Preparation method of catalyst for preparing ethylene glycol monomethyl ether through dimethyl oxalate hydrogenation
The catalyst with SiO2 carrier and copper and silver as the main active components is prepared through the dimethyl oxalate hydrogenation method, which solves the problems in the existing technology of relying on petrochemical products for raw materials and poor catalyst stability, and achieves efficient and economical ethylene dioxide production. The preparation of alcohol methyl ether is suitable for industrial production.
Patent Information
- Application Number
- CN202411012112.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing preparation method of ethylene glycol methyl ether, the raw materials rely on petrochemical products, and the cost and output are greatly affected by the oil market. The catalyst is easy to swell and has low mechanical strength, making it difficult to apply on a large scale.
The dimethyl oxalate hydrogenation method is used to prepare a catalyst with SiO2 as a carrier and copper and silver as the main active components by mixing, roasting and tableting soluble copper salts, silver salts and silicon sources under specific conditions. Catalytic hydrogenation reaction of dimethyl oxalate to prepare ethylene glycol methyl ether.
It significantly improves the reaction efficiency and activity of the catalyst, is suitable for a wide range of industrial conditions, reduces energy consumption and costs, extends the service life of the catalyst, and reduces the generation of by-products.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a method for preparing a catalyst for preparing ethylene glycol methyl ether by hydrogenating dimethyl oxalate. Background Art
[0002] The molecular structure of ethylene glycol methyl ether contains hydrocarbon groups, hydroxyl groups and ether bonds. It is widely used in various solvents, pharmaceutical intermediates and fuel additives in industrial production.
[0003] At present, the commonly used preparation methods of ethylene glycol methyl ether mainly include: (1) Ethylene oxide method, which is the most important method in current industrial production. Ethylene oxide, methanol and solid base are reacted in the presence of a catalyst to synthesize ethylene glycol methyl ether. The raw materials of this method come from the petrochemical industry, and the output and cost are largely affected by the oil market. (2) Ethylene method, which consists of two steps: the first step is to oxidize ethylene to ethylene oxide ring; the second step is to react ethylene oxide with methanol to generate ethylene glycol methyl ether through ring-opening etherification reaction. For example, China's invention patent "a method for preparing ethylene glycol monoether from ethylene" (publication number: CN102452908A) uses ethylene, hydrogen peroxide and low-carbon alcohol as raw materials, and produces ethylene glycol monoether in a single step under the action of a catalyst. The raw material ethylene of this method is greatly affected by the supply and demand relationship, which has a certain impact on industrial production. (3) Ethylene glycol method, such as the foreign patent: Method for preparing ethylene glycol ether (publication number: AU2003265407A1) reports a method for preparing ethylene glycol methyl ether using methanol and ethylene glycol as raw materials in the presence of a perfluorocarbon sulfonic acid polymer catalyst; however, the catalyst of this reaction has the disadvantages of being easy to swell, having low mechanical strength, and being easy to deactivate, making it difficult to apply on a large scale.
[0004] In addition, the diethylene glycol method, halogenated hydrocarbon method and synthesis gas method all have certain technical problems and are difficult to apply industrially. Summary of the invention
[0005] Based on the above technical problems, the present invention proposes a method for preparing a catalyst for preparing ethylene glycol methyl ether by hydrogenating dimethyl oxalate.
[0006] A method for preparing a catalyst for preparing ethylene glycol methyl ether by hydrogenating dimethyl oxalate, comprising the following steps: S1. The soluble copper salt, silver salt and soluble additive salt are dissolved in deionized water, mixed and stirred, and aqueous ammonia is added to adjust the pH value to obtain a mixed solution; S2. Weigh a certain amount of silicon source and add it to the mixed solution prepared in step S1, heat and stir in an oil bath at 80 to 130 ° C for 2 to 8 hours to obtain a slurry; S3. The slurry obtained in step S2 is washed, filtered and dried; S4. The solid after drying in step S3 was calcined at 300 to 900 ° C for 3 to 8 hours to obtain a catalyst; S5. tableting, crushing and screening the catalyst obtained in step S4.
[0007] In step S1, the soluble copper salt and the silver salt are one or more of nitrates, acetates, sulfates and chlorides of copper and silver; the soluble auxiliary agent salt is one or more of nitrates, acetates, sulfates and chlorides of Ni, In, B, Zr, Mg, Re, Ru, Rh, Ti, Ce, Ga, Fe, Co, Au, Pd and Mn.
[0008] In step S1, the molar ratio of the soluble copper salt to the silver salt is 0.1-10.
[0009] In step S1, the pH value of the mixed solution is 8-12.
[0010] In step S2, the silicon source is at least one of silica sol, methyl orthosilicate and ethyl orthosilicate.
[0011] In step S2, the silicon source is calculated as SiO2, and the mass ratio of the silicon source solution to the mixed solution is 1:10 to 5:1.
[0012] The prepared catalyst for preparing ethylene glycol methyl ether by hydrogenation of dimethyl oxalate uses SiO2 as a carrier, copper and silver as main active components, and metal M as an auxiliary agent, wherein the mass fractions of Cu and Ag are 3-60%, the mass fraction of the auxiliary metal M is 0.1-20%, and the rest is SiO2.
[0013] The catalyst for preparing ethylene glycol methyl ether by hydrogenation of dimethyl oxalate is used for preparing ethylene glycol methyl ether by catalytic hydrogenation of dimethyl oxalate. The catalyst is evaluated after activation and reduction. The reduction conditions are as follows: the reaction is carried out in a fixed bed microreactor, the prepared catalyst is molded and placed in the fixed bed microreactor, and reduced by a reducing gas. The reducing gas is hydrogen or a mixture of hydrogen and an inert gas, the volume fraction of hydrogen content is 1-100%, the reduction pressure is 1-6.0 MPa, and the volume space velocity of hydrogen or the mixture is 20-2000 h -1 The reduction temperature is 200-700°C, the rate of rising from room temperature to the reduction temperature is 1-10°C / min, and the reduction time is 0.5-24h.
[0014] The catalyst for preparing ethylene glycol methyl ether by hydrogenation of dimethyl oxalate is used for preparing ethylene glycol methyl ether by gas phase catalytic hydrogenation of dimethyl oxalate. Hydrogen and methanol solution of dimethyl oxalate are used as reaction raw materials. The pressure of the reaction system is controlled to be 1-10 MPa. The mass fraction of methanol solution of dimethyl oxalate is 3-70%, and the liquid hourly space velocity is 0.1-5.0 h -1 The reaction temperature is 180-350°C, and the hydrogen-ester molar ratio is 70-400; the product after the reaction is condensed and separated, the liquid product is collected, and the product is quantitatively analyzed by gas chromatography.
[0015] Beneficial effects: 1. High-efficiency catalytic performance: The catalyst obtained by a specific preparation method uses SiO2 as a carrier, copper and silver as the main active components, and other metals as additives. This combination can significantly improve the reaction efficiency of hydrogenating dimethyl oxalate to prepare ethylene glycol methyl ether; 2. Optimized preparation process: The preparation method provided by the present invention includes key steps such as the preparation method of the catalyst, pH adjustment of the solution, the amount and proportion of the silicon source added, the calcination temperature and time, etc. These optimized process parameters can improve the activity and selectivity of the catalyst; 3. Wide range of applications: The prepared catalyst is suitable for the catalytic hydrogenation reaction of dimethyl oxalate and can operate stably within a wide range of reaction conditions (such as temperature, pressure, raw material concentration and space velocity, etc.) to meet the needs of different industrial production; 4. Environmental friendliness and economy: The catalyst and method of the present invention can realize the effective conversion of dimethyl oxalate at low energy consumption and cost, reduce the generation of by-products, and be beneficial to environmental protection and resource conservation; 5. Good stability and life: The catalyst obtained through a special preparation process exhibits excellent stability and a long service life, which is of great significance for reducing production costs and improving production efficiency. DETAILED DESCRIPTION
[0016] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
[0017] Example 1 The steps of the preparation method of the catalyst for preparing ethylene glycol methyl ether by hydrogenation of dimethyl oxalate in this embodiment are as follows: weigh 48.4 g of copper nitrate trihydrate and 17 g of silver nitrate, dissolve them in 100 mL of deionized water, add 100 mL of ammonia water, and stir them thoroughly to dissolve; add 100 mL of silica sol to the solution, heat it to 110° C. and stir it thoroughly for 6 h, age it for 12 h, wash and filter it, dry it at 120° C. for 12 h, and then calcine it at 400° C. for 4 h to obtain the catalyst.
[0018] Catalyst reduction: The prepared catalyst was tableted, crushed, and sieved into 20-40 mesh; 2 mL of catalyst was placed in a fixed bed microreactor and programmed temperature reduction was performed using pure H2 at a heating rate of 2 °C / min and a space velocity of 200 h -1 , the pressure is 2.3MPa.
[0019] Catalyst evaluation: After the catalyst reduction was completed, dimethyl oxalate methanol solution was fed using a micro-metering pump at a mass space velocity of 0.5 h -1 The molar ratio of hydrogen to ester was 230. After the reaction was fully completed, samples were taken every 2 hours and analyzed by gas chromatography to calculate the conversion rate of dimethyl oxalate and the selectivity of ethylene glycol methyl ether. The results are shown in Table 1.
[0020] Example 2 The steps of the preparation method of the catalyst for preparing ethylene glycol methyl ether by hydrogenation of dimethyl oxalate in this embodiment are as follows: weigh 24.2 g of copper nitrate trihydrate, 6.8 g of silver nitrate, and 21.5 g of zirconium nitrate pentahydrate, dissolve in 100 mL of deionized water, add 100 mL of aqueous ammonia, and stir thoroughly to dissolve; add 100 mL of silica sol to the solution, heat to 110° C. and stir thoroughly for 6 h, age for 12 h, wash and filter, dry at 120° C. for 12 h, and then calcine at 400° C. for 4 h to obtain the catalyst.
[0021] Catalyst reduction and catalyst evaluation conditions: the same as in Example 1. The results are shown in Table 1.
[0022] Example 3 Weigh 24.2 g of copper nitrate trihydrate, 8.35 g of silver acetate, and 2.91 g of nickel nitrate pentahydrate, dissolve in 100 mL of deionized water, add 100 mL of aqueous ammonia, and stir thoroughly to dissolve; add 100 mL of silica sol to the solution, heat to 110°C, stir thoroughly for 6 hours, age for 12 hours, wash and filter, dry at 120°C for 12 hours, and then calcine at 400°C for 4 hours to obtain a catalyst.
[0023] Catalyst reduction and catalyst evaluation conditions: the same as in Example 1. The results are shown in Table 1.
[0024] Example 4 Weigh 24.2 g of copper nitrate trihydrate, 8.35 g of silver acetate, and 4.34 g of cerium nitrate hexahydrate, dissolve in 100 mL of deionized water, add 100 mL of aqueous ammonia, and stir thoroughly to dissolve; add 100 mL of silica sol to the solution, heat to 110°C, stir thoroughly for 6 hours, age for 12 hours, wash and filter, dry at 120°C for 12 hours, and then calcine at 400°C for 4 hours to obtain a catalyst.
[0025] Catalyst reduction and catalyst evaluation conditions: the same as in Example 1. The results are shown in Table 1.
[0026] Example 5 Weigh 18.1 g of copper acetate monohydrate, 8.35 g of silver acetate, and 14.9 g of zinc nitrate, dissolve in 100 mL of deionized water, add 100 mL of aqueous ammonia, and stir thoroughly to dissolve; add 100 mL of silica sol to the solution, heat to 110°C, stir thoroughly for 6 hours, age for 12 hours, wash and filter, dry at 120°C for 12 hours, and then calcine at 400°C for 4 hours to obtain a catalyst.
[0027] Catalyst reduction and catalyst evaluation conditions: the same as in Example 1. The results are shown in Table 1.
[0028] Example 6 Weigh 18.1 g of copper acetate monohydrate, 8.35 g of silver acetate, and 7.45 g of NH4OH, dissolve them in 100 mL of deionized water, add 100 mL of aqueous ammonia, and stir thoroughly to dissolve; add 100 mL of silica sol to the solution, heat to 110 ° C, stir thoroughly for 6 h, age for 12 h, wash and filter, dry at 120 ° C for 12 h, and then calcine at 400 ° C for 4 h to obtain a catalyst.
[0029] Catalyst reduction and catalyst evaluation conditions: the same as in Example 1. The results are shown in Table 1.
[0030] Example 7 The steps of the preparation method of the catalyst for preparing ethylene glycol methyl ether by hydrogenation of dimethyl oxalate in this embodiment are as follows: weigh 24.2 g of copper nitrate trihydrate, 6.8 g of silver nitrate, and 17.9 g of manganese nitrate, dissolve them in 100 mL of deionized water, add 100 mL of ammonia water, and stir them thoroughly to dissolve; add 100 mL of silica sol to the solution, heat it to 110° C. and stir it thoroughly for 6 h, age it for 12 h, wash and filter it, dry it at 120° C. for 12 h, and then calcine it at 400° C. for 4 h to obtain the catalyst.
[0031] Catalyst reduction and catalyst evaluation conditions: the same as in Example 1. The results are shown in Table 1.
[0032] Example 8 The steps of the preparation method of the catalyst for preparing ethylene glycol methyl ether by hydrogenation of dimethyl oxalate in this embodiment are as follows: weigh 24.2 g of copper nitrate trihydrate, 6.8 g of silver nitrate, and 12.8 g of gallium nitrate, dissolve them in 100 mL of deionized water, add 100 mL of ammonia water, and stir well to dissolve; add 100 mL of silica sol to the solution, heat to 110° C. and stir well for 6 h, age for 12 h, wash and filter, dry at 120° C. for 12 h, and then calcine at 400° C. for 4 h to obtain the catalyst.
[0033] Catalyst reduction and catalyst evaluation conditions: the same as in Example 1. The results are shown in Table 1.
[0034] Example 9 The steps of the preparation method of the catalyst for preparing ethylene glycol methyl ether by hydrogenation of dimethyl oxalate in this embodiment are as follows: weigh 24.2 g of copper nitrate trihydrate, 6.8 g of silver nitrate, and 14.55 g of cobalt nitrate hexahydrate, dissolve them in 100 mL of deionized water, add 100 mL of ammonia water, and stir well to dissolve; add 100 mL of silica sol to the solution, heat to 110° C. and stir well for 6 h, age for 12 h, wash and filter, dry at 120° C. for 12 h, and then calcine at 400° C. for 4 h to obtain the catalyst.
[0035] Catalyst reduction and catalyst evaluation conditions: the same as in Example 1. The results are shown in Table 1.
[0036] Table 1 Evaluation results of catalysts in the examples Example DMO conversion rate / % Ethanol selectivity / % Ethylene glycol methyl ether selectivity / % Methyl glycolate selectivity / % Ethylene glycol selectivity / % Example 1 99.47 2.80 69.06 25.02 3.07 Example 2 99.81 4.62 69.57 22.37 2.88 Example 3 99.79 4.28 67.26 23.54 4.85 Example 4 99.61 2.91 65.86 28.09 3.09 Example 5 99.50 2.79 67.22 27.38 2.39 Example 6 98.91 2.80 66.12 28.02 3.07 Example 7 99.51 2.72 67.02 26.90 3.19 Example 8 100.00 3.90 59.24 27.35 8.75 Example 9 99.49 2.76 66.04 28.37 2.18 As can be seen from Table 1, the catalyst has a very high conversion rate for DMO and excellent selectivity for ethylene glycol methyl ether and methyl glycolate, showing good application prospects.
[0037] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a catalyst for preparing ethylene glycol methyl ether by hydrogenating dimethyl oxalate, characterized in that: Here are the steps: S1. The soluble copper salt, silver salt and soluble additive salt are dissolved in deionized water, mixed and stirred, and aqueous ammonia is added to adjust the pH value to obtain a mixed solution; S2. Weigh a certain amount of silicon source and add it to the mixed solution prepared in step S1, heat and stir in an oil bath at 80 to 130 ° C for 2 to 8 hours to obtain a slurry; S3. The slurry obtained in step S2 is washed, filtered and dried; S4. The solid after drying in step S3 was calcined at 300 to 900 ° C for 3 to 8 hours to obtain a catalyst; S5. tableting, crushing and screening the catalyst obtained in step S4.
2. The method for preparing a catalyst for preparing ethylene glycol methyl ether by hydrogenating dimethyl oxalate according to claim 1, characterized in that: In step S1, the soluble copper salt and the silver salt are one or more of nitrates, acetates, sulfates and chlorides of copper and silver; the soluble auxiliary agent salt is one or more of nitrates, acetates, sulfates and chlorides of Ni, In, B, Zr, Mg, Re, Ru, Rh, Ti, Ce, Ga, Fe, Co, Au, Pd and Mn.
3. The method for preparing a catalyst for preparing ethylene glycol methyl ether by hydrogenating dimethyl oxalate according to claim 1, characterized in that: In step S1, the molar ratio of the soluble copper salt to the silver salt is 0.1-10.
4. The method for preparing a catalyst for preparing ethylene glycol methyl ether by hydrogenating dimethyl oxalate according to claim 1, characterized in that: In step S1, the pH value of the mixed solution is 8-12.
5. The method for preparing a catalyst for preparing ethylene glycol methyl ether by hydrogenating dimethyl oxalate according to claim 1, characterized in that: In step S2, the silicon source is at least one of silica sol, methyl orthosilicate and ethyl orthosilicate.
6. The method for preparing the catalyst for preparing ethylene glycol methyl ether by hydrogenation of dimethyl oxalate according to claim 5, characterized in that: In step S2, the silicon source is calculated as SiO2, and the mass ratio of the silicon source to the mixed solution is 1:10 to 5:
1.
7. A catalyst for preparing ethylene glycol methyl ether by hydrogenating dimethyl oxalate obtained by any preparation method according to claim 1, wherein SiO2 is used as a carrier, copper and silver are used as main active components, and metal M is used as an auxiliary agent, wherein: The mass fraction of Cu and Ag is 3~60%, the mass fraction of the auxiliary metal M is 0.1~20%, and the rest is SiO2.
8. The catalyst for preparing ethylene glycol methyl ether by hydrogenation of dimethyl oxalate according to claim 7 is used for preparing ethylene glycol methyl ether by catalytic hydrogenation reaction of dimethyl oxalate, characterized in that: The reaction is carried out in a fixed bed microreactor. The prepared catalyst is formed and placed in the fixed bed microreactor, and reduced using a reducing gas. The reducing gas is hydrogen or a mixture of hydrogen and an inert gas, the hydrogen content volume fraction is 1-100%, the reduction pressure is 1-6.0 MPa, and the volume space velocity of hydrogen or the mixture is 20-2000 h -1 The reduction temperature is 200-700°C, the rate of rising from room temperature to the reduction temperature is 1-10°C / min, and the reduction time is 0.5-24h.
9. The catalyst for preparing ethylene glycol methyl ether by hydrogenation of dimethyl oxalate according to claim 7 is used for preparing ethylene glycol methyl ether by gas phase catalytic hydrogenation reaction of dimethyl oxalate, characterized in that: Hydrogen and methanol solution of dimethyl oxalate were used as the reaction raw materials. The pressure of the reaction system was controlled to be 1-10 MPa. The mass fraction of dimethyl oxalate methanol solution was 3-70%, and the liquid hourly space velocity was 0.1-5.0 h -1 , the reaction temperature is 180~350℃, and the hydrogen ester molar ratio is 70~400.
Citation Information
Patent Citations
Glycol catalyst prepared by dimethyl oxalate hydrogenation and preparation method thereof
CN101607205A
Catalyst for hydrogenation of dimethyl oxalate to prepare methyl glycolate, preparation method and application thereof
CN101954288A
Copper-based catalyst for preparing ethylene glycol and ethylene glycol monomethyl ether through hydrogenation of dimethyl oxalate and preparation method thereof
CN103566949A
Catalyst for preparing ethylene glycol monomethyl ether by hydrogenation of dimethyl oxalate and methyl alcohol and process
CN103816915A
Preparation method and application of supported catalyst for catalyzing hydrogenation of dimethyl oxalate
CN111774050A