System for activating vanadium phosphorus oxide catalyst and method for activating vanadium phosphorus oxide catalyst
By performing a three-stage activation process in a vanadium-phosphorus-oxygen catalyst activation system, the problem of uneven catalyst activation is solved, and efficient catalyst activation and high-performance n-butane oxidation to maleic anhydride reaction are achieved.
Patent Information
- Application Number
- CN202310376979.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-15
AI Technical Summary
During the activation process of the existing vanadium phosphorus oxygen catalyst, due to insufficient temperature or condition control, the catalyst does not transfer heat in a timely manner and may be burned or activated unevenly, affecting its performance in the reaction of n-butane oxidation to maleic anhydride.
A system including a furnace shell, an inner tank and a control unit is used to perform a three-stage activation process. The first activation temperature is 20-350°C, the second activation temperature is 300-410°C, and the third activation temperature is 390-450°C. , through different atmosphere and heating rate control to ensure uniform activation of the catalyst.
It achieves uniform activation of the catalyst, shortens the activation time, improves production efficiency, and exhibits high n-butane conversion rate and high maleic anhydride selectivity in the reaction of n-butane oxidation to maleic anhydride.
Smart Images

Figure CN118767955A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of catalyst synthesis, and in particular to a system for activating a vanadium phosphorus oxygen catalyst and an activation method for the vanadium phosphorus oxygen catalyst. Background Art
[0002] Maleic anhydride (maleic anhydride) is an important organic chemical raw material and fine chemical product. It is the third largest anhydride in the world after phthalic anhydride and acetic anhydride. It is mainly used in the production of thermosetting resins, unsaturated polyester resins, pesticides, medicines, coatings, inks, lubricant additives, paper chemicals, textile chemicals, textile finishing agents, food additives and surfactants. In addition, maleic anhydride can also be used as a raw material to produce a series of widely used fine chemical products such as 1,4-butanediol (GBL), tetrahydrofuran (THF), maleic acid, fumaric acid and tetrahydroanhydride. The development and utilization prospects are very broad, and its application range is still expanding.
[0003] Vanadium phosphorus oxide (VPO) catalysts are the most widely used industrial catalysts for the oxidation of n-butane to maleic anhydride. The surface properties of the catalyst, the addition of additives and the activation method of the catalyst all have a significant impact on the performance of the catalyst.
[0004] The vanadium phosphorus oxygen catalyst used in the early maleic anhydride device is an unactivated catalyst. After the enterprise purchases the catalyst, it is necessary to carry out the activation with material under a certain temperature and a certain butane concentration in the reactor. This process is called in-vessel activation. In the in-vessel activation, the catalyst often needs a long equilibrium time in the reaction to complete the activation of the catalyst, which reduces the industrial production efficiency and the economic efficiency of the catalyst. It is necessary for the maleic anhydride manufacturer to invest a lot of manpower, material resources and financial resources in the early stage of the catalyst use. The activation process of the catalyst also lacks the space for optimization, and the activity of the catalyst cannot be well controlled at the same time. To solve these problems, people have developed an out-vessel activation technology, that is, the catalyst has been activated before entering the reaction unit and can be directly used. CN1068053A uses the method of heating the vanadium phosphorus oxygen catalyst precursor in a molecular oxygen / water vapor / inert gas mixed atmosphere for activation, rapidly heating in a molecular oxygen / water vapor mixed atmosphere, and then keeping warm in a molecular oxygen / water vapor mixed atmosphere, and continuing to keep a period of time in an inert gas / water vapor to activate the catalyst. CN1849170A heats the vanadium phosphorus oxygen catalyst precursor to 380-600°C in an atmosphere containing steam, and maintains the final active catalyst under superatmospheric pressure. CN112705243A controls the catalyst activation temperature by heat exchange treatment during the activation process, but the actual structure control effect of the catalyst is not clarified. Due to the rapid phase change reaction of the physical phase during the activation process, a significant thermal effect will be produced, especially due to the large amount of accumulation of catalysts, the over-intensive loading will produce more complex thermal effects after activation, resulting in uneven catalyst activation effect. Therefore, it often occurs that the catalyst body is not timely in heat transfer or heat transfer due to the inaccurate control of the activator temperature or conditions, thereby causing the catalyst to be burned and lose activity, or the catalyst is not completely activated or the activation is uneven, affecting its catalytic performance in the subsequent n-butane oxidation to maleic anhydride reaction. How to enable the n-butane maleic anhydride catalyst to be activated at a stable temperature and improve the activation effect of the catalyst is a problem that needs to be solved urgently. Summary of the invention
[0005] In order to overcome the problems in the prior art that the temperature or conditions of the activator are not accurately controlled, resulting in untimely heat transfer or heat removal of the catalyst body, causing the catalyst to be burned and lose activity, or the catalyst is not completely activated or activated unevenly, thereby affecting its catalytic performance in the subsequent n-butane oxidation to maleic anhydride reaction, the present invention provides a system for activating a vanadium phosphorus oxygen catalyst and an activation method for a vanadium phosphorus oxygen catalyst, so as to achieve relatively stable activation of a large number of vanadium phosphorus oxygen catalyst precursor particles. The prepared vanadium phosphorus oxygen catalyst is applied to the n-butane oxidation to maleic anhydride reaction and has a higher n-butane conversion rate and a higher maleic anhydride selectivity.
[0006] In order to achieve the above-mentioned objectives, the present invention provides, on one hand, a system for activating a vanadium-phosphorus-oxygen catalyst, the system comprising: a furnace shell, an inner tank and a control unit; the inner tank comprises furnace wires and vanadium-phosphorus-oxygen catalyst precursor particles arranged in parallel along the axial direction of the inner tank, the furnace wires pass through the vanadium-phosphorus-oxygen catalyst precursor particles to activate the catalyst precursor particles; the control unit is used to control the activation temperature.
[0007] A second aspect of the present invention provides a method for activating a vanadium phosphorus oxygen catalyst, the activation method comprising: subjecting vanadium phosphorus oxygen catalyst precursor particles to a first activation, a second activation, and a third activation; the temperature of the third activation is greater than the temperature of the second activation, and the temperature of the second activation is greater than the temperature of the first activation;
[0008] Wherein, the activation is carried out in the system described in the first aspect.
[0009] Through the above technical solution, the beneficial effects of the present invention include:
[0010] The system for activating vanadium phosphorus oxygen catalyst provided by the present invention fundamentally eliminates the amplification effect of mass transfer and heat transfer during the activation process, making the activation more uniform, while shortening the activation time, improving the production efficiency, and having great market application potential.
[0011] The method provided by the present invention can stably activate a large number of vanadium phosphorus oxygen catalyst precursor particles by performing a three-stage activation process in the activation system provided by the present invention. The prepared vanadium phosphorus oxygen catalyst is applied to the reaction of n-butane oxidation to prepare maleic anhydride and has a high n-butane conversion rate and a high maleic anhydride selectivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 is a schematic diagram of an activation system provided in Example 1 of the present invention;
[0013] Figure 2 is a schematic diagram of an activation system provided in Example 4 of the present invention;
[0014] Figure 3 is a schematic diagram of an activation system provided in Example 5 of the present invention;
[0015] Figure 4 It is a schematic diagram of an activation system provided in Comparative Example 3 of the present invention.
[0016] Description of Reference Numerals
[0017] 1. Inner liner pores; 2. Inner liner; 3. Vanadium phosphorus oxygen catalyst precursor particles;
[0018] 4. Furnace shell; 5. Furnace wire; 6. Furnace shell pipe. DETAILED DESCRIPTION
[0019] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0020] In the description of the present invention, it should be understood that the terms "longitudinal", "lateral", "upper", "lower", "vertical", "horizontal", "top", "bottom", "axial", "radial" and the like indicating the orientation or positional relationship are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, "inside and outside" refer to the inside and outside relative to the outline of each component itself.
[0021] On the one hand, the present invention provides a system for activating a vanadium phosphorus oxygen catalyst, which includes: a furnace shell, an inner shell and a control unit; the inner shell includes furnace wires and vanadium phosphorus oxygen catalyst precursor particles arranged in parallel along the axial direction of the inner shell, and the furnace wires pass through the vanadium phosphorus oxygen catalyst precursor particles to activate the catalyst precursor particles; the control unit is used to control the activation temperature.
[0022] In the existing vanadium phosphorus oxygen catalyst activation technology, the vanadium phosphorus oxygen catalyst precursor particles are usually stacked in an activation furnace in a disordered manner. This activation method will produce a significant thermal effect due to the rapid phase change reaction of the physical phase, especially when the catalyst is piled up in large quantities and loaded too densely, a more complex thermal effect will be produced after activation, resulting in uneven catalyst activation effect. Therefore, it often occurs that the catalyst body is not timely in heat transfer or heat transfer due to the inaccurate control of the activator temperature or conditions, thereby causing the catalyst to be burned and lose activity, or the catalyst is not completely activated or the activation is uneven, affecting its catalytic performance in the subsequent n-butane oxidation to maleic anhydride reaction. When the system provided by the present invention is used for vanadium phosphorus oxygen catalyst activation, the activation effect is significantly improved, and a large number of vanadium phosphorus oxygen catalyst precursor particles can be activated more stably. The prepared vanadium phosphorus oxygen catalyst is applied to the n-butane oxidation to maleic anhydride reaction with a higher n-butane conversion rate and a higher maleic anhydride selectivity.
[0023] In the present invention, the system may include unactivated vanadium phosphorus oxygen catalyst precursor particles or activated vanadium phosphorus oxygen catalysts, that is, both the system before and after activation are within the protection scope of the present invention.
[0024] The present invention has no particular limitation on the control unit, and any commonly used control unit in the art may be used, as long as the purpose of controlling the activation temperature can be achieved. The control unit may be commercially available.
[0025] According to the present invention, preferably, the vanadium phosphorus oxygen catalyst precursor particles are provided with through holes for the furnace wire to pass through.
[0026] The present invention has no particular limitation on the shape of the vanadium phosphorus oxygen catalyst precursor particles, which can be any shape conventionally used in the art, and the shape of the vanadium phosphorus oxygen catalyst precursor particles can be regular or irregular, as long as they can meet the above-mentioned requirement of being able to pass through the furnace wire. Preferably, the shape of the vanadium phosphorus oxygen catalyst precursor particles is a hollow cylinder.
[0027] Preferably, the vanadium phosphorus oxygen catalyst precursor particles have an inner diameter of 1-5 mm and an outer diameter of 4-20 mm.
[0028] The system of the present invention has no particular restrictions on the composition and structural parameters (content of each component, bulk density, etc.) of the vanadium phosphorus oxygen catalyst precursor particles, which can be various vanadium phosphorus oxygen catalyst precursor particles in the art. The vanadium phosphorus oxygen catalyst precursor particles can be any particle as long as they can meet the above-mentioned requirement of being able to pass through the furnace wire.
[0029] According to the present invention, preferably, based on the total weight of the vanadium phosphorus oxygen catalyst, the mass content of V2O5 is 20-80%, and the mass content of P2O5 is 20-50%.
[0030] According to the present invention, preferably, the atomic ratio of vanadium to phosphorus is 0.8-2, preferably 0.8-1.4.
[0031] According to the present invention, preferably, the bulk density of the vanadium phosphorus oxygen catalyst precursor particles is 0.6-0.85 g / cm 3 , preferably 0.7-0.8 g / cm 3 .
[0032] The present invention has no particular limitation on the method for preparing the vanadium phosphorus oxygen catalyst precursor particles. As long as the vanadium phosphorus oxygen catalyst precursor particles satisfying the above characteristics can be obtained, the present invention is not limited here.
[0033] The present invention has no particular limitation on the diameter of the furnace wire, as long as it can pass through the phosphorus-oxygen catalyst precursor. Preferably, the diameter of the furnace wire is smaller than the inner diameter of the vanadium-phosphorus-oxygen catalyst precursor particles.
[0034] According to the present invention, preferably, the spacing between adjacent furnace wires is greater than the outer diameter of the vanadium phosphorus oxygen catalyst precursor particles, preferably 1.1-3 times the outer diameter of the vanadium phosphorus oxygen catalyst precursor particles. This preferred embodiment can ensure uniform mass and heat transfer of the catalyst precursor particles while saving space in the furnace.
[0035] The present invention has no particular limitation on the arrangement of the furnace wires, and any arrangement is possible. In order to efficiently utilize the space in the furnace, preferably, the furnace wires are arranged in a hexagonal or orthogonal manner.
[0036] The arrangement of the furnace wires of the present invention is appropriately selected according to the shape of the inner container. For example, when the cross section of the inner container is square, an orthogonal arrangement can be adopted. The orthogonal arrangement refers to arrangement in rows and columns. When the cross section of the inner container is circular, a hexagonal distribution can be adopted. The hexagonal distribution refers to a simple hexagon with a hexagon and a center point, which is spread out to the surroundings to obtain multiple intersecting hexagons.
[0037] In the present invention, the number of the furnace wires can be appropriately selected according to the specific activation amount of the vanadium phosphorus oxygen catalyst precursor particles.
[0038] According to the present invention, preferably, the furnace wire is a metal wire with an insulation treatment on the surface, and the metal wire is selected from at least one of stainless steel wire, iron wire, iron-chromium-aluminum alloy wire, nickel-chromium alloy wire, molybdenum wire and tungsten wire. The above furnace wire is a commonly used furnace wire and can be obtained commercially.
[0039] According to the present invention, preferably, the inner container is provided with a hole for introducing the activated atmosphere.
[0040] The present invention has no particular limitation on the specific size and number of the pores, which can be appropriately selected according to specific circumstances, as long as the activation can proceed smoothly.
[0041] According to the present invention, preferably, the inner container further comprises a connection terminal for connecting two ends of the furnace wire.
[0042] The present invention has no particular limitation on the type of the connection terminal, and the connection terminals commonly used in the art can be used, and the present invention does not make any requirements therefor.
[0043] The present invention has no particular limitation on the size of the inner container, and the size can be appropriately selected according to the specific activation amount of the vanadium phosphorus oxygen catalyst precursor particles.
[0044] According to the present invention, preferably, the furnace shell is provided with a pipeline for introducing the activation atmosphere.
[0045] The present invention has no particular limitation on the specific diameter, length and location of the pipeline, which can be appropriately selected according to specific circumstances, as long as the activation can be carried out smoothly.
[0046] According to the present invention, preferably, the furnace shell is made of high temperature resistant material.
[0047] The high temperature resistant material described in the present invention refers to an inorganic material that can withstand temperatures above 450°C.
[0048] The present invention has no particular limitation on the type of the high temperature resistant material, and it can be any conventional material in the art. Preferably, the high temperature resistant material is steel.
[0049] The present invention has a wide range of choices for the shape of the furnace shell. Preferably, the shape of the furnace shell is a cuboid, a cylinder, a sphere or a polygonal prism.
[0050] The present invention has no particular limitation on the size of the furnace shell, which can be appropriately selected according to specific circumstances, as long as it can seal the inner container.
[0051] Preferably, the inner container is sealed in the furnace shell.
[0052] The present invention has no particular limitation on how the inner container is sealed in the furnace shell. The inner container can be sealed in the furnace shell longitudinally or transversely.
[0053] The “longitudinally sealed in the furnace body shell” mentioned in the present invention means that the furnace wire in the inner container is vertically sealed in the furnace body shell.
[0054] The term “transversely placed in the furnace body shell” in the present invention means that the furnace wire in the inner container is transversely sealed in the furnace body shell.
[0055] A second aspect of the present invention provides a method for activating a vanadium phosphorus oxygen catalyst, the activation method comprising: subjecting vanadium phosphorus oxygen catalyst precursor particles to a first activation, a second activation, and a third activation; the temperature of the third activation is greater than the temperature of the second activation, and the temperature of the second activation is greater than the temperature of the first activation;
[0056] Wherein, the activation is carried out in the system described in the first aspect.
[0057] According to the present invention, preferably, the first activation comprises: heating the catalyst precursor particles from room temperature to a first activation temperature in a first activation atmosphere, and then maintaining the temperature at a first constant temperature.
[0058] According to the present invention, preferably, the first activation temperature is 20-350° C., preferably 200-300° C.; the first constant temperature time is 0-5 h, preferably 0-2 h.
[0059] According to the present invention, preferably, the heating rate for heating to the first activation temperature is 0.5-10°C / min, preferably 1-5°C / min, for example 0.5°C / min, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min, 6°C / min, 6.5°C / min, 7°C / min, 7.5°C / min, 8°C / min, 8.5°C / min, 9°C / min, 9.5°C / min, 10°C / min, and any value in the range formed by any two of these values.
[0060] According to the present invention, preferably, the volume space velocity of the first activation atmosphere is 0-1000h -1 , preferably 0-50h -1 .
[0061] In the present invention, “the volume space velocity is 0” means that the first activation is performed under the closed condition of the first activation atmosphere.
[0062] According to the present invention, preferably, the first activation atmosphere is air.
[0063] When the first activation atmosphere is air, there is no need to introduce air separately, and the first activation can be carried out directly.
[0064] According to the present invention, preferably, the second activation condition comprises: heating the catalyst precursor particles from a first activation temperature to a second activation temperature in a second activation atmosphere, and then performing a second constant temperature maintenance.
[0065] According to the present invention, preferably, the second activation temperature is 300-410°C, preferably 350-410°C; the second constant temperature time is 0-5h, preferably 0-2h.
[0066] According to the present invention, preferably, the heating rate for heating to the second activation temperature is 1-20°C / min, preferably 4-12°C / min, for example, 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, 11°C / min, 12°C / min, 13°C / min, 14°C / min, 15°C / min, 16°C / min, 17°C / min, 18°C / min, 19°C / min, 20°C / min, and any value in the range formed by any two of these values.
[0067] According to the present invention, preferably, the volume space velocity of the second activation atmosphere is 0-2000h-1 , preferably 800-1500h -1 .
[0068] In the present invention, “the volume space velocity is 0” means that the second activation is performed under the closed condition of the second activation atmosphere.
[0069] According to the present invention, preferably, the second activation atmosphere is a mixed gas of air and water vapor.
[0070] According to the present invention, preferably, based on the total volume of the mixed gas of air and water vapor, the volume proportion of air is 85-95%, and the volume proportion of water vapor is 5-15%.
[0071] According to a preferred embodiment of the present invention, the second activation conditions include: heating the catalyst precursor particles from the first activation temperature to the second activation temperature in the second activation atmosphere, and then maintaining the second constant temperature; the second activation temperature is 350-410°C; the second constant temperature time is 0-2h; the heating rate to the second activation temperature is 4-12°C / min; the volume space velocity of the second activation atmosphere is 800-1500h -1 The second activation atmosphere is a mixture of air and water vapor; based on the total volume of the mixture of air and water vapor, the volume of air accounts for 85-95%, and the volume of water vapor accounts for 5-15%. This preferred embodiment makes mass transfer and heat transfer more rapid and uniform, supports a faster heating rate, is conducive to the transformation of the catalyst crystal phase, and thus makes the catalyst have better catalytic performance.
[0072] According to a specific embodiment of the present invention, the second activation atmosphere is introduced for 5-60 minutes, and then the temperature is raised. With this preferred embodiment, the first activation atmosphere can be completely replaced.
[0073] The time for introducing the second activation atmosphere of the present invention depends on the size of the activation furnace.
[0074] According to the present invention, preferably, the third activation comprises: raising the temperature of the catalyst precursor particles from the second activation temperature to the third activation temperature in a third activation atmosphere, and then performing a third constant temperature maintenance.
[0075] According to the present invention, preferably, the third activation temperature is 390-450°C, preferably 405-450°C; the third constant temperature time is 3-10h, preferably 4-8h.
[0076] According to the present invention, preferably, the heating rate for heating to the third activation temperature is 0.1-10°C / min, preferably 0.5-5°C / min, for example 0.1°C / min, 0.5°C / min, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min, 6°C / min, 6.5°C / min, 7°C / min, 7.5°C / min, 8°C / min, 8.5°C / min, 9°C / min, 9.5°C / min, 10°C / min, and any value in the range formed by any two of these values.
[0077] According to the present invention, preferably, the volume space velocity of the third activation atmosphere is 0-2000h -1 , preferably 0-1500h -1 .
[0078] In the present invention, “the volume space velocity is 0” means that the third activation is performed under the closed condition of the third activation atmosphere.
[0079] According to the present invention, preferably, the third activation atmosphere is a mixed gas of an inert gas and water vapor.
[0080] According to the present invention, preferably, based on the total volume of the mixed gas of the inert gas and the water vapor, the volume proportion of the inert gas is 40-60%, and the volume proportion of the water vapor is 40-60%.
[0081] According to a preferred embodiment of the present invention, the third activation comprises: heating the catalyst precursor particles from the second activation temperature to the third activation temperature in the third activation atmosphere, and then maintaining the third constant temperature; the third activation temperature is 405-450°C; the third constant temperature time is 4-8h; the heating rate to the third activation temperature is 0.5-5°C / min; the volume space velocity of the third activation atmosphere is 0-1500h -1 ; The third activation atmosphere is a mixed gas of inert gas and water vapor; based on the total volume of the mixed gas of inert gas and water vapor, the volume of the inert gas accounts for 40-60%, and the volume of water vapor accounts for 40-60%. By adopting this preferred embodiment, the catalyst is finally converted into more desired crystal composition. The obtained catalyst is applied to the reaction of preparing maleic anhydride by oxidation of n-butane, which is beneficial to the improvement of the yield of maleic anhydride.
[0082] According to a specific embodiment of the present invention, the third activation atmosphere is introduced for 5-60 minutes, and then the temperature is raised. With this preferred embodiment, the second activation atmosphere can be completely replaced.
[0083] The time for introducing the third activation atmosphere of the present invention depends on the size of the activation furnace.
[0084] According to the present invention, preferably, the activation method further comprises: cooling the vanadium phosphorus oxygen catalyst precursor particles from the third activation temperature to room temperature in an inert atmosphere.
[0085] According to the present invention, preferably, the volume space velocity of the inert atmosphere is 0-1500h -1 , preferably 0-1000h -1 .
[0086] In the present invention, "the volume space velocity is 0" means that the temperature is lowered under a closed condition of an inert atmosphere.
[0087] According to the present invention, preferably, the inert atmosphere is nitrogen.
[0088] According to a specific embodiment of the present invention, the inert atmosphere is introduced for 5-60 minutes, and then the temperature is lowered. With this preferred embodiment, the third activation atmosphere can be completely replaced.
[0089] The time for introducing the inert atmosphere of the present invention depends on the size of the activation furnace.
[0090] According to the present invention, preferably, the activation method further comprises: before performing the second activation, first preheating the second activation atmosphere.
[0091] According to the present invention, preferably, the first preheating temperature and the first activation temperature satisfy the following condition: (first activation temperature-100° C.)<first preheating temperature<(first activation temperature+50° C.).
[0092] According to the present invention, preferably, the activation method further comprises: before performing the third activation, performing a second preheating on the third activation atmosphere.
[0093] According to the present invention, preferably, the second preheating temperature and the second activation temperature satisfy the following condition: (second activation temperature-100° C.)<second preheating temperature<(second activation temperature+50° C.).
[0094] In the present invention, the "first", "second" and "third" do not limit the substances and operations, but are only used to distinguish the substances introduced in different steps and the operations performed in different stages.
[0095] The present invention will be described in detail below through examples.
[0096] Preparation Example 1
[0097] This preparation is used to illustrate the preparation of vanadium phosphorus oxygen catalyst precursor particles.
[0098] In a 50L double-layer glass reactor, add 2120g of V2O5, 20L of isobutyl alcohol and 3L of benzyl alcohol mixed solution, stir evenly and reflux for 3h, then dropwise add 2170g of 105wt% phosphoric acid and heat and stir until reflux and maintain for 16h, the resulting precipitate is filtered and vacuum dried at 150°C for 24h to obtain the original powder. The original powder is mixed with graphite powder (the mass ratio of the original powder to the graphite powder is 96:4) and granulated and pressed into hollow cylindrical catalyst precursor particles with an outer diameter of 12mm, an inner diameter of 4mm and a height of 5mm, and the bulk density is 0.71g / cm 3 The mass content of V2O5 in the vanadium phosphorus oxygen catalyst is 53%, the mass content of P2O5 is 42%, and the atomic ratio of vanadium to phosphorus is 1:1.14.
[0099] Example 1
[0100] Make a cubic activation furnace with an inner tank side length of 40 cm, such as Figure 1 As shown, the activation furnace includes a furnace shell, an inner tank longitudinally sealed to the furnace shell, and a control unit. The inner tank includes furnace wires arranged parallel to the axis of the inner tank and vanadium phosphorus oxygen catalyst precursor particles prepared in Preparation Example 1 and threaded on the furnace wires. The control unit is used to control the activation temperature. The furnace wires are iron-chromium-aluminum alloy wires with insulation treatment on the surface. They are arranged orthogonally, with 12 wires in each row, a total of 12 columns, and a spacing of 3 cm between adjacent furnace wires. A hole is provided on the inner tank for the introduction of an activation atmosphere. The inner tank also includes a terminal for connecting the two ends of the furnace wire. A pipe is provided on the furnace shell for the introduction of an activation atmosphere. The furnace shell is made of steel material.
[0101] First activation: In air atmosphere, heat up to 250°C at a heating rate of 2°C / min and maintain at this temperature for 0.5h.
[0102] Second activation: The atmosphere was replaced with a preheated gas mixture of 90% steam and 10% air at a volume space velocity of 1000 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was continued to rise to 380°C at a heating rate of 10°C / min and maintained at this temperature for 0.5h.
[0103] Third activation: The atmosphere was replaced with a preheated gas mixture of 55% by volume water vapor and 45% by volume nitrogen at a volume space velocity of 1000 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was raised to 410°C at a rate of 1°C / min and maintained at this temperature for 5 hours.
[0104] The atmosphere was replaced with nitrogen at a volume space velocity of 500 h -1After replacing the gas in the furnace for 15 minutes, the temperature was naturally cooled to room temperature to obtain a vanadium phosphorus oxygen catalyst.
[0105] Example 2
[0106] Using the activation furnace described in Example 1, Figure 1 shown.
[0107] First activation: In air atmosphere, heat to 210°C at a heating rate of 1°C / min and maintain at this temperature for 1 h.
[0108] Second activation: The atmosphere was replaced with a preheated gas mixture of 85% steam and 15% air at a volume space velocity of 1200 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was continued to rise to 400°C at a heating rate of 4°C / min and maintained at this temperature for 1 hour.
[0109] Third activation: The atmosphere was replaced with a preheated gas mixture of 50% steam and 50% nitrogen at a volume space velocity of 1300 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was raised to 410°C at a rate of 0.5°C / min and maintained at this temperature for 6 hours.
[0110] The atmosphere was replaced with nitrogen at a volume space velocity of 500 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was naturally cooled to room temperature to obtain a vanadium phosphorus oxygen catalyst.
[0111] Example 3
[0112] Using the activation furnace described in Example 1, Figure 1 shown.
[0113] First activation: In air atmosphere, heat up to 280°C at a heating rate of 4°C / min and maintain at this temperature for 1 h.
[0114] Second activation: The atmosphere was replaced with a preheated gas mixture of 92% water vapor and 8% air at a volume space velocity of 1200 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was continued to rise to 405°C at a heating rate of 8°C / min and maintained at this temperature for 1 hour.
[0115] Third activation: The atmosphere was replaced with a preheated gas mixture of 45% by volume water vapor and 55% by volume nitrogen at a volume space velocity of 1500 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was raised to 430°C at 3°C / min, while the gas was continuously introduced for 2 hours and maintained at this temperature for 8 hours.
[0116] The atmosphere was replaced with nitrogen at a volume space velocity of 500 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was naturally cooled to room temperature to obtain a vanadium phosphorus oxygen catalyst.
[0117] Example 4
[0118] The method of Example 1 is followed, except that the inner container is transversely sealed in the furnace shell, such as Figure 2 As shown, a vanadium phosphorus oxygen catalyst was obtained.
[0119] Example 5
[0120] Make as Figure 3 The cylindrical activation furnace shown has a furnace inner shell with a diameter of 40 cm and a height of 40 cm. The activation furnace includes a furnace shell, an inner shell longitudinally sealed to the furnace shell, and a control unit. The inner shell includes furnace wires arranged parallel to the axis of the inner shell and vanadium phosphorus oxygen catalyst precursor particles prepared in Preparation Example 1 and threaded on the furnace wires. The control unit is used to control the activation temperature. The furnace wires are iron-chromium-aluminum alloy wires with insulation treatment on the surface, distributed in a hexagonal pattern, and the spacing between adjacent furnace wires is 4 cm. A hole is provided on the inner shell for the introduction of an activation atmosphere. The inner shell also includes a terminal for connecting the two ends of the furnace wire. A pipe is provided on the furnace shell for the introduction of an activation atmosphere. The furnace shell is made of steel.
[0121] First activation: In air atmosphere, heat up to 250°C at a heating rate of 2°C / min and maintain at this temperature for 0.5h.
[0122] Second activation: The atmosphere was replaced with a preheated gas mixture of 90% steam and 10% air at a volume space velocity of 1000 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was continued to rise to 380°C at a heating rate of 10°C / min and maintained at this temperature for 0.5h.
[0123] Third activation: The atmosphere was replaced with a preheated gas mixture of 55% by volume water vapor and 45% by volume nitrogen at a volume space velocity of 1000 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was raised to 410°C at a rate of 1°C / min and maintained at this temperature for 5 hours.
[0124] The atmosphere was replaced with nitrogen at a volume space velocity of 500 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was naturally cooled to room temperature to obtain a vanadium phosphorus oxygen catalyst.
[0125] Comparative Example 1
[0126] The method of Example 1 is followed, except that no inner liner is provided, 5 cm ceramic particles are laid in the furnace shell as support, and then vanadium phosphorus oxygen catalyst precursor particles are randomly stacked on the ceramic particles to obtain a vanadium phosphorus oxygen catalyst.
[0127] Comparative Example 2
[0128] The method of Example 5 is followed, except that no inner liner is provided, 5 cm ceramic particles are laid in the furnace shell as support, and then vanadium phosphorus oxygen catalyst precursor particles are randomly stacked on the ceramic particles to obtain a vanadium phosphorus oxygen catalyst.
[0129] Comparative Example 3
[0130] use Figure 4 The activation furnace shown is a cylindrical stainless steel tube with an inner diameter of 2.1 cm and a height of 40 cm. It is equipped with an external electric heater. 5 cm of ceramic particles are laid on the bottom of the tube as support, and then vanadium phosphorus oxygen catalyst precursor particles are randomly stacked on the ceramic particles.
[0131] First activation: In air atmosphere, heat up to 250°C at a heating rate of 2°C / min and maintain at this temperature for 0.5h.
[0132] Second activation: The atmosphere was replaced with a preheated gas mixture of 90% steam and 10% air at a volume space velocity of 1000 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was continued to rise to 380°C at a heating rate of 10°C / min and maintained at this temperature for 0.5h.
[0133] Third activation: The atmosphere was replaced with a preheated gas mixture of 55% by volume water vapor and 45% by volume nitrogen at a volume space velocity of 1000 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was raised to 410°C at 1°C / min, while the gas was continuously introduced for 30 minutes and maintained at this temperature for 5 hours.
[0134] The atmosphere was replaced with nitrogen at a volume space velocity of 500 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was naturally cooled to room temperature to obtain a vanadium phosphorus oxygen catalyst.
[0135] Because the amount of catalyst required for one small-scale experiment was insufficient, it had to be repeated three times.
[0136] Comparative Example 4
[0137] use Figure 4The activation furnace D shown is a cylindrical stainless steel tube with an inner diameter of 2.1 cm and a height of 40 cm. It is equipped with an external electric heater. 5 cm of ceramic particles are laid on the bottom of the tube as support, and then vanadium phosphorus oxygen catalyst precursor particles are randomly stacked on the ceramic particles.
[0138] First activation: In air atmosphere, heat to 210°C at a heating rate of 1°C / min and maintain at this temperature for 1 h.
[0139] Second activation: The atmosphere was replaced with a preheated gas mixture of 85% steam and 15% air at a volume space velocity of 1200 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was continued to rise to 400°C at a heating rate of 4°C / min and maintained at this temperature for 1 hour.
[0140] Third activation: The atmosphere was replaced with a preheated gas mixture of 50% steam and 50% nitrogen at a volume space velocity of 1300 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was raised to 410°C at a rate of 0.5°C / min, while continuously introducing gas for 1 hour and maintaining this temperature for 6 hours.
[0141] The atmosphere was replaced with nitrogen at a volume space velocity of 500 h -1 After replacing the gas in the furnace for 15 minutes, the temperature was naturally cooled to room temperature to obtain a vanadium phosphorus oxygen catalyst.
[0142] Because the amount of catalyst required for one small-scale experiment was insufficient, it had to be repeated three times.
[0143] Test Example 1
[0144] The vanadium phosphorus oxygen catalysts obtained in the examples and comparative examples were evaluated in a 120 mL small-scale fixed bed reactor. The evaluation conditions were as follows: the reaction raw material was n-butane gas, the oxidant was air, the volume fraction of n-butane was 1.8%, the molten salt temperature was 400°C, and the volume space velocity of n-butane and air was 1500 h -1 , the evaluation results are shown in Table 1.
[0145] Volume fraction of n-butane = volume of n-butane introduced / (volume of n-butane introduced + volume of air introduced) × 100%.
[0146] Table 1
[0147] catalyst n-Butane conversion rate / % Maleic anhydride selectivity / % Maleic anhydride yield / wt% Example 1 86.1 70.5 102.6 Example 2 85.6 70 101.2 Example 3 85.9 70.2 101.9 Example 4 85.9 70.6 102.5 Example 5 86.1 70.7 102.9 Comparative Example 1 82.2 68.5 95.1 Comparative Example 2 83.3 68.7 96.7 Comparative Example 3 83.5 69 97.4 Comparative Example 4 84.5 70.1 100.1
[0148] Note: Weight yield = molar yield × (relative molecular mass of product / relative molecular mass of reactant)
[0149] It can be seen from the results in Table 1 that the vanadium phosphorus oxygen catalyst prepared by the activation method of the present invention has a higher n-butane conversion rate and a higher maleic anhydride selectivity when applied to the n-butane oxidation reaction to produce maleic anhydride.
[0150] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A system for activating a vanadium phosphorus oxygen catalyst, the system comprising: A furnace shell, an inner shell and a control unit; the inner shell includes furnace wires and vanadium phosphorus oxygen catalyst precursor particles arranged in parallel along the axial direction of the inner shell, the furnace wires pass through the vanadium phosphorus oxygen catalyst precursor particles to activate the catalyst precursor particles; the control unit is used to control the activation temperature.
2. The system according to claim 1, wherein: The vanadium phosphorus oxygen catalyst precursor particles are provided with through holes for the furnace wire to pass through; Preferably, the vanadium phosphorus oxygen catalyst precursor particles are in the shape of a hollow cylinder; Preferably, the inner diameter of the vanadium phosphorus oxygen catalyst precursor particles is 1-5 mm and the outer diameter is 4-20 mm; Preferably, based on the total weight of the vanadium phosphorus oxygen catalyst, the mass content of V2O5 is 20-80%, and the mass content of P2O5 is 20-50%; Preferably, the atomic ratio of vanadium to phosphorus is 0.8-2, preferably 0.8-1.4; Preferably, the bulk density of the vanadium phosphorus oxygen catalyst precursor particles is 0.6-0.85 g / cm 3 , preferably 0.7-0.8 g / cm 3 .
3. The system according to claim 1, wherein: The diameter of the furnace wire is smaller than the inner diameter of the vanadium phosphorus oxygen catalyst precursor particles; Preferably, the spacing between adjacent furnace wires is greater than the outer diameter of the vanadium phosphorus oxygen catalyst precursor particles, preferably 1.1-3 times the outer diameter of the vanadium phosphorus oxygen catalyst precursor particles; Preferably, the furnace wire is a metal wire with an insulation treatment on the surface, and the metal wire is selected from at least one of stainless steel wire, iron wire, iron-chromium-aluminum alloy wire, nickel-chromium alloy wire, molybdenum wire and tungsten wire.
4. The system according to any one of claims 1 to 3, wherein: The inner container is provided with a hole for introducing the activated atmosphere; Preferably, the inner container further comprises a connection terminal for connecting the two ends of the furnace wire; Preferably, the furnace shell is provided with a pipeline for introducing the activated atmosphere; Preferably, the furnace shell is made of high temperature resistant material; Preferably, the shape of the furnace shell is a cuboid, a cylinder, a sphere or a polygonal prism; Preferably, the inner container is sealed in the furnace shell.
5. A method for activating a vanadium phosphorus oxygen catalyst, the activation method comprising: Performing a first activation, a second activation, and a third activation on the vanadium phosphorus oxygen catalyst precursor particles; The temperature of the third activation is greater than the temperature of the second activation, and the temperature of the second activation is greater than the temperature of the first activation; Wherein, the activation is carried out in the system described in any one of claims 1-4.
6. The activation method according to claim 5, wherein: The first activation comprises: heating the catalyst precursor particles from room temperature to a first activation temperature in a first activation atmosphere, and then maintaining the temperature at a first constant temperature; Preferably, the first activation temperature is 20-350°C, preferably 200-300°C; the first constant temperature time is 0-5h, preferably 0-2h; Preferably, the heating rate of heating to the first activation temperature is 0.5-10°C / min, preferably 1-5°C / min; Preferably, the volume space velocity of the first activation atmosphere is 0-1000h -1 , preferably 0-50h -1 ; Preferably, the first activation atmosphere is air.
7. The activation method according to claim 5, wherein: The second activation conditions include: heating the catalyst precursor particles from a first activation temperature to a second activation temperature in a second activation atmosphere, and then maintaining the temperature at a second constant temperature; Preferably, the second activation temperature is 300-410°C, preferably 350-410°C; the second constant temperature time is 0-5h, preferably 0-2h; Preferably, the heating rate of heating to the second activation temperature is 1-20°C / min, preferably 4-12°C / min; Preferably, the volume space velocity of the second activation atmosphere is 0-2000h -1 , preferably 800-1500h -1 ; Preferably, the second activation atmosphere is a mixture of air and water vapor; Preferably, based on the total volume of the mixed gas of air and water vapor, the volume proportion of air is 85-95%, and the volume proportion of water vapor is 5-15%.
8. The activation method according to claim 5, wherein: The third activation comprises: heating the catalyst precursor particles from the second activation temperature to the third activation temperature in a third activation atmosphere, and then maintaining the temperature at a third constant temperature; Preferably, the third activation temperature is 390-450°C, preferably 405-450°C; the third constant temperature time is 3-10h, preferably 4-8h; Preferably, the heating rate of heating to the third activation temperature is 0.1-10°C / min, preferably 0.5-5°C / min; Preferably, the volume space velocity of the third activation atmosphere is 0-2000h -1 , preferably 0-1500h -1 ; Preferably, the third activation atmosphere is a mixed gas of an inert gas and water vapor; Preferably, based on the total volume of the mixed gas of the inert gas and the water vapor, the volume proportion of the inert gas is 40-60%, and the volume proportion of the water vapor is 40-60%.
9. The activation method according to any one of claims 5 to 8, wherein: The activation method further comprises: cooling the vanadium phosphorus oxygen catalyst precursor particles from a third activation temperature to room temperature in an inert atmosphere; Preferably, the volume space velocity of the inert atmosphere is 0-1500h -1 , preferably 0-1000h -1 ; Preferably, the inert atmosphere is nitrogen.
10. The activation method according to any one of claims 5 to 9, wherein: The activation method further comprises: before performing the second activation, first preheating the second activation atmosphere; Preferably, the first preheating temperature and the first activation temperature satisfy the following condition: (first activation temperature-100° C.)<first preheating temperature<(first activation temperature+50° C.).
11. The activation method according to any one of claims 5 to 10, wherein: The activation method further comprises: before performing the third activation, first performing a second preheating of the third activation atmosphere; Preferably, the second preheating temperature and the second activation temperature satisfy the following condition: (second activation temperature-100°C)<second preheating temperature<(second activation temperature+50°C).
Citation Information
Patent Citations
Catalyst molded bodies and method for producing maleic acid anhydride
CN102325593A
Process for transformation of vanadium / phosphorus mixed oxide catalyst precursors into active catalysts for production of maleic anhydride
CN1068053A
Preparation method of vanadium-phosphorus oxide catalyst
CN111097465A
Catalyst for preparing phthalic anhydride through oxidation and preparation method thereof
CN112547103A
Vanadium phosphorus oxide catalyst and activation method and application thereof
CN112691686A
Cited By
Activation method for vanadium phosphorus oxygen catalyst for use in oxidation of butane to prepare maleic anhydride
WO2026124202A1