Catalytic cracking catalyst, preparation method thereof and catalytic cracking method

By modifying the hollow ZSM-5 hierarchical pore molecular sieve, nano-molecular sieve and Y-type molecular sieve compound catalyst, the problem of low conversion efficiency of light and heavy components of full distillate oil in the existing technology has been solved, and the yield and yield of low-carbon olefins have been improved. Catalytic cracking efficiency.

CN118767979AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310334647.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-15
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

It is difficult for existing catalysts to efficiently convert the light and heavy components in the full distillate oil in the same reaction system, resulting in a low yield of low-carbon olefins.

Method used

Modified hollow ZSM-5 multi-stage pore molecular sieve, nano-molecular sieve and Y-type molecular sieve are used as catalysts, combined with phosphorus and metal components, to optimize the pore structure and acidic performance of the molecular sieve, and are used for catalysis of full distillate oil or intermediate heavy oil. lysis.

Benefits of technology

The yield and catalytic cracking efficiency of light olefins are significantly improved, and efficient conversion of light and heavy components is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118767979A_ABST
    Figure CN118767979A_ABST
Patent Text Reader

Abstract

The invention relates to a catalytic cracking catalyst, a preparation method thereof and a catalytic cracking method, and the catalytic cracking method comprises the following steps: raw oil is contacted with the catalytic cracking catalyst for reaction, the raw oil is full distillate oil or intermediate heavy oil, and the intermediate heavy oil is a low-carbon heavy oil or a low-carbon heavy oil; the catalytic cracking catalyst contains a modified hollow ZSM-5 hierarchical pore molecular sieve, a nano molecular sieve, a Y-type molecular sieve and a carrier. The catalytic cracking method disclosed by the invention has higher yield of low-carbon olefins.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a catalytic cracking catalyst and a preparation method thereof and a catalytic cracking method. Background Art

[0002] Low-carbon olefins represented by ethylene and propylene are important basic organic chemical raw materials and are known as the cornerstone of the modern chemical industry. There are many technologies for producing low-carbon olefins using catalytic cracking or catalytic cracking units at home and abroad, but the process of directly catalytically cracking crude oil into small-molecule olefins is rarely reported. Since the molecular cracking performance of reactants in different fractions of full-fraction crude oil is significantly different, although the crude oil can be simply cut first to change the feed position of light and heavy components, thereby changing the reaction conditions of light and heavy fractions, the biggest challenge is to achieve efficient conversion of light and heavy components in the same catalytic reaction system using the same catalyst.

[0003] Catalytic cracking of heavy oil is based on catalytic cracking, using catalysts that can produce more light olefins and appropriately adjusting reaction conditions such as increasing the reaction temperature to convert heavy oil under more severe conditions. Catalytic cracking catalysts are key factors affecting catalytic cracking of heavy oil. According to the hydrocarbon composition, petroleum is generally divided into paraffinic, intermediate, and cycloalkyl. In fact, all crude oils are a mixture of paraffinic and cycloalkyl. If the content of the two is roughly equal, it is called intermediate crude oil. Intermediate heavy oil is a type of oil product with properties between paraffinic heavy oil and cycloalkyl heavy oil. Its alkane and cycloalkane contents are basically similar, so the catalysts required to achieve satisfactory processing results are often different.

[0004] In the catalysts for producing light olefins, ZSM-5 molecular sieves with MFI topology and β molecular sieves with BEA topology are usually used. Although ZSM-5 molecular sieves have shape-selective function, their pore size is small, which is not conducive to the diffusion and adsorption of macromolecular reactants, especially cyclic hydrocarbons, resulting in low light olefin yields. Summary of the invention

[0005] The purpose of the present disclosure is to provide a catalytic cracking catalyst and a preparation method thereof and a catalytic cracking method, which can achieve efficient conversion of full-fraction oil or intermediate base heavy oil by using one catalyst and significantly improve the yield of light olefins.

[0006] In order to achieve the above-mentioned object, the first aspect of the present disclosure provides a catalytic cracking method, which comprises: contacting a feedstock oil with a catalytic cracking catalyst for reaction, wherein the feedstock oil is a full-fraction oil or an intermediate base heavy oil, and the catalytic cracking catalyst comprises a modified hollow ZSM-5 multi-level pore molecular sieve, a nano molecular sieve, a Y-type molecular sieve and a carrier;

[0007] Based on the dry weight of the catalytic cracking catalyst, the content of the modified hollow ZSM-5 multi-level pore molecular sieve is 15-40% by weight, the content of the nano molecular sieve is 1-10% by weight, the content of the Y-type molecular sieve is 5-15% by weight, and the content of the carrier is 40-80% by weight;

[0008] The modified hollow ZSM-5 multi-level pore molecular sieve contains a molecular sieve and phosphorus and metal components loaded on the molecular sieve; the phosphorus-aluminum molar ratio of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.1-1.5; the content of the metal component is 0.1-5% by weight based on the oxide of the metal component and the dry basis weight of the modified hollow ZSM-5 multi-level pore molecular sieve; the modified hollow ZSM-5 multi-level pore molecular sieve has a closed hollow structure, the average grain size of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.2-3.0 μm, and the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.0-1.5; the total specific surface area of ​​the modified hollow ZSM-5 multi-level pore molecular sieve is 250-350 m 2 / g, mesopore specific surface area is 20-100m 2 / g, the mesoporous specific surface area accounts for 15-40% of the total specific surface area, the strong B acid content accounts for 55-70% of the total B acid content, and the strong L acid content accounts for 50-70% of the total L acid content;

[0009] The pore size of the nano molecular sieve is 0.56-0.75 nm.

[0010] Optionally, the feedstock oil is a full-fraction oil, and the reaction conditions include: a reaction temperature of 550-600°C; based on the dry weight of the catalytic cracking catalyst, the content of the modified hollow ZSM-5 multi-level pore molecular sieve is 20-40% by weight, the content of the nano molecular sieve is 1-5% by weight, the content of the Y-type molecular sieve is 5-15% by weight, and the content of the carrier is 40-80% by weight.

[0011] Optionally, the feedstock oil is intermediate base heavy oil, and the reaction conditions include: a reaction temperature of 550-600°C; based on the dry weight of the catalytic cracking catalyst, the content of the modified hollow ZSM-5 multi-level pore molecular sieve is 15-30% by weight, the content of the nano molecular sieve is 5-10% by weight, the content of the Y-type molecular sieve is 5-10% by weight, and the content of the carrier is 50-75% by weight.

[0012] In a second aspect of the present disclosure, a catalytic cracking catalyst is provided, the catalytic cracking catalyst comprising a modified hollow ZSM-5 multi-level pore molecular sieve, a nano molecular sieve, a Y-type molecular sieve and a carrier, wherein, based on the dry weight of the catalytic cracking catalyst, the content of the modified hollow ZSM-5 multi-level pore molecular sieve is 15-40% by weight, the content of the nano molecular sieve is 1-10% by weight, the content of the Y-type molecular sieve is 5-15% by weight, and the content of the carrier is 40-80% by weight;

[0013] The modified hollow ZSM-5 multi-level pore molecular sieve contains a molecular sieve and phosphorus and metal components loaded on the molecular sieve; the phosphorus-aluminum molar ratio of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.1-1.5; the content of the metal component is 0.1-5% by weight based on the oxide of the metal component and the dry basis weight of the modified hollow ZSM-5 multi-level pore molecular sieve; the modified hollow ZSM-5 multi-level pore molecular sieve has a closed hollow structure, the average grain size of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.2-3.0 μm, and the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.0-1.5; the total specific surface area of ​​the modified hollow ZSM-5 multi-level pore molecular sieve is 250-350 m 2 / g, mesopore specific surface area is 20-100m 2 / g, the mesoporous specific surface area accounts for 15-40% of the total specific surface area, the strong B acid content accounts for 55-70% of the total B acid content, and the strong L acid content accounts for 50-70% of the total L acid content;

[0014] The pore size of the nano molecular sieve is 0.56-0.75 nm.

[0015] Optionally, the phosphorus to aluminum molar ratio of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.2-1.3;

[0016] The content of the metal component is 0.5-4% by weight, calculated as the oxide of the metal component and based on the dry weight of the modified hollow ZSM-5 multi-level pore molecular sieve.

[0017] Optionally, the average grain size of the modified hollow ZSM-5 multi-level pore molecular sieve grains is 0.5-3.0 μm, the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.0-1.3, and the relative crystallinity is 80-90%.

[0018] Optionally, the total specific surface area of ​​the modified hollow ZSM-5 multi-level pore molecular sieve is 260-340m 2 / g, mesopore specific surface area is 25-100m 2 / g, and the mesoporous specific surface area accounts for 18-35% of the total specific surface area.

[0019] Optionally, the metal component is selected from one or more of lanthanum, cerium, tungsten, iron, cobalt, nickel, copper, manganese, zinc, tin, bismuth and gallium;

[0020] The nano molecular sieve is one or more of the molecular sieves having the structures of AET, AFR, AFS, AFI, BEA, BOG, CFI, CON, GME, IFR, ISV, LTL, MEI, MOR, OFF and SAO; preferably at least one of Beta, SAPO-5, SAPO-40, SSZ-13, CIT-1, ITQ-7, ZSM-18, mordenite and gmelinite;

[0021] The Y-type molecular sieve is one or more selected from REY molecular sieve, DASY molecular sieve, USY molecular sieve, phosphorus-containing DASY molecular sieve, phosphorus-containing USY molecular sieve, PSRY molecular sieve, HRY molecular sieve, HSY molecular sieve, SCY molecular sieve, and RSCY molecular sieve.

[0022] Optionally, the carrier is selected from one or more of natural clay, alumina carrier, silica carrier, aluminum phosphate carrier and silica-alumina carrier;

[0023] Preferably, the silica carrier is one or more of neutral silica sol, acidic silica sol or alkaline silica sol; the alumina carrier is one or more of aluminum sol, acidified pseudo-boehmite, hydrated alumina and activated alumina; the aluminum phosphate carrier is phosphate aluminum gel; the silica aluminum oxide carrier is one or more of solid silica aluminum material, silica aluminum sol and silica aluminum gel.

[0024] Optionally, the carrier comprises a silicon oxide carrier; the content of the silicon oxide carrier in terms of SiO2 is 1-20 wt % based on the dry weight of the catalytic cracking catalyst.

[0025] The third aspect of the present disclosure provides a method for preparing the catalytic cracking catalyst described in the second aspect of the present disclosure, the method comprising: drying and optionally calcining a slurry containing a carrier, a modified hollow ZSM-5 multi-level pore molecular sieve, a nano molecular sieve, a Y-type molecular sieve and water.

[0026] Optionally, the preparation steps of the modified hollow ZSM-5 multi-level pore molecular sieve include:

[0027] Mixing a first solution containing a first phosphorus source and a first metal source with a hollow ZSM-5 multi-level pore molecular sieve raw material, and performing a first drying and a first calcination on the obtained first slurry, wherein the weight ratio of the first solution to the hollow ZSM-5 multi-level pore molecular sieve raw material is 1:(0.5-2.0);

[0028] Alternatively, the preparation steps of the modified hollow ZSM-5 multi-level pore molecular sieve include:

[0029] S1, mixing a second solution containing a second phosphorus source with a hollow ZSM-5 multi-level pore molecular sieve raw material, and performing a second drying and a second calcination on the obtained second slurry to obtain a first solid product; wherein the weight ratio of the second solution containing the second phosphorus source to the hollow ZSM-5 multi-level pore molecular sieve raw material is 1: (0.5-2.0);

[0030] S2, subjecting the first solid product to hydrothermal treatment to obtain a second solid product;

[0031] S3. Mixing a third solution containing a second metal source with the second solid product, and performing a third drying and a third calcination on the obtained third slurry, wherein the weight ratio of the third solution containing the second metal source to the second solid product is 1:(0.5-2.0).

[0032] Optionally, the first phosphorus source and the second phosphorus source are each independently selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate and ammonium phosphate;

[0033] The first metal source and the second metal source are each independently selected from one or more of metal nitrates, chlorides and sulfates, and the metal is selected from one or more of lanthanum, cerium, tungsten, iron, cobalt, nickel, copper, manganese, zinc, tin, bismuth and gallium;

[0034] The hollow ZSM-5 multi-level pore molecular sieve raw material is an H-type hollow ZSM-5 multi-level pore molecular sieve.

[0035] Optionally, the conditions of the hydrothermal treatment include: a temperature of 400-800° C. and a time of 1-12 hours;

[0036] The conditions of the first drying, the second drying and the third drying independently include: a temperature of 90-120° C. and a time of 2-24 hours;

[0037] The conditions of the first calcination, the second calcination and the third calcination independently include: a temperature of 450-600° C. and a time of 2-6 hours.

[0038] Through the above technical scheme, the present invention adopts a modified hollow ZSM-5 multi-level pore molecular sieve and a composite of a nano molecular sieve and a Y-type molecular sieve as the main active component of the catalyst. Using it in the catalytic cracking of full-fraction oil or intermediate base heavy oil can achieve efficient conversion of multiple components and improve the yield of the target product.

[0039] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:

[0041] Figure 1 is a SEM photograph of the phosphorus hollow ZSM-5 multi-level pore molecular sieve prepared in Example 1 of the present disclosure;

[0042] Figure 2 is a SEM photograph of the phosphorus hollow ZSM-5 multi-level pore molecular sieve prepared in Example 2 of the present disclosure;

[0043] Figure 3 is a SEM photograph of the nanomolecular sieve in Examples 4-6 of the present disclosure;

[0044] Figure 4 This is a SEM photograph of the Y-type molecular sieve in Examples 4-6 of the present disclosure. DETAILED DESCRIPTION

[0045] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.

[0046] In a first aspect of the present disclosure, a catalytic cracking method is provided, the method comprising: contacting a crude oil with a catalytic cracking catalyst for reaction, wherein the crude oil is a full-fraction oil or an intermediate base heavy oil, and the catalytic cracking catalyst contains a modified hollow ZSM-5 multi-level pore molecular sieve, a nano molecular sieve, a Y-type molecular sieve and a carrier.

[0047] Wherein, based on the dry weight of the catalytic cracking catalyst, the content of the modified hollow ZSM-5 multi-level pore molecular sieve is 15-40% by weight, the content of the nano molecular sieve is 1-10% by weight, the content of the Y-type molecular sieve is 5-15% by weight, and the content of the carrier is 40-80% by weight; the modified hollow ZSM-5 multi-level pore molecular sieve contains a molecular sieve and phosphorus and metal components loaded on the molecular sieve; the phosphorus-aluminum molar ratio of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.1-1.5 ; The content of the metal component is 0.1-5 wt % based on the oxide of the metal component and the dry basis weight of the modified hollow ZSM-5 multi-level pore molecular sieve; the modified hollow ZSM-5 multi-level pore molecular sieve has a closed hollow structure, the average grain size of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.2-3.0 μm, and the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.0-1.5; the total specific surface area of ​​the modified hollow ZSM-5 multi-level pore molecular sieve is 250-350 m 2 / g, mesopore specific surface area is 20-100m 2 / g, the mesoporous specific surface area accounts for 15-40% of the total specific surface area, the strong B acid content accounts for 55-70% of the total B acid content, and the strong L acid content accounts for 50-70% of the total L acid content; the pore size of the nano molecular sieve is 0.56-0.75nm.

[0048] In a specific embodiment of the present disclosure, the feedstock oil is a whole distillate oil, and the reaction conditions include: a reaction temperature of 550-600°C; based on the dry weight of the catalytic cracking catalyst, the content of the modified hollow ZSM-5 multi-level pore molecular sieve is 20-40% by weight, the content of the nano molecular sieve is 1-5% by weight, the content of the Y-type molecular sieve is 5-15% by weight, and the content of the carrier is 40-80% by weight. The whole distillate oil catalytic cracking method disclosed in the present disclosure uses a special catalyst containing a modified hollow ZSM-5 multi-level pore molecular sieve, which can achieve efficient conversion of light and heavy components and improve the yield of the target product.

[0049] In another specific embodiment of the present disclosure, the feedstock oil is an intermediate base heavy oil, and the reaction conditions include: a reaction temperature of 550-600°C; based on the dry weight of the catalytic cracking catalyst, the content of the modified hollow ZSM-5 multi-level pore molecular sieve is 15-30% by weight, the content of the nano molecular sieve is 5-10% by weight, the content of the Y-type molecular sieve is 5-10% by weight, and the content of the carrier is 50-75% by weight. The intermediate base heavy oil catalytic cracking method disclosed in the present disclosure uses a special catalyst containing a modified hollow ZSM-5 multi-level pore molecular sieve, which can achieve efficient conversion of multiple components of alkanes and cycloalkanes and improve the yield of the target product.

[0050] In a second aspect of the present disclosure, the above-mentioned catalytic cracking catalyst is provided, which contains a modified hollow ZSM-5 multi-level pore molecular sieve, a nano molecular sieve, a Y-type molecular sieve and a carrier. Based on the dry weight of the catalytic cracking catalyst, the content of the modified hollow ZSM-5 multi-level pore molecular sieve is 15-40% by weight, the content of the nano molecular sieve is 1-10% by weight, the content of the Y-type molecular sieve is 5-15% by weight, and the content of the carrier is 40-80% by weight; the modified hollow ZSM-5 multi-level pore molecular sieve contains a molecular sieve and phosphorus and metal components loaded on the molecular sieve; The phosphorus-aluminum molar ratio of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.1-1.5; the content of the metal component is 0.1-5% by weight, calculated as the oxide of the metal component and based on the dry basis weight of the modified hollow ZSM-5 multi-level pore molecular sieve; the modified hollow ZSM-5 multi-level pore molecular sieve has a closed hollow structure, the average grain size of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.2-3.0 μm, and the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.0-1.5; the total specific surface area of ​​the modified hollow ZSM-5 multi-level pore molecular sieve is 250-350 m 2 / g, mesopore specific surface area is 20-100m 2 / g, the mesoporous specific surface area accounts for 15-40% of the total specific surface area, the strong B acid content accounts for 55-70% of the total B acid content, and the strong L acid content accounts for 50-70% of the total L acid content; the pore size of the nano molecular sieve is 0.56-0.75nm.

[0051] The catalytic cracking catalyst disclosed in the present invention contains a modified hollow ZSM-5 multi-level pore molecular sieve, which has a multi-level pore structure of micropores-mesopores-mesopores, can provide multi-directional diffusion paths, expand confined space, improve the accessibility of active centers, and optimize the diffusion performance of molecular sieves. It also contains phosphorus and metal components to further effectively modify active sites, and compound nano molecular sieves and Y-type molecular sieves. Using them in the catalytic cracking of full-fraction oil or intermediate base heavy oil can effectively increase the yield of light olefins.

[0052] In a specific embodiment of the present disclosure, the phosphorus-aluminum molar ratio (in terms of P / Al) of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.2-1.3; the content of the metal component is 0.5-4% by weight, based on the oxide of the metal component and the dry weight of the metal-modified hollow ZSM-5 multi-level pore molecular sieve composite material. In the present disclosure, the phosphorus-aluminum molar ratio of the modified hollow ZSM-5 multi-level pore molecular sieve is obtained by XRF fluorescence detection, and the content of the metal component is obtained by XRF fluorescence detection.

[0053] In a specific embodiment of the present disclosure, the average grain size of the modified hollow ZSM-5 multi-level pore molecular sieve grains is 0.5-3.0 μm, the ratio of the bulk silicon-aluminum molar ratio (in terms of SiO2 / Al2O3) to the surface silicon-aluminum molar ratio (in terms of SiO2 / Al2O3) is 1.0-1.3, and the relative crystallinity is 80-90%. In the present disclosure, the grain size refers to the size of the widest part of the grain, which can be obtained by measuring the size of the widest part of the grain projection surface in the SEM or TEM image of the sample, and the average grain size is obtained by selecting any 10 molecular sieves in the SEM or TEM image and calculating their average value. The bulk silicon-aluminum molar ratio refers to the silicon-aluminum molar ratio of the entire ZSM-5 nanocrystalline material, which is determined by the XRF method, and the surface silicon-aluminum molar ratio is determined by the XPS method. The specific test method is well known to those skilled in the art and will not be repeated here. The bulk silicon-aluminum molar ratio is 15-200. In the present disclosure, the relative crystallinity of the molecular sieve is based on the XRD standard ZSM-5 molecular sieve standard sample of the China Petroleum and Chemical Research Institute, and the crystallinity of the standard sample is regarded as 100%.

[0054] In a specific embodiment of the present disclosure, the total specific surface area of ​​the modified hollow ZSM-5 multi-level pore molecular sieve is 260-340m 2 / g, mesopore specific surface area is 25-100m 2 / g, the mesopore specific surface area accounts for 18-35% of the total specific surface area, and the N2 adsorption-desorption curve presents an H4-type hysteresis loop. In the present disclosure, the total specific surface area and the mesopore specific surface area are obtained by BET analysis.

[0055] In a specific embodiment of the present disclosure, the strong B acid content accounts for 55-68% of the total B acid content, and the strong L acid content accounts for 50-65% of the total L acid content. The strong B acid content and the total B acid content are prepared by a pyridine infrared acid method, and the strong L acid content and the total L acid content are prepared by a pyridine infrared acid method.

[0056] According to the present disclosure, the metal component is selected from one or more of Group VIIB metals, Group VIII metals and Group IIIB metals, Group IIIA metals and Group IIB metals. In a specific embodiment of the present invention, the metal component is selected from one or more of lanthanum, cerium, tungsten, iron, cobalt, nickel, copper, manganese, zinc, tin, bismuth and gallium.

[0057] According to the present disclosure, the nano molecular sieve can be one or more of the molecular sieves having AET, AFR, AFS, AFI, BEA, BOG, CFI, CON, GME, IFR, ISV, LTL, MEI, MOR, OFF and SAO structures; preferably at least one of Beta, SAPO-5, SAPO-40, SSZ-13, CIT-1, ITQ-7, ZSM-18, mordenite and sodium chabazite.

[0058] According to the present disclosure, the Y-type molecular sieve can be a Y-type molecular sieve that is hydrothermally ultrastable or gas-phase ultrastable. The Y-type molecular sieve may contain rare earth or not contain rare earth, specifically, the rare earth content of the Y-type molecular sieve is 0-25% by weight in terms of rare earth element oxide (RE2O3), and the rare earth element may be lanthanum and / or cerium; the Y-type molecular sieve may contain phosphorus or not contain phosphorus, specifically, the phosphorus content of the Y-type molecular sieve is 0-10% by weight in terms of P2O5. The Y-type molecular sieve may be selected from one or more of REY molecular sieve, DASY molecular sieve, USY molecular sieve, phosphorus-containing DASY molecular sieve, phosphorus-containing USY molecular sieve, PSRY molecular sieve, HRY molecular sieve, HSY molecular sieve, SCY molecular sieve, and RSCY molecular sieve.

[0059] According to the present disclosure, the carrier is selected from one or more of natural clay, alumina carrier, silica carrier, aluminum phosphate carrier and silica-alumina oxide carrier. In one embodiment, the silica carrier is one or more of neutral silica sol, acidic silica sol or alkaline silica sol; the alumina carrier is one or more of aluminum sol, acidified pseudo-boehmite, hydrated alumina and activated alumina; the aluminum phosphate carrier is phosphate aluminum gel; the silica-alumina oxide carrier is one or more of solid silica-alumina material, silica-alumina sol and silica-alumina gel.

[0060] In a specific embodiment of the present disclosure, the carrier comprises a silicon oxide carrier; based on the dry weight of the catalytic cracking catalyst, the content of the silicon oxide carrier in terms of SiO2 is 1-20 wt%.

[0061] In a specific embodiment of the present disclosure, based on the dry weight of the catalytic cracking catalyst, the catalytic cracking catalyst contains 20-40 wt% of modified hollow ZSM-5 multi-level pore molecular sieve, 1-5 wt% of nano molecular sieve, 5-15 wt% of Y-type molecular sieve, 20-60 wt% such as 25-50 wt% of clay, 5-35 wt% such as 10-30 wt% of acidified pseudo-boehmite, 3-25 wt% such as 5-15 wt% or 3-20 wt% of aluminum sol and 0-15 wt% such as 3-10 wt% or 5-15 wt% of silica sol.

[0062] In a specific embodiment of the present disclosure, based on the dry weight of the catalytic cracking catalyst, the content of sodium oxide in the catalytic cracking catalyst is preferably less than 0.15 wt %.

[0063] The third aspect of the present disclosure provides a method for preparing the above-mentioned catalytic cracking catalyst, which comprises: drying and optionally calcining a slurry containing a carrier, a modified hollow ZSM-5 multi-level pore molecular sieve, a nano molecular sieve, a Y-type molecular sieve and water. The present disclosure does not limit the specific form of the drying, which can be conventionally adopted by those skilled in the art. In a preferred embodiment, the drying is spray drying, which can have a molding effect on the catalyst while drying the material. Spray drying is well known to those skilled in the art, and the specific method will not be repeated here.

[0064] In a specific embodiment of the present disclosure, the preparation step of the modified hollow ZSM-5 multi-level pore molecular sieve includes: mixing a first solution containing a first phosphorus source and a first metal source with a hollow ZSM-5 multi-level pore molecular sieve raw material, and performing a first drying and a first calcination on the obtained first slurry, wherein the weight ratio of the first solution to the hollow ZSM-5 multi-level pore molecular sieve raw material is 1: (0.5-2.0). In a preferred specific embodiment, the step includes: dropping the first solution containing the first phosphorus source and the first metal source into the flat hollow ZSM-5 multi-level pore molecular sieve raw material, so that the molecular sieve raw material is in a "viscous paste".

[0065] According to the present disclosure, the weight ratio of the first solution to the hollow ZSM-5 multi-level pore molecular sieve raw material can vary within a large range, for example, it can be 1: (0.5-2.0), preferably 1: (0.8-1.5).

[0066] In another embodiment, the preparation steps of the modified hollow ZSM-5 multi-level pore molecular sieve include: S1, mixing a second solution containing a second phosphorus source with a hollow ZSM-5 multi-level pore molecular sieve raw material, and performing a second drying and a second calcination on the obtained second slurry to obtain a first solid product, wherein the weight ratio of the second solution containing the second phosphorus source to the hollow ZSM-5 multi-level pore molecular sieve raw material is 1: (0.5-2.0), and the second solution containing the second phosphorus source is measured in P; S2, hydrothermally treating the first solid product to obtain a second solid product; S3, mixing a third solution containing a second metal source with the second solid product, and performing a third drying and a third calcination on the obtained third slurry, wherein the weight ratio of the third solution containing the second metal source to the second solid product is 1: (0.5-2.0), and the third solution containing the second metal source is measured in metal oxide. In a preferred embodiment, step S1 comprises: dropping a second solution containing a second phosphorus source into a flat hollow ZSM-5 multi-level pore molecular sieve raw material, so that the molecular sieve raw material is in a "viscous paste state".

[0067] According to the present disclosure, the first phosphorus source and the second phosphorus source are independently selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate and ammonium phosphate; the first metal source and the second metal source are independently selected from one or more of metal nitrates, chlorides and sulfates, and the metal can be selected from one or more of Group VIIB metals, Group VIII metals and Group IIIB metals, Group IIIA metals, and Group IIB metals, preferably one or more of lanthanum, cerium, tungsten, iron, cobalt, nickel, copper, manganese, zinc, tin, bismuth and gallium; the hollow ZSM-5 multi-level pore molecular sieve raw material can be purchased from commercial sources or prepared by itself. In one embodiment, the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio of the hollow ZSM-5 multi-level pore molecular sieve raw material can be 1.0-1.5, and the total specific surface area can be 340-420m 2 / g, the mesopore specific surface area can be 15-150m 2 / g; preferably, the hollow ZSM-5 multi-level pore molecular sieve raw material is an H-type hollow ZSM-5 multi-level pore molecular sieve, and the sodium oxide content of the H-type hollow ZSM-5 multi-level pore molecular sieve is less than 0.1% by weight.

[0068] According to the present disclosure, hydrothermal treatment is well known to those skilled in the art, and can be performed in a heat-resistant sealed container, for example. The conditions of the hydrothermal treatment include: a temperature of 400-800°C and a time of 1-12 hours; the present invention does not limit the pressure of the hydrothermal treatment, and the hydrothermal treatment can be performed under the autogenous pressure of the reaction system or under an external pressure, preferably under the autogenous pressure.

[0069] According to the present disclosure, drying is a technical means commonly used by those skilled in the art, for example, it can be performed in a constant temperature drying oven. The conditions of the first drying, the second drying and the third drying can each independently include: a temperature of 90-120° C. and a time of 2-24 hours.

[0070] According to the present disclosure, calcination is a technical means conventionally adopted by those skilled in the art, and can be performed in a muffle furnace, a tube furnace, etc. The conditions of the first calcination, the second calcination, and the third calcination can each independently include: a temperature of 450-600° C. and a time of 2-6 hours. The present invention does not specifically limit the calcination atmosphere, and can be, for example, an air atmosphere, an inert gas atmosphere, etc.

[0071] In a specific embodiment of the present disclosure, a hollow ZSM-5 multi-level pore molecular sieve raw material is prepared by a method comprising the following steps: (1) mixing a first organosilicon source and a first solvent at 30-50° C. and stirring for 0.5-5 hours, then heating to 70-100° C. and stirring for 2-10 hours, and mixing the obtained mixed liquid with a first template at 20-30° C. for 0.5-3.0 hours to obtain a first mixed product; (2) mixing a first alkali metal hydroxide, calculated as alkali metal oxide, a second solvent and a first aluminum source, calculated as Al2O3, at a molar ratio of (1.5-5):(60-350):1 at 20-80° C. for 0.5-2.0 hours, Obtain a second mixed product; (3) Mix the first mixed product and the second mixed product and then perform dynamic crystallization, take out the obtained solid and perform a fourth calcination to obtain a third solid product; (4) Mix the third solid product with the first solution containing alkali, heat the temperature to the reaction temperature at a heating rate of 1-5°C / min, and react at the reaction temperature for 10-90min to obtain a fourth solid product; wherein the reaction temperature is 60-90°C, and the content of alkali in the first solution containing alkali is 0.45-2mol / L; (5) Perform a first ammonium exchange on the fourth solid product, and optionally perform a sixth calcination to obtain a hollow ZSM-5 multi-level pore molecular sieve raw material.

[0072] According to the present disclosure, the total amount of the first template, the first solvent and the second solvent, and the molar ratio of the first alkali metal hydroxide and the first organic silicon source can vary in a large range, for example, it can be (0.06-0.55): (10-100): (0.02-1.5): 1, preferably (0.1-0.50): (15-85): (0.03-1.2): 1, and the molar ratio of the first organic silicon source to the first aluminum source can be (20-500): 1; wherein the first organic silicon source is calculated as SiO2, the first alkali metal hydroxide is calculated as alkali metal oxide (for example, when the first alkali metal hydroxide is NaOH, the first alkali metal hydroxide is calculated as Na2O), and the first aluminum source is calculated as Al2O3. In one embodiment, the first template and the first alkali metal hydroxide contain OH - The ratio of the total molar amount of to the molar amount of the first organic silicon source calculated as SiO2 is (0.01-1.5):1, preferably (0.02-1.2):1.

[0073] According to the present disclosure, in step (2), the molar ratio of the first alkali metal hydroxide, calculated as alkali metal oxide, the second solvent and the first aluminum source, calculated as Al2O3, is preferably (2.0-4.5): (80-350): 1.

[0074] According to the present disclosure, in step (3), dynamic crystallization is well known to those skilled in the art, and the conditions of the dynamic crystallization may include: a temperature of 80-200°C and a time of 4-80 hours; preferably, a temperature of 160-180°C and a time of 12-60 hours.

[0075] According to the present disclosure, in step (4), the weight ratio of the third solid product to the first alkali-containing solution can be 1:(2-10), preferably 1:(8-10); the ratio of the bulk silicon-aluminum molar ratio and the surface silicon-aluminum molar ratio of the third solid product can be 1.2-5.0.

[0076] According to the present disclosure, in step (5), the first ammonium exchange of the fourth solid product comprises: mixing the fourth solid product, the first ammonium source and the fifth solvent in a weight ratio of 1: (0.5-1.0): (8-10), and reacting the obtained mixture at 70-90°C for 0.5-5 hours. The first ammonium source is selected from one or more of ammonium chloride, ammonium sulfate and ammonium nitrate. Optionally, the product obtained by the first ammonium exchange is filtered, washed and dried; optionally, the product obtained by the first ammonium exchange is subjected to a sixth roasting, preferably, the product obtained by the first ammonium exchange is subjected to a sixth roasting after being filtered, washed and dried; the temperature of the sixth roasting can be 400-600°C, and the time can be 1-24 hours, preferably 1-10 hours or 1.5-6 hours, more preferably, the temperature is 450-580°C, and the time is 2-4.5 hours.

[0077] In one embodiment, compared with the third solid product, the mesopore specific surface area of ​​the hollow ZSM-5 multi-level pore molecular sieve raw material increases by 100-500%, the mesopore volume increases by 150-600%, and the total acid content increases by 50-250%.

[0078] In another specific embodiment of the present disclosure, a hollow ZSM-5 multi-level pore molecular sieve raw material is prepared by a method comprising the following steps: S1, mixing a second template, a second inorganic silicon source and a third solvent at 30-50°C for 0.5-3.0 hours, and subjecting the obtained third mixed product to a first hydrothermal treatment and a second hydrothermal treatment in sequence to obtain a fourth mixed product; wherein the conditions of the first hydrothermal treatment include: a temperature of 80-150°C and a time of 1-6 hours; the conditions of the second hydrothermal treatment include: a temperature of 160-180°C and a time of 12-60 hours; S2, mixing a second alkali metal hydroxide, a fourth solvent and a third solvent in terms of alkali metal oxide in a molar ratio of (1.5-5): (60-350): 1. The two aluminum sources are mixed at 20-80°C for 0.5-2.0 hours to obtain a fifth mixed product; S3, the fourth mixed product and the fifth mixed product are mixed, the obtained mixture is subjected to a third hydrothermal treatment, the obtained solid is taken out and subjected to a fifth roasting to obtain a fifth solid product; S4, the fifth solid product is mixed with the second alkali-containing solution, the temperature is increased to the reaction temperature at a heating rate of 1-5°C / min, and the reaction is carried out at the reaction temperature for 10-90min to obtain a sixth solid product, wherein the reaction temperature is 60-90°C, and the alkali content in the second alkali-containing solution is 0.45-2mol / L; S5, the sixth solid product is subjected to a second ammonium exchange, and optionally a seventh roasting to obtain a hollow ZSM-5 multi-level pore molecular sieve raw material.

[0079] According to the present disclosure, the molar ratio of the total amount of the second template, the third solvent and the fourth solvent, the amount of the second alkali metal hydroxide and the second inorganic silicon source is (0.06-0.55): (10-100): (0.02-1.5): 1, preferably (0.10-0.50): (15-85): (0.03-1.2): 1, and the molar ratio of the second inorganic silicon source to the second aluminum source is (20-500): 1; wherein the second inorganic silicon source is calculated as SiO2, the second alkali metal hydroxide is calculated as alkali metal oxide (for example, when the second alkali metal hydroxide is NaOH, the second alkali metal hydroxide is calculated as Na2O), and the second aluminum source is calculated as Al2O3. In one embodiment, the second template and the second alkali metal hydroxide contain OH - The ratio of the total molar amount of to the molar amount of the second inorganic silicon source calculated as SiO2 (abbreviated as OH / SiO2) is (0.01-1.5):1, preferably (0.02-1.2):1.

[0080] According to the present disclosure, hydrothermal treatment is well known to those skilled in the art, and can be performed in a heat-resistant sealed container, for example. The present invention does not limit the conditions of the hydrothermal treatment, and the hydrothermal treatment can be performed under the autogenous pressure of the reaction system or under an applied pressure, preferably under autogenous pressure.

[0081] According to the present disclosure, in step S2, the molar ratio of the second alkali metal hydroxide calculated as alkali metal oxide, the fourth solvent and the second aluminum source calculated as Al2O3 is preferably (2.0-4.5): (80-350): 1.

[0082] In one embodiment, in step S3, the conditions of the third hydrothermal treatment include: 160-180° C., and time of 12-60 hours.

[0083] According to the present disclosure, in step S4, the weight ratio of the fifth solid product to the second alkali-containing solution is 1:(2-10), preferably 1:(8-10), and the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio of the fifth solid product is 1.2-5.0.

[0084] According to the present disclosure, in step S5, the second ammonium exchange of the sixth solid product comprises: mixing the sixth solid product, the second ammonium source and the sixth solvent in a weight ratio of 1: (0.5-1.0): (8-10), and reacting the obtained mixture at 70-90°C for 0.5-2 hours. The second ammonium source is selected from one or more of ammonium chloride, ammonium sulfate and ammonium nitrate. Optionally, the product obtained by the second ammonium exchange is filtered, washed and dried; optionally, the product obtained by the second ammonium exchange is subjected to the seventh roasting, preferably, the product obtained by the second ammonium exchange is subjected to the seventh roasting after filtering, washing and drying; the temperature of the seventh roasting can be 400-600°C, and the time can be 1-24 hours, preferably 1-10 hours or 1.5-6 hours, more preferably, the temperature is 450-580°C, and the time is 2-4.5 hours.

[0085] According to the present disclosure, compared with the fifth solid product, the mesopore specific surface area of ​​the hollow ZSM-5 multi-level pore molecular sieve increases by 100-500%, the mesopore volume increases by 150-600%, and the total acid content increases by 50-250%.

[0086] In one embodiment, the conditions of the fourth calcination and the fifth calcination each independently include: a temperature of 400-600° C. and a time of 2-6 hours, preferably, a temperature of 450-580° C. and a time of 3-5 hours.

[0087] According to the present disclosure, the first organic silicon source is selected from one or more of methyl orthosilicate and ethyl orthosilicate; the second inorganic silicon source is selected from one or more of silica sol, water glass and solid silica gel; the first template and the second template are each independently selected from one or more of tetrapropylammonium bromide, tetrapropylammonium hydroxide, n-butylamine and hexamethylenediamine; the first aluminum source and the second aluminum source are each independently selected from one or more of sodium aluminate, aluminum sulfate, aluminum nitrate, aluminum isopropoxide and aluminum sol; the first alkali metal hydroxide and the second alkali metal hydroxide are each independently selected from one or more of lithium hydroxide, sodium hydroxide and potassium hydroxide; the first alkali solution and the second alkali solution are each independently selected from one or more of sodium hydroxide solution, potassium hydroxide solution, lithium hydroxide and barium hydroxide.

[0088] According to the present disclosure, in one embodiment, the first solvent, the second solvent, the third solvent, the fourth solvent, the fifth solvent and the sixth solvent are each water.

[0089] The present disclosure is further illustrated below by way of examples, but the present disclosure is not limited thereby.

[0090] The raw materials used in the following examples and comparative examples are commercially available unless otherwise specified, wherein kaolin is an industrial product of China Kaolin Corporation, with a solid content of 75% by weight; pseudo-boehmite is produced by Shandong Aluminum Plant, with an alumina content of 65% by weight; aluminum sol is produced by Qilu Branch of Sinopec Catalyst Co., Ltd., with an alumina content of 21% by weight; silica sol is produced by Beijing Chemical Plant, with a silicon oxide content of 25% by weight (acidic silica sol, pH 3.0); concentrated hydrochloric acid is chemically pure, produced by Beijing Chemical Plant. β molecular sieve, brand BETA-25-NKC, pore size of 0.59 nm, produced by Tianjin Nanhua Catalyst Co., Ltd., its SEM picture is as follows Figure 3 Y-type molecular sieve, grade SCY-12, rare earth content 12% by weight, produced by Qilu Branch of Sinopec Catalyst Co., Ltd., its SEM picture is as shown in Figure 4 shown.

[0091] In the embodiments and comparative examples, the crystal size of the molecular sieve was measured by SEM, and 10 crystal sizes were randomly measured and the average value was taken to obtain the average crystal size of the molecular sieve sample.

[0092] The bulk silicon-aluminum ratio of the sample was determined by XRF method, the instrument was ZSX Primus II (Rigaku) ​​X-ray fluorescence spectrometer; the test conditions were: excitation voltage 50kV, excitation current 50mA, rhodium and palladium. The intensity of each element peak was measured by scintillation counter and proportional counter to analyze the elemental composition of the molecular sieve.

[0093] The surface silicon-aluminum molar ratio of the sample was determined by the XPS method, using the ESCALab250 X-ray photoelectron spectrometer from ThermoFisher, under the following test conditions: the excitation source was monochromatic Al Kα X-ray, the excitation energy was 1496.6 eV, and the power was 150 W. The electron binding energy was corrected using the C1s peak (284.8 eV) of the contaminated carbon.

[0094] The total specific surface area, mesopore specific surface area and N2 adsorption-desorption curve of the sample were detected by BET adsorption full analysis method. Instrument: ASAP 2420 adsorption instrument from Micromeritics, USA. Test conditions: The sample was vacuum degassed at 100℃ and 300℃ for 0.5h and 6h respectively, and N2 adsorption-desorption test was carried out at 77.4K. The adsorption and desorption amount of nitrogen of the purified sample under different specific pressure conditions were tested to obtain the N2 adsorption-desorption isotherm. The BET specific surface area was calculated by BET formula, the micropore area was calculated by t-plot, and the pore size distribution was calculated by BJH.

[0095] The relative crystallinity of the sample was detected by X-ray diffraction method, instrument: Empyrean. Test conditions: tube voltage 40 kV, tube current 40 mA, Cu target Kα radiation, 2θ scanning range 5°-35°, scanning rate 2 (°) / min.

[0096] The phosphorus-aluminum molar ratio of the sample is detected by X-ray fluorescence method. Instrument: ZSX Primus II (Rigaku) ​​X-ray fluorescence spectrometer. Test conditions: excitation voltage 50kV, excitation current 50mA, rhodium-palladium. The intensity of each element peak is measured by scintillation counter and proportional counter to analyze the elemental composition of molecular sieve.

[0097] The content of metal components in the sample was detected by X-ray fluorescence method, and the detection conditions were the same as above.

[0098] The strong B acid content and total B acid content of the sample were detected by pyridine infrared adsorption method, and the strong L acid content and total L acid content were detected by pyridine infrared adsorption method. Instrument: NICOLET 6700 Fourier transform infrared spectrometer of BIQ-RAD Company, USA. Test method: After the sample is pressed into a tablet, it is placed in the in-situ cell of the infrared spectrometer and sealed, and adsorption and desorption are carried out according to the set program. The pyridine adsorbed acid content is calculated by peak area.

[0099] Examples 1-3 are examples of preparing modified hollow ZSM-5 multi-level pore molecular sieves

[0100] Example 1

[0101] (1) 456.0 g of ethyl orthosilicate was weighed, and 3115.7 g of deionized water was added. The mixture was stirred and heated in a water bath at 40° C. for 2 h, and then the water bath temperature was raised to 70° C. and stirred and heated for 4 h to remove ethanol produced by hydrolysis of the silicon source. During this process, water evaporated simultaneously with the ethanol was intermittently added to the system. The obtained mixed liquid was mixed and stirred with 558.3 ​​g of a tetrapropylammonium hydroxide aqueous solution (mass fraction of 25.0%) at 25° C. for 1 h to obtain a first mixed product;

[0102] (2) weighing 17.2 g of sodium hydroxide particles, adding 384.0 g of deionized water to completely dissolve the sodium hydroxide, then adding 40.8 g of aluminum nitrate nonahydrate, and stirring at room temperature for 1.0 h to obtain a second mixed product (i.e., an aluminum source solution);

[0103] (3) slowly adding the second mixed product to the first mixed product, mixing evenly, stirring at room temperature for 4.0 hours, transferring the obtained precursor solution into a synthesis reactor, and dynamically crystallizing at 170° C. for 48 hours; after the crystallization, centrifugally filtering, washing, drying, and calcining at 550° C. for 4 hours to obtain a third solid product (referred to as molecular sieve I-M1);

[0104] (4) the third solid product and a sodium hydroxide solution with a concentration of 0.5 mol / L were mixed evenly, the mass ratio of the third solid product to the alkaline solution was 1:10, the temperature was raised to 80°C at a heating rate of 2°C / min, and then stirred at this temperature for 30 minutes, filtered, washed, and dried to obtain a fourth solid product (referred to as molecular sieve I-S1-Na);

[0105] (5) The fourth solid product: ammonium chloride: deionized water are mixed uniformly in a weight ratio of 1:1:10, stirred and heated in a water bath at 80°C for 30 minutes, filtered, washed, and dried; the obtained solid product: ammonium chloride: deionized water are mixed uniformly in a weight ratio of 1:0.5:10, subjected to a second ammonium exchange, filtered, washed, dried, and calcined at 550°C for 2 hours to obtain a hydrogen-type hollow ZSM-5 multi-level pore molecular sieve, denoted as I-S1-H.

[0106] (6) The hydrogen-type hollow ZSM-5 multi-level pore molecular sieve I-S1-H was modified, and the solid content of the molecular sieve was 96.65% by weight. 2.69g of H3PO4 solution (concentration 85% by weight) was dissolved in 46.25g of deionized water, and stirred evenly to fully dissolve to obtain a phosphorus-containing solution; 50g of the hollow ZSM-5 multi-level pore molecular sieve I-S1-H was spread on a surface dish, and the phosphorus-containing solution was slowly added dropwise, and fully mixed to obtain a "viscous paste" slurry of the molecular sieve, and then the slurry was dried at 115°C in an air atmosphere for 4h, and then calcined at 550°C for 2h to obtain a first solid product;

[0107] (7) hydrothermally treating the first solid product at 600° C. and 100% water vapor for 4 h to obtain a second solid product;

[0108] (8) 2.48 g of lanthanum chloride was dissolved in 46.26 g of deionized water, and the mixture was stirred to obtain a metal salt solution. The metal salt solution was added to the second solid product and mixed to obtain a slurry of the molecular sieve in a "viscous paste" state. The slurry was then dried at 110° C. in an air atmosphere for 4 h and calcined at 550° C. for 2 h to obtain a modified hollow ZSM-5 hierarchical pore molecular sieve SS-1, the SEM image of which is shown in FIG. Figure 1 The properties of the samples are shown in Table 1.

[0109] Example 2

[0110] (1) weighing 550.0 g of methyl orthosilicate, adding 2975.0 g of deionized water, stirring and heating in a water bath at 30° C. for 5 h, raising the water bath temperature to 70° C. and stirring for 4 h to remove ethanol produced by hydrolysis of the silicon source, intermittently replenishing the system with water evaporated simultaneously with the ethanol during the process, and mixing the obtained mixed liquid with 241.5 g of a tetrapropylammonium bromide aqueous solution (mass fraction of 25.0%) at 20° C. and stirring for 0.5 h to obtain a first mixed product;

[0111] (2) weighing 9.1 g of sodium hydroxide particles, adding 217.0 g of deionized water to completely dissolve the sodium hydroxide, then adding 6.0 g of sodium aluminate (alumina content is 62.0%), stirring at 20° C. for 2.0 h, and obtaining a second mixed product;

[0112] (3) slowly adding the second mixed product to the first mixed product, mixing evenly, and stirring at room temperature for 4.0 hours; transferring the obtained precursor solution into a synthesis reactor, and dynamically crystallizing at 180° C. for 24 hours; after the crystallization, centrifugally filtering, washing, drying, and calcining at 550° C. for 4 hours to obtain a third solid product (referred to as molecular sieve I-M2);

[0113] (4) mixing the third solid product and a sodium hydroxide alkaline solution having a concentration of 0.6 mol / L, wherein the mass ratio of the third solid product to the alkaline solution is 1:10, heating the mixture to 80° C. at a heating rate of 4° C. / min, and then heating and stirring the mixture at 80° C. for 30 min, filtering, washing, and drying the mixture to obtain a fourth solid product (referred to as molecular sieve I-S2-Na);

[0114] (5) The fourth solid product: ammonium chloride: deionized water are mixed uniformly in a weight ratio of 1:1:10, stirred and heated in a water bath at 80°C for 30 min, filtered, washed, and dried, and the obtained solid product: ammonium chloride: deionized water = 1:0.5:10 is mixed uniformly, subjected to a second ammonium exchange, filtered, washed, dried, and calcined at 550°C for 2 h to obtain a hydrogen-type hollow ZSM-5 multi-level pore molecular sieve, denoted as I-S2-H.

[0115] (6) The hollow ZSM-5 multi-level pore molecular sieve I-S2-H was modified, and the solid content of the molecular sieve was 94.21% by weight. 2.68g of ammonium dihydrogen phosphate was dissolved in 44.21g of deionized water, and then 4.25g of Fe(NO3)3·6H2O was added and stirred to obtain a solution containing a phosphorus source and a metal source; 50g of the hollow ZSM-5 multi-level pore molecular sieve I-S2-H was spread on a surface dish, and the solution containing a phosphorus source and a metal source was slowly added dropwise, and mixed to obtain a slurry of the molecular sieve in a "viscous paste" state, and then the slurry was dried at 110°C in an air atmosphere for 4h, and calcined at 550°C for 2h to obtain a modified hollow ZSM-5 multi-level pore molecular sieve SS-2, whose SEM image is shown as follows: Figure 2 The properties of the samples are shown in Table 1.

[0116] Example 3

[0117] (1) Weigh 455.9 g of tetrapropylammonium hydroxide aqueous solution (mass fraction 25.0%), add 3238.3 g of deionized water, stir at room temperature for 10 min, then add 1156.4 g of silica sol (SiO2 content 25%), stir for 1.0 h in a 50° C. water bath, transfer the obtained third mixed product into a reactor, crystallize at 80° C. for 2 h, and then heat to 170° C. for crystallization for 12 h to obtain a fourth mixed product;

[0118] (2) weighing 9.7 g of sodium hydroxide particles, adding 277.9 g of deionized water to completely dissolve the sodium hydroxide, then adding 33.3 g of aluminum nitrate nonahydrate, and stirring at 25° C. for 1.0 h to obtain a fifth mixed product;

[0119] (3) adding the fourth mixed product to the fifth mixed product, stirring evenly, and continuing to crystallize at 170° C. for 36 hours; after the crystallization is completed, centrifugation is performed, washed, dried, and calcined at 550° C. for 4 hours to obtain a fifth solid product (referred to as molecular sieve I-M3);

[0120] (4) the fifth solid product and a sodium hydroxide solution with a concentration of 1.0 mol / L were mixed evenly, the mass ratio of the fourth solid product to the alkaline solution was 1:10, the temperature was raised to 80°C at a heating rate of 5°C / min, and then stirred at this temperature for 30 minutes, filtered, washed, and dried to obtain a sixth solid product (referred to as molecular sieve I-S3-Na);

[0121] (5) The sixth solid product: ammonium chloride: deionized water were mixed uniformly in a weight ratio of 1:1:10, stirred and heated in a water bath at 80°C for 30 min, filtered, washed, and dried, and then the obtained solid product: ammonium chloride: deionized water were mixed uniformly in a weight ratio of 1:0.5:10, subjected to a second ammonium exchange, filtered, washed, dried, and calcined at 550°C for 2 h to obtain a hollow ZSM-5 multi-level pore molecular sieve, denoted as I-S3-H.

[0122] (6) The hollow ZSM-5 multi-level pore molecular sieve I-S3-H was modified, and the solid content of the molecular sieve was 92.75% by weight. 1.71g of H3PO4 solution (concentration 85% by weight) was dissolved in 42.49g of deionized water, and stirred evenly to fully dissolve to obtain a phosphorus-containing solution; 50g of the hollow ZSM-5 multi-level pore molecular sieve I-S3-H was spread on a surface dish, and the phosphorus-containing solution was slowly added dropwise, and fully mixed to obtain a "viscous paste" slurry of the molecular sieve, and then the slurry was dried at 115°C in an air atmosphere for 4h, and then calcined at 550°C for 2h to obtain a first solid product;

[0123] (7) hydrothermally treating the first solid product at 600° C. and 100% water vapor for 4 h to obtain a second solid product;

[0124] (8) 4.48 g of gallium nitrate nonahydrate was dissolved in 46.26 g of deionized water, and the mixture was stirred to obtain a metal salt solution. The metal salt solution was added to the second solid product and mixed to obtain a slurry of the molecular sieve in a "viscous paste-like" state. The slurry was then dried at 110° C. in an air atmosphere for 4 h and calcined at 550° C. for 2 h to obtain a modified hollow ZSM-5 multi-level pore molecular sieve SS-3. The properties of the modified hollow ZSM-5 multi-level pore molecular sieve SS-3 are shown in Table 1.

[0125] Comparative Example 1

[0126] Conventional crystalline ZSM-5 molecular sieve DSS-1 was purchased from Qilu Branch of Sinopec Catalyst Company, with a silicon-aluminum molar ratio (SiO2 / Al2O3) of 25. Its properties are listed in Table 1.

[0127] Table 1

[0128]

[0129]

[0130]

[0131] In Table 1, R represents a template, and the bulk-surface silicon-aluminum molar ratio represents the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio;

[0132] Increased value of mesoporous specific surface area = 100% × [mesoporous specific surface area of ​​hollow ZSM-5 multi-level pore molecular sieve (or hollow multi-level pore ZSM-5 nanocrystalline material, hydrogen-type hollow ZSM-5 multi-level pore molecular sieve before introduction of phosphorus) / mesoporous specific surface area of ​​the first solid product (or fourth solid product) - 1];

[0133] Mesopore specific volume increase value = 100% × [mesopore specific volume of hollow ZSM-5 hierarchical pore molecular sieve (or hollow multi-level pore ZSM-5 nanocrystalline material, hydrogen-type hollow ZSM-5 hierarchical pore molecular sieve before introduction of phosphorus) / mesopore specific volume of the first solid product (or fourth solid product) - 1];

[0134] Total acid increase value = 100% × [total acid amount of hollow ZSM-5 multi-level pore molecular sieve (or hollow multi-level pore ZSM-5 nanocrystalline material, hydrogen-type hollow ZSM-5 multi-level pore molecular sieve before the introduction of phosphorus) / total acid amount of the first solid product (or the fourth solid product) - 1].

[0135] Examples 4-9 are examples of preparing catalytic cracking catalysts

[0136] Embodiment 4-9

[0137] Catalysts were prepared using the modified hollow ZSM-5 multi-level pore molecular sieves prepared in Examples 1-3, and the catalyst numbers were A1-A6.

[0138] The preparation method of the catalytic cracking catalyst comprises:

[0139] (1) Pseudo-boehmite and water are uniformly mixed, and concentrated hydrochloric acid with a concentration of 36% by weight is added under stirring, and the acid-aluminum molar ratio is 0.2 (the weight ratio of HCl to pseudo-boehmite calculated as Al2O3); the resulting mixture is aged at 70°C for 1.5 hours to obtain an aged pseudo-boehmite slurry. The aged pseudo-boehmite slurry has an aluminum oxide content of 12% by weight;

[0140] (2) uniformly mixing the prepared modified hollow ZSM-5 multi-level pore molecular sieve, β molecular sieve, Y-type molecular sieve, aluminum sol, silica sol, kaolin, the aged pseudo-boehmite slurry and deionized water to form a slurry with a solid content of 30 wt%, and spray drying to obtain catalyst microspheres;

[0141] (3) calcining the catalyst microspheres at 550°C for 4 h;

[0142] (4) The calcined catalyst microspheres were exchanged at 80°C for 1 hour according to a weight ratio of catalyst microspheres: ammonium salt: H2O = 1:1:10, filtered, and the above exchange and filtration process was repeated once, and then dried, wherein the ammonium salt was ammonium chloride, and the sodium oxide content in the obtained catalytic cracking catalyst was less than 0.15% by weight. The composition of the prepared catalyst is shown in Table 2.

[0143] Comparative Examples 2-3

[0144] Catalysts DA1 and DA2 were prepared in the same manner as in Example 4, except that the molecular sieve DSS-1 of Comparative Example 1 was used instead of the molecular sieve SS-1 prepared in Example 1. The compositions of the prepared catalysts are shown in Table 2.

[0145] Table 2

[0146]

[0147] Test Example 1

[0148] After aging the catalytic cracking catalysts prepared in Examples 7-9 and Comparative Example 3 at 820°C and 100% by volume steam for 30 hours, their catalytic cracking performance of whole-fraction oil was evaluated in a small fixed fluidized bed reactor. The evaluation conditions were a reaction temperature of 580°C and a weight space velocity of 20 h. -1 , agent-oil weight ratio 8. The properties of the whole fraction oil are shown in Table 3, and the reaction results are shown in Table 4. The product mass distribution is calculated based on the raw material feed.

[0149] Table 3

[0150]

[0151] Table 4

[0152]

[0153]

[0154] It can be seen from Table 4 that the catalytic cracking catalyst provided by the present disclosure has a higher cracking ability and a higher yield of light olefins.

[0155] Test Example 2

[0156] The catalytic cracking catalysts prepared in Examples 4-6 and Comparative Example 2 were aged at 820°C and 100% by volume steam for 30 hours, and then their intermediate base heavy oil catalytic cracking reaction performance was evaluated in a small fixed fluidized bed reactor. The evaluation conditions were a reaction temperature of 580°C and a weight space velocity of 20 h. -1 , agent-oil weight ratio is 8. The properties of the intermediate base heavy oil are shown in Table 5, and the reaction results are shown in Table 6.

[0157] The product mass distribution described therein is calculated based on the raw material feed.

[0158] Table 5

[0159] Intermediate base heavy oil properties Carbon content, weight % 86.43 Hydrogen content, weight % 12.88 <![CDATA[Density at 20 °C, kg / m 3 > 901 Carbon residue, weight % 4.8 Freezing point, ℃ 42 Initial distillation point, ℃ 278.8 Final distillation point, ℃ 540.2 Saturated hydrocarbons, weight % 40 Aromatics, weight % 22.6 Gel, weight% 37.3 Asphaltenes, weight % 0.1 Paraffins, weight % 29.4 Monocycloalkanes, weight % 8.4 Bicycloalkanes, weight % 9.5 Tricycloalkanes, weight % 6.7 Total cycloalkanes, weight % 26.4 Total bicyclic aromatic hydrocarbons, weight % 10.2

[0160] Table 6

[0161]

[0162]

[0163] It can be seen from Table 6 that the heavy oil catalytic cracking catalyst provided by the present disclosure has a higher intermediate-base heavy oil catalytic cracking capacity and a higher light olefin yield.

[0164] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.

[0165] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

[0166] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.

Claims

1. A catalytic cracking method, characterized in that: The method comprises: contacting a crude oil with a catalytic cracking catalyst for reaction, wherein the crude oil is a full-fraction oil or an intermediate base heavy oil, and the catalytic cracking catalyst comprises a modified hollow ZSM-5 multi-level pore molecular sieve, a nano molecular sieve, a Y-type molecular sieve and a carrier; Based on the dry weight of the catalytic cracking catalyst, the content of the modified hollow ZSM-5 multi-level pore molecular sieve is 15-40% by weight, the content of the nano molecular sieve is 1-10% by weight, the content of the Y-type molecular sieve is 5-15% by weight, and the content of the carrier is 40-80% by weight; The modified hollow ZSM-5 multi-level pore molecular sieve contains a molecular sieve and phosphorus and metal components loaded on the molecular sieve; the phosphorus-aluminum molar ratio of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.1-1.5; the content of the metal component is 0.1-5% by weight based on the oxide of the metal component and the dry basis weight of the modified hollow ZSM-5 multi-level pore molecular sieve; the modified hollow ZSM-5 multi-level pore molecular sieve has a closed hollow structure, the average grain size of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.2-3.0 μm, and the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.0-1.5; the total specific surface area of ​​the modified hollow ZSM-5 multi-level pore molecular sieve is 250-350 m 2 / g, mesopore specific surface area is 20-100m 2 / g, the mesoporous specific surface area accounts for 15-40% of the total specific surface area, the strong B acid content accounts for 55-70% of the total B acid content, and the strong L acid content accounts for 50-70% of the total L acid content; The pore size of the nano molecular sieve is 0.56-0.75 nm.

2. The method according to claim 1, wherein: The raw oil is a full-fraction oil, and the reaction conditions include: a reaction temperature of 550-600° C.; based on the dry weight of the catalytic cracking catalyst, the content of the modified hollow ZSM-5 multi-level pore molecular sieve is 20-40% by weight, the content of the nano molecular sieve is 1-5% by weight, the content of the Y-type molecular sieve is 5-15% by weight, and the content of the carrier is 40-80% by weight.

3. The method according to claim 1, wherein: The feedstock oil is intermediate base heavy oil, and the reaction conditions include: a reaction temperature of 550-600° C.; based on the dry weight of the catalytic cracking catalyst, the content of the modified hollow ZSM-5 multi-level pore molecular sieve is 15-30% by weight, the content of the nano molecular sieve is 5-10% by weight, the content of the Y-type molecular sieve is 5-10% by weight, and the content of the carrier is 50-75% by weight.

4. A catalytic cracking catalyst, characterized in that: The catalytic cracking catalyst contains a modified hollow ZSM-5 multi-level pore molecular sieve, a nano molecular sieve, a Y-type molecular sieve and a carrier. Based on the dry weight of the catalytic cracking catalyst, the content of the modified hollow ZSM-5 multi-level pore molecular sieve is 15-40% by weight, the content of the nano molecular sieve is 1-10% by weight, the content of the Y-type molecular sieve is 5-15% by weight, and the content of the carrier is 40-80% by weight; The modified hollow ZSM-5 multi-level pore molecular sieve contains a molecular sieve and phosphorus and metal components loaded on the molecular sieve; the phosphorus-aluminum molar ratio of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.1-1.5; the content of the metal component is 0.1-5% by weight based on the oxide of the metal component and the dry basis weight of the modified hollow ZSM-5 multi-level pore molecular sieve; the modified hollow ZSM-5 multi-level pore molecular sieve has a closed hollow structure, the average grain size of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.2-3.0 μm, and the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.0-1.5; the total specific surface area of ​​the modified hollow ZSM-5 multi-level pore molecular sieve is 250-350 m 2 / g, mesopore specific surface area is 20-100m 2 / g, the mesoporous specific surface area accounts for 15-40% of the total specific surface area, the strong B acid content accounts for 55-70% of the total B acid content, and the strong L acid content accounts for 50-70% of the total L acid content; The pore size of the nano molecular sieve is 0.56-0.75 nm.

5. The catalytic cracking catalyst according to claim 4, wherein The phosphorus-aluminum molar ratio of the modified hollow ZSM-5 multi-level pore molecular sieve is 0.2-1.3; The content of the metal component is 0.5-4% by weight, calculated as the oxide of the metal component and based on the dry weight of the modified hollow ZSM-5 multi-level pore molecular sieve.

6. The catalytic cracking catalyst according to claim 4, wherein: The average grain size of the modified hollow ZSM-5 multi-level pore molecular sieve grains is 0.5-3.0 μm, the ratio of the bulk silicon-aluminum molar ratio to the surface silicon-aluminum molar ratio is 1.0-1.3, and the relative crystallinity is 80-90%.

7. The catalytic cracking catalyst according to claim 4, wherein The total specific surface area of ​​the modified hollow ZSM-5 multi-level pore molecular sieve is 260-340 m 2 / g, mesopore specific surface area is 25-100m 2 / g, and the mesoporous specific surface area accounts for 18-35% of the total specific surface area.

8. The catalytic cracking catalyst according to claim 4, wherein The metal component is selected from one or more of lanthanum, cerium, tungsten, iron, cobalt, nickel, copper, manganese, zinc, tin, bismuth and gallium; The nano molecular sieve is one or more of the molecular sieves having the structures of AET, AFR, AFS, AFI, BEA, BOG, CFI, CON, GME, IFR, ISV, LTL, MEI, MOR, OFF and SAO; preferably at least one of Beta, SAPO-5, SAPO-40, SSZ-13, CIT-1, ITQ-7, ZSM-18, mordenite and gmelinite; The Y-type molecular sieve is one or more selected from REY molecular sieve, DASY molecular sieve, USY molecular sieve, phosphorus-containing DASY molecular sieve, phosphorus-containing USY molecular sieve, PSRY molecular sieve, HRY molecular sieve, HSY molecular sieve, SCY molecular sieve, and RSCY molecular sieve.

9. The catalytic cracking catalyst according to claim 4, wherein: The carrier is selected from one or more of natural clay, alumina carrier, silica carrier, aluminum phosphate carrier and silica-alumina carrier; Preferably, the silica carrier is one or more of neutral silica sol, acidic silica sol or alkaline silica sol; the alumina carrier is one or more of aluminum sol, acidified pseudo-boehmite, hydrated alumina and activated alumina; the aluminum phosphate carrier is phosphate aluminum gel; the silica aluminum oxide carrier is one or more of solid silica aluminum material, silica aluminum sol and silica aluminum gel.

10. The catalytic cracking catalyst according to claim 4, wherein: The carrier comprises a silicon oxide carrier; based on the dry weight of the catalytic cracking catalyst, the content of the silicon oxide carrier in terms of SiO2 is 1-20% by weight.

11. A method for preparing the catalytic cracking catalyst according to any one of claims 4 to 10, the method comprising: The slurry containing the support, the modified hollow ZSM-5 hierarchical pore molecular sieve, the nano molecular sieve, the Y-type molecular sieve and water is dried and optionally calcined.

12. The method according to claim 11, wherein: The preparation steps of the modified hollow ZSM-5 multi-level pore molecular sieve include: Mixing a first solution containing a first phosphorus source and a first metal source with a hollow ZSM-5 multi-level pore molecular sieve raw material, and performing a first drying and a first calcination on the obtained first slurry, wherein the weight ratio of the first solution to the hollow ZSM-5 multi-level pore molecular sieve raw material is 1:(0.5-2.0); Alternatively, the preparation steps of the modified hollow ZSM-5 multi-level pore molecular sieve include: S1, mixing a second solution containing a second phosphorus source with a hollow ZSM-5 multi-level pore molecular sieve raw material, and performing a second drying and a second calcination on the obtained second slurry to obtain a first solid product; wherein the weight ratio of the second solution containing the second phosphorus source to the hollow ZSM-5 multi-level pore molecular sieve raw material is 1: (0.5-2.0); S2, subjecting the first solid product to hydrothermal treatment to obtain a second solid product; S3. Mixing a third solution containing a second metal source with the second solid product, and performing a third drying and a third calcination on the obtained third slurry, wherein the weight ratio of the third solution containing the second metal source to the second solid product is 1:(0.5-2.0).

13. The method according to claim 12, wherein: The first phosphorus source and the second phosphorus source are each independently selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate and ammonium phosphate; The first metal source and the second metal source are each independently selected from one or more of metal nitrates, chlorides and sulfates, and the metal is selected from one or more of lanthanum, cerium, tungsten, iron, cobalt, nickel, copper, manganese, zinc, tin, bismuth and gallium; The hollow ZSM-5 multi-level pore molecular sieve raw material is an H-type hollow ZSM-5 multi-level pore molecular sieve.

14. The method according to claim 12, wherein: The conditions of the hydrothermal treatment include: a temperature of 400-800°C and a time of 1-12 hours; The conditions of the first drying, the second drying and the third drying independently include: a temperature of 90-120° C. and a time of 2-24 hours; The conditions of the first calcination, the second calcination and the third calcination independently include: a temperature of 450-600° C. and a time of 2-6 hours.

Citation Information

Patent Citations

  • Catalytic cracking catalyst and preparation method thereof

    CN107971015A

  • Catalyst for increasing yield of low-carbon olefins by directly catalytically cracking crude oil and preparation method thereof

    CN113385223A

  • Cracking catalyst, preparation method and application

    CN114425432A

  • Petroleum hydrocarbon catalytic cracking catalyst

    CN114797962A

  • Metal-modified zeolite for catalytic cracking of heavy oils and process for producing light olefins

    US20150165427A1