co3O4-loaded noble metal catalyst and its application, wherein the catalyst has good catalytic activity and stability.
[0008] In a first aspect, the present invention provides a method for preparing a Co3O4-supported noble metal catalyst for catalytic oxidation of gaseous carbon-containing compounds, the preparation method comprising the following steps:
[0009] S1. dissolving a soluble cobalt salt in water, mixing and reacting with an alkaline reagent to obtain a cobalt salt precipitate;
[0010] S2. calcining the cobalt salt precipitate to obtain a carrier Co3O4;
[0011] S3. The carrier Co3O4 and the soluble salt corresponding to the precious metal M are dissolved in a solvent and mixed, H2O2 is added to react and calcine to obtain M / Co3O4.
[0012] According to an embodiment of the present invention, the mixing of the soluble cobalt salt aqueous solution and the alkaline reagent in step S1 comprises the following steps: adding the alkaline reagent to the soluble cobalt salt aqueous solution, stirring at room temperature for 0.1 to 1 hour to obtain a mixed solvent, for example, stirring for 0.5 hour.
[0013] According to an embodiment of the present invention, the alkaline agent is an aqueous solution of an alkaline substance.
[0014] According to an embodiment of the present invention, the concentration of the alkaline agent is 1 to 3 times the concentration of the soluble cobalt salt aqueous solution.
[0015] According to an embodiment of the present invention, the reaction in step S1 is a solvent thermal reaction, and the solvent thermal reaction comprises the following steps: reacting the mixed solvent at a temperature of 100 to 200° C. for 4 to 24 hours.
[0016] Preferably, the temperature of the solvent thermal reaction is 120-180° C., and the reaction time is 8-20 hours.
[0017] According to an embodiment of the present invention, the calcination temperature in step S2 is 300-800° C., and the calcination time is 2-12 hours. Preferably, the calcination temperature is 400-600° C., and the calcination time is 5-8 hours.
[0018] According to an embodiment of the present invention, the carrier Co3O4 has an amorphous structure or a crystalline structure.
[0019] As an example, the calcination temperature is 400° C., the calcination time is 4 hours, the carrier Co3O4 is a sheet-like amorphous structure, and the size of the nanosheet is 50 to 500 nm.
[0020] As another example, the calcination temperature is 650° C., the calcination time is 4 h, the carrier Co 3 O 4 is a granular nanocrystalline structure, and the size of the nanoparticles is 100 to 250 nm.
[0021] According to an embodiment of the present invention, in step S2, the microstructure and crystallization degree of the carrier Co3O4 are regulated by the calcination temperature. When the calcination temperature increases, the crystallization degree of the carrier Co3O4 crystals increases, the size of the carrier Co3O4 crystals increases, the pores decrease, and the interaction with the precious metal M weakens.
[0022] According to an embodiment of the present invention, after step S1 and before step S2, the following steps are further included: filtering, washing and drying the cobalt salt precipitate.
[0023] According to an embodiment of the present invention, the washing comprises water washing and / or ethanol washing, for example, water washing and ethanol washing are used in sequence.
[0024] According to an embodiment of the present invention, the drying comprises the following steps: drying the washed cobalt salt precipitate at a temperature of 50 to 100° C. for 10 to 20 hours, for example, drying at a temperature of 80° C. for 12 hours.
[0025] According to an embodiment of the present invention, the soluble cobalt salt is selected from at least one of Co(NO3)2, CoCl2 and Co(CH3COO)2.
[0026] According to an embodiment of the present invention, the alkaline substance is selected from at least one of NaOH, Na2CO3, and NaHCO3.
[0027] According to an embodiment of the present invention, the mixing of the carrier Co3O4 and the soluble precious metal salt dissolved in a solvent in step S3 includes the following steps: dispersing the carrier Co3O4 in a solvent, adding a soluble salt of the precious metal M, and stirring at room temperature for 0.1 to 1 hour to obtain a mixed solution.
[0028] According to an embodiment of the present invention, the noble metal M is selected from at least one of Pd, Pt, Au and Ru, for example, Pd.
[0029] According to an embodiment of the present invention, the loading amount of the precious metal is 0.1-5% of the carrier Co3O4 by mass, and preferably the loading amount of the precious metal is 1-3% of the carrier Co3O4.
[0030] According to an embodiment of the present invention, the reaction of the mixed solution with the redox reaction driven hydrolysis precipitant comprises the following steps: heating the mixed solution to 20-100° C., adding the redox reaction driven hydrolysis precipitant H2O2 to react for 2-10 hours to obtain a solid reactant.
[0031] According to an embodiment of the present invention, the concentration of H2O2 in the aqueous solution of H2O2 is 20-30%, for example, 30%.
[0032] According to an embodiment of the present invention, the amount of H2O2 is more than 50 times that of the precious metal in terms of amount of substance.
[0033] According to an embodiment of the present invention, the calcination in step S3 comprises the following steps: calcining the solid reactant at a temperature of 200 to 400° C. for 2 to 12 hours, for example, calcining at a temperature of 400° C. for 4 hours.
[0034] According to an embodiment of the present invention, after the solid reactant is obtained by reaction in step S3 and before calcination, the following steps are further included: filtering the reaction solution, washing and drying the solid reactant.
[0035] According to an embodiment of the present invention, the washing comprises water washing and / or ethanol washing, for example, water washing and ethanol washing are used in sequence.
[0036] According to an embodiment of the present invention, the drying comprises the following steps: drying the washed solid reactant at a temperature of 50 to 100° C. for 10 to 20 hours, for example, drying at a temperature of 80° C. for 12 hours.
[0037] According to an embodiment of the present invention, a catalyst having a Co3O4 carrier with a lower degree of crystallization has a better activity in catalytic degradation of gaseous carbon-containing compounds than a catalyst having a carrier with a higher degree of crystallization.
[0038] According to an embodiment of the present invention, the catalyst with a lower degree of crystallization of the Co3O4 support has a worse high temperature stability.
[0039] According to an embodiment of the present invention, after Co3O4 is loaded with precious metals, the activity of catalytic oxidation of gaseous carbon-containing compounds is significantly improved. At the same time, the precious metal loading can be used to suppress the crystallization of the carrier under high temperature conditions to a certain extent.
[0040] According to an embodiment of the present invention, the Co3O 4(400C) 、Co3O 4(650C) 、3%Pd / Co3O 4(400C) 、3%Pd / Co3O 4(650C) With basic Figure 1 TEM image shown.
[0041] According to an embodiment of the present invention, the Co3O 4(400C) 、Co3O 4(650C) 、3%Pd / Co3O 4(400C) 、3%Pd / Co3O 4(650C) With basic Figure 2 XRD pattern shown.
[0042] According to an embodiment of the present invention, the Co3O 4(400C) 、Co3O 4(650C) 、3%Pd / Co3O 4(400C) 、3%Pd / Co3O 4(650C) With basic Figure 3 BET diagram shown.
[0043] According to an embodiment of the present invention, the Co3O 4(400C) 、Co3O 4(650C) 、3%Pd / Co3O 4(400C) 、3%Pd / Co3O 4(650C) With basic Figure 4 The methane conversion test graph is shown.
[0044] According to an embodiment of the present invention, the Co3O 4(400C) 、Co3O 4(650C) 、3%Pd / Co3O 4(400C) 、3%Pd / Co3O 4(650C) With basic Figure 5 The methane conversion stability test graph is shown.
[0045] According to an embodiment of the present invention, Co3O 4(400c) At 500 °C and 3% Pd / Co3O 4(400C) The catalytic oxidation of methane at 600℃ for 24h has the following characteristics: Figure 6 XRD pattern shown.
[0046] According to an embodiment of the present invention, the Co3O 4(400C) 、Co3O 4(650C) 、3%Pd / Co3O 4(400C) 、3%Pd / Co3O 4(650C) With basic Figure 4Toluene conversion test graph shown.
[0047] In a second aspect, the present invention provides a Co3O4-loaded precious metal catalyst prepared by the above method, wherein the catalyst has an amorphous structure or a crystalline structure, wherein the precious metal content of the catalyst is 0.1 to 5% of the carrier Co3O4, and the precious metal M is at least one of Pd, Pt, Au, and Ru.
[0048] According to an embodiment of the present invention, the catalyst is a nanostructure, such as a nanosheet, nanorod, nanoparticle or nanocluster structure.
[0049] According to an embodiment of the present invention, the specific surface area of the catalyst is greater than 5m 2 / g, preferably the specific surface area of the catalyst is greater than 6m 2 / g.
[0050] In a third aspect, the present invention further provides an application of the above-mentioned Co3O4-loaded precious metal catalyst in catalytic oxidation of gaseous carbon-containing compounds, wherein the gaseous carbon-containing compounds are, for example, VOCs or methane.
[0051] Beneficial Effects
[0052] (1) The preparation method of the present invention prepares a Co3O4 carrier by alkali precipitation, solvent thermal reaction and high-temperature calcination. During the reaction, the ratio of raw materials, reaction temperature and / or time are controlled to control the synthesis of carrier Co3O4 with different morphologies and crystal structures. The catalytic function of the carrier Co3O4 drives the H2O2 redox reaction, thereby indirectly driving the deposition of precious metals on the surface of the carrier Co3O4. The Co3O4-loaded precious metal catalyst prepared by this method can be used for low-temperature catalytic oxidation of common gaseous carbon-containing compounds. The inventors unexpectedly found that compared with catalysts with a higher degree of carrier crystallization, catalysts with amorphous morphology or a lower degree of crystallization have more abundant active oxygen species, more defect structures and a larger specific surface area, and exhibit better catalytic oxidation performance after loading precious metals.
[0053] (2) The Co3O4-loaded noble metal catalyst prepared by the present invention can achieve a 100% conversion rate when catalyzing the methane reaction at a temperature below 340°C. At the same time, it has good stability at a temperature of 340°C and can be used as an efficient and stable catalyst to catalyze the oxidation of gaseous carbon-containing compounds. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 These are SEM test images of the catalysts prepared in Examples 1, 2, 3, and 4 of the present invention.
[0055] Figure 21 is the XRD diagram of the catalysts prepared in Examples 1, 2, 3 and 4 of the present invention.
[0056] Figure 3 It is the BET diagram of the catalysts prepared in Examples 1, 2, 3 and 4 of the present invention.
[0057] Figure 4 It is a graph showing the methane conversion activity test results of the catalysts prepared in Examples 1, 2, 3 and 4 of the present invention.
[0058] Figure 5 1 is a graph showing the stability test results of the methane conversion of the catalysts prepared in Examples 1, 2, 3 and 4 of the present invention.
[0059] Figure 6 The XRD diagrams of the catalysts prepared in Examples 1 and 3 of the present invention before and after the catalytic oxidation of methane at 500° C. and 600° C. for 24 hours are shown.
[0060] Figure 7 It is a graph showing the methane conversion activity test results of the catalysts prepared in Examples 1, 2, 3 and 4 of the present invention. DETAILED DESCRIPTION
[0061] The catalyst of the present invention and its preparation method and application will be described in further detail below in conjunction with specific examples. It should be understood that the following examples are only for exemplary description and explanation of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies realized based on the above content of the present invention are included in the scope of protection of the present invention.
[0062] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0063] Example 1 Catalyst Co3O 4(400C) Preparation:
[0064] (1) Weigh 23.2 g Co(NO3)2·6H2O and 6.4 g NaOH and dissolve them in 200 mL and 50 mL secondary water respectively;
[0065] (2) rapidly mixing the Co(NO3)2 aqueous solution and the NaOH aqueous solution, stirring and reacting for 0.5 h at room temperature to obtain a reaction solution;
[0066] (3) The reaction solution was transferred to a 500 mL high pressure reactor and subjected to a hydrothermal reaction at 180° C. for 12 h to obtain a hydrothermal reaction product;
[0067] (4) filtering the hydrothermal reaction product, washing it with water and then with ethanol, and drying it at 80° C. for 12 h to obtain a drying product;
[0068] (5) The dried product was calcined at 400 °C in air for 4 h to obtain a product named Co3O 4(400C) .
[0069] See also Figure 1 As can be seen from the upper left, the Co3O prepared in this example 4(400C) It has a flake structure and its size is about 50 to 500 nm. Figure 2 It can be seen that the Co3O prepared in this embodiment 4(400C) The diffraction peak intensity at the diffraction angle 2θ = 36.8° is 400. Figure 3 It can be seen that the Co3O prepared in this embodiment 4(400C) The specific surface area is 32.04m 2 / g.
[0070] Example 2 Catalyst Co3O 4(650C) Preparation:
[0071] (1) Weigh 23.2 g Co(NO3)2·6H2O and 6.4 g NaOH and dissolve them in 200 mL and 50 mL secondary water respectively;
[0072] (2) rapidly mixing the Co(NO3)2 aqueous solution and the NaOH aqueous solution, stirring and reacting for 0.5 h at room temperature to obtain a reaction solution;
[0073] (3) The reaction solution was transferred to a 500 mL high pressure reactor and subjected to a hydrothermal reaction at 180° C. for 12 h to obtain a hydrothermal reaction product;
[0074] (4) filtering the hydrothermal reaction product, washing it with water and then with ethanol, and drying it at 80° C. for 12 h to obtain a drying product;
[0075] (5) The dried product was calcined at 650°C for 4 h in an air atmosphere to obtain a product named Co3O 4(650C) .
[0076] See also Figure 1 As can be seen from the upper right, the Co3O prepared in this example 4(650C) It is a nanoparticle structure with a size of 100 to 250 nm, see Figure 2 It can be seen that the Co3O prepared in this embodiment 4(650C) The diffraction peak intensity at the diffraction angle 2θ = 36.8° is 1600. Figure 3 It can be seen that the Co3O prepared in this embodiment 4(650C) The specific surface area is 9.54m 2 / g.
[0077] Example 3 Catalyst 3% Pd / Co3O 4(400C) Preparation:
[0078] (1) 1.0 g of Co3O prepared in Example 1 was added 4(400C) The solid powder was ultrasonically dispersed in 100 mL of secondary water to obtain Co3O 4(400C) Aqueous solution;
[0079] (2) Co3O under stirring conditions 4(400C) 11.6 mL of H2PdCl4 (Pd concentration: 2.57 mg / mL) solution was added to the aqueous solution, and the mixture was stirred for 0.5 h at room temperature to obtain a mixed solution;
[0080] (3) The mixed solution prepared in step (2) was heated to 80°C, and 50 mL of an aqueous solution containing 4 mL of 30% H2O2 was added dropwise to the Co3O 4(400C) and H2PdCl4 in a mixed solution to obtain a reaction solution;
[0081] (4) stirring the reaction solution in step (3) at 80° C. for 4 h to obtain a reaction product;
[0082] (5) filtering the reaction product prepared in step (4), washing with water and ethanol in sequence, and drying at 80° C. for 12 h to obtain a drying product;
[0083] (6) The dried product of step (5) was calcined at 200°C for 2.0 h in an air atmosphere, and the calcined product was named 3% Pd / Co3O 4(400C) .
[0084] See also Figure 1 As can be seen from the lower left, the 3% Pd / Co3O prepared in this example 4(400C) It has a flake structure and its size is about 50-500nm. Figure 2 It can be seen that the 3% Pd / Co3O prepared in this example 4(400C) The diffraction peak intensity at the diffraction angle 2θ = 36.8° is 300. Figure 3 It can be seen that the 3% Pd / Co3O prepared in this example 4(400C) The specific surface area is 32.07m 2 / g.
[0085] Example 4 Catalyst 3% Pd / Co3O 4(650C) Preparation:
[0086] (1) 1.0 g of Co3O prepared in Example 2 was added 4(650C) The solid powder was ultrasonically dispersed in 100 mL of secondary water to obtain Co3O 4(650C) Aqueous solution;
[0087] (2) Co3O under stirring conditions 4(650C) 11.6 mL of H2PdCl4 (Pd concentration: 2.57 mg / mL) solution was added to the aqueous solution, and the mixture was stirred for 0.5 h at room temperature to obtain a mixed solution;
[0088] (3) The mixed solution prepared in step (2) was heated to 80°C, and 50 mL of an aqueous solution containing 4 mL of 30% H2O2 was added dropwise to the Co3O 4(650C) and H2PdCl4 in a mixed solution to obtain a reaction solution;
[0089] (4) stirring the reaction solution prepared in step (3) at 80° C. for 4 h to obtain a reaction product;
[0090] (5) filtering the reaction product prepared in step (4), washing with water and ethanol in sequence, and drying at 80° C. for 12 h to obtain a drying product;
[0091] (6) The dried product prepared in step (5) was calcined at 200°C for 2.0 h in an air atmosphere, and the calcined product was named 3% Pd / Co3O 4(650C) .
[0092] See also Figure 1 As can be seen from the lower right, the 3% Pd / Co3O prepared in this example 4(650C) It has a nanoparticle structure and its size is about 100-250nm. Figure 2 It can be seen that the 3% Pd / Co3O prepared in this example 4(650C) The diffraction peak intensity at the diffraction angle 2θ = 36.8° is 1500. Figure 3 It can be seen that the 3% Pd / Co3O prepared in this example 4(400C) The specific surface area is 6.86m 2 / g.
[0093] Test Case
[0094] Evaluation of the activity of catalysts in catalytic oxidation of gaseous carbon-containing compounds: methane and toluene CO were used as target pollutants to represent common gaseous carbon-containing compounds. The concentrations of methane and toluene were controlled to be 1% and 1000ppm respectively, and the catalytic reaction space velocity was controlled to be 20000-80000ml / (g·h). The catalytic oxidation performance of the catalyst was evaluated by increasing the temperature.
[0095] Test Example 1: Co3O prepared in Examples 1-4 4(400C) 、Co3O 4(650C) 、3%Pd / Co3O 4(400C) 、3%Pd / Co3O 4(650C)As a catalyst, the conversion rate of 1.0% CH4 was tested under the condition of GHSV = 40000 ml / (g·h). Figure 4 As shown, Co 3O4(400C) The temperature at which the conversion rate of CH4 in catalytic oxidation degradation reaches 90% (T 90 ) is 415℃, Co 3O4(650C) The temperature at which the conversion rate of CH4 in catalytic oxidation degradation reaches 90% (T 90 ) is 530℃, 3%Pd / Co 3O4(400C) The temperature at which the conversion rate of CH4 in catalytic oxidation degradation reaches 90% (T 90 ) is 335℃, 3% Pd / Co 3O4(650C) The temperature at which the conversion rate of CH4 in catalytic oxidation degradation reaches 90% (T 90 ) is 515℃.
[0096] Test Example 2: Co3O prepared in Examples 1-4 4(400C) 、Co3O 4(650C) 、3%Pd / Co3O 4(400C) 、3%Pd / Co3O 4(650C) As a catalyst, the stability of catalytic oxidation degradation of 1.0% CH4 was tested at different temperatures under the condition of reaction space velocity GHSV = 40000 ml / (g·h), see Figure 5 As shown, Co3O 4(400C) The catalytic performance at 500℃ gradually decreases with time, while Co3O 4(650C) The catalytic performance at 540 °C is stable over time, indicating that Co3O 4(650C) The stability at high temperature is significantly higher than that of Co3O 4(400C) , that is, Co3O4 with a higher degree of crystallization has a higher stability; 3% Pd / Co3O 4(400C) The stability at 340 °C is good, and the catalytic performance is also improved. The 3% Pd / Co3O 4(650C) The stability is higher at 500℃, and the catalytic performance is improved, but the improvement is significantly less than 3% Pd / Co3O 4(400C) ; It shows that Co3O4 synthesized at low temperature has better catalytic activity but poorer stability. However, after Co3O4 synthesized at low temperature is compounded with precious metals, the catalytic performance and stability are greatly improved, which is better than Co3O4 with a higher degree of crystallization synthesized at high temperature.
[0097] Test Example 3: Test the Co3O prepared in Example 1 and Example 3 4(400C) and 3%Pd / Co3O 4(400C)As a catalyst, the catalytic oxidation degradation reaction space velocity GHSV = 40000 ml / (g·h) at the reaction temperature of 500 and 600°C, the concentration of CH4 was 1.0%, and the reaction time was 12h before and after the XRD changes, see Figure 6 Co3O 4(400C) The diffraction peak at 2θ=36.8° of 1.0% CH4 catalytic oxidation at 500℃ for 12h is more enhanced than that of 3% Pd / Co3O 4(400C) The catalytic oxidation of 1.0% CH4 at 600℃ for 12h is more than that of the catalyst, indicating that the precious metal Pd loading is beneficial to inhibit the degradation of the carrier Co3O 4(400C) High temperature crystallization.
[0098] Test Example 4: Co3O prepared in Examples 1-4 4(400C) 、Co3O 4(650C) 、3%Pd / Co3O 4(400C) 、3%Pd / Co3O 4(650C) As a catalyst, the conversion rate of catalytic oxidation degradation of 1000 ppm toluene was tested under the condition of reaction space velocity GHSV = 40000 ml / (g·h), see Figure 7 As shown, Co3O 4(400C) The temperature at which the conversion rate of toluene in catalytic oxidation degradation reaches 90% (T 90 ) is 249℃, Co3O 4(650C) The temperature at which the conversion rate of toluene in catalytic oxidation degradation reaches 90% (T 90 ) is 254℃, 3%Pd / Co3O 4(400C) The temperature at which the conversion rate of toluene in catalytic oxidation degradation reaches 90% (T 90 ) is 213℃, 3%Pd / Co3O 4(650C) The temperature at which the conversion rate of toluene in catalytic oxidation degradation reaches 90% (T 90 ) is 24℃.
[0099] The above examples are used to illustrate the specific implementation of the present invention. However, the protection scope of the present invention is not limited to the above exemplary implementation. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a Co3O4-supported noble metal catalyst for catalytic oxidation of gaseous carbon-containing compounds, characterized in that: The preparation method comprises the following steps: S1. dissolving a soluble cobalt salt in water, mixing and reacting with an alkaline reagent to obtain a cobalt salt precipitate; S2. calcining the cobalt salt precipitate to obtain a carrier Co3O4; S3. The carrier Co3O4 and the soluble salt of the precious metal M are dissolved in a solvent and mixed, H2O2 is added to react and calcine to obtain M / Co3O4.
2. The preparation method according to claim 1, characterized in that: The mixing of the soluble cobalt salt aqueous solution and the alkaline reagent in step S1 comprises the following steps: adding the alkaline reagent to the soluble cobalt salt aqueous solution, stirring at room temperature for 0.1 to 1 hour, and obtaining a mixed solvent. Preferably, the concentration of the alkaline agent is 1 to 3 times the concentration of the soluble cobalt salt aqueous solution.
3. The preparation method according to claim 1, characterized in that: The reaction in step S1 is a solvent thermal reaction, which comprises the following steps: reacting the mixed solvent at a temperature of 100 to 200° C. for 4 to 24 hours. Preferably, the calcination temperature in step S2 is 300-800°C, and the calcination time is 2-12h.
4. The preparation method according to any one of claims 1 to 3, characterized in that: The soluble cobalt salt is selected from at least one of Co(NO3)2, CoCl2 and Co(CH3COO)2; the alkaline substance is selected from at least one of NaOH, Na2CO3 and NaHCO3.
5. The preparation method according to any one of claims 1 to 3, characterized in that: In step S3, the carrier Co3O4 and the soluble precious metal salt are dissolved in a solvent and mixed, which comprises the following steps: dispersing the carrier Co3O4 in a solvent, adding the soluble precious metal salt, and stirring at room temperature for 0.1 to 1 hour to obtain a mixed solution.
6. The preparation method according to claim 5, characterized in that: In terms of mass percent, the reaction of the mixed solution with the redox reaction driven hydrolysis precipitant comprises the following steps: heating the mixed solution to 20-100° C., adding the redox reaction driven hydrolysis precipitant H2O2, reacting for 2-10 hours, and obtaining a solid reactant. Preferably, the amount of H2O2 is more than 50 times that of the noble metal.
7. The preparation method according to claim 6, characterized in that: The precious metal loading precipitation process mainly uses Co3O4 as a catalyst to promote the redox reaction of H2O2. At the same time, the OH- produced by the redox reaction of H2O2 further reacts with the precious metal for precipitation, helping to complete the uniform loading of the precious metal.
8. The preparation method according to claim 6, characterized in that: The calcination in step S3 includes the following steps: calcining the solid reactant at a temperature of 200 to 400° C. for 2 to 12 hours. According to an embodiment of the present invention, after the solid reactant is obtained by reaction in step S3 and before calcination, the following steps are further included: filtering the reaction solution, washing and drying the solid reactant.
9. A Co3O4-supported noble metal catalyst prepared by the method according to any one of claims 1 to 8, characterized in that: The catalyst comprises amorphous or crystalline Co3O4, on which a noble metal having catalytic performance is loaded. Preferably, the Co3O4 has a flaky or granular structure, the size of the crystal structure is 50-500 nm, the noble metal M is at least one of Pd, Pt, Au, and Ru, and the loading amount of the noble metal is 0.1-5% of the carrier Co3O4.
10. Use of a Co3O4-supported noble metal catalyst prepared by the method according to any one of claims 1 to 8 or a Co3O4-supported noble metal catalyst according to any one of claims 9 to 10 in catalytic oxidation of gaseous carbon-containing compounds, such as VOCs or methane.
Citation Information
Patent Citations
Supported gold catalyst for cyclohexane oxidation and preparation method thereof
CN101992103A
Supported catalyst, preparation method and application thereof
CN109046345A
Cobaltosic oxide precious metal composite material and preparation method and application thereof, and direct hydrazine fuel cell
CN114005998A
Preparation method and application of supported noble metal tricobalt tetraoxide nanocatalyst
WO2018138618A1