Catalytic cracking catalyst as well as preparation method and application thereof
Through the combination of aluminum sol and molecular sieve, a catalyst with high wear resistance and heavy oil conversion ability is prepared, which solves the shortcomings of existing catalysts in heavy oil conversion and light olefin yield, and achieves higher catalytic cracking performance.
Patent Information
- Application Number
- CN202310376748.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-15
AI Technical Summary
Existing catalytic cracking catalysts cannot simultaneously meet the requirements for higher wear resistance, heavy oil conversion capacity and low carbon olefin yield.
Aluminum sol is mixed and beaten with clay, molecular sieves and water, and the catalyst is prepared after drying and roasting. The Al element in the aluminum sol is mainly in the medium and high polymerization state, and is combined with Y-type and ZSM-5 type molecular sieves to improve the cohesion and stability of the catalyst. Cracking performance.
It significantly improves the catalyst's wear resistance, heavy oil conversion capacity and light olefin yield, reduces the monomer aluminum content, enhances the bonding performance and pore volume retention, and improves the catalytic cracking performance.
Smart Images

Figure CN118767982A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalytic cracking, and in particular to a catalytic cracking catalyst and a preparation method and application thereof. Background Art
[0002] my country's external dependence on oil is as high as 72%. Realizing efficient utilization of oil resources is a major demand for ensuring national energy security. Fluidized catalytic cracking (FCC) is the most important means of secondary processing of crude oil. Looking at the development history of catalytic cracking, the development of catalysts has strongly promoted the transformation of catalytic cracking. Under the new situation, the oil refining industry is facing the objective demand of heavy raw materials and the transformation of products from fuel oil to low-carbon olefins. How to improve the cracking activity of catalysts, product selectivity and wear resistance has become an important research direction. At present, FCC catalysts are mainly composed of molecular sieves, kaolin and binders. However, for the macromolecules of raw heavy oil, they cannot directly enter the molecular sieve pores for cracking. They need to be pre-cracked into small molecules by the matrix (kaolin, binder), and then cracked into target products by the molecular sieve. Therefore, the acidity, adhesion and pore structure of the binder will have an important impact on the activity and wear resistance of the catalyst.
[0003] Commonly used binders are silica sol, pseudo-boehmite and alumina sol. Literature shows that silica sol will form a high content of mesopores and macropores after calcination, but it has no acidity, weak cracking performance, and Na + It has a strong affinity with the acid center of the molecular sieve, resulting in a decrease in the acidity of the catalyst. Pseudo-boehmite will form alumina materials with abundant mesopores after being calcined with nitric acid, which has L acid and cracking activity. In comparison, the alumina formed after the calcination of aluminum sol has less mesopores, small pore volume, and single performance, and is only used to improve mechanical strength. Therefore, it has been less studied.
[0004] The US patent application US4028216A first introduced in detail the preparation method of metallic aluminum sol. This method has a simple process flow and is easy to operate. However, since aluminum sol is prepared by electrolysis of aluminum hydroxide, the production cost is high and a large amount of electricity is consumed. At the same time, the generation of hydrogen during the preparation process also poses a safety hazard, and the hydrochloric acid used will corrode the equipment. Chinese patent application CN101087653A provides a method of combining a precursor solution or suspension of an aluminum-containing inorganic oxide with a molecular sieve and other compounding reagents to form a catalyst slurry; after aging, the aluminum atoms of the aluminum-containing precursor in the form of oligomers (with a sharp peak at 62-63ppm) are generated. 27Al NMR peak), and made into molecular sieve catalyst particles. This method can improve the wear resistance of the catalyst. Chinese patent application CN110876948A discloses a method for preparing aluminum sol and catalytic cracking catalyst, wherein metallic aluminum and hydrochloric acid are reacted under ultrasonic conditions, and the prepared aluminum sol has a high Alb content and a high (Ala+Alb) content, and has good stability and bonding performance. Summary of the invention
[0005] The purpose of the present invention is to overcome the technical problem that the catalytic cracking catalyst in the prior art cannot simultaneously meet the requirements of high wear resistance, heavy oil conversion capacity and low carbon olefin yield, and to provide a catalytic cracking catalyst and a preparation method thereof, the method and application. The catalyst prepared by the preparation method can improve the wear resistance, heavy oil conversion capacity and low carbon olefin yield of the catalytic cracking catalyst.
[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a catalytic cracking catalyst, wherein the method comprises the following steps:
[0007] (1) mixing aluminum sol with clay, molecular sieve, water and optionally a binder to obtain a catalyst slurry; the molecular sieve includes a Y-type molecular sieve and a ZSM-5 type molecular sieve;
[0008] (2) drying and calcining the catalyst slurry obtained in step (1) to obtain a catalytic cracking catalyst;
[0009] Among them, in the aluminum sol, Al 2 O 3 The aluminum content is 19-24% by weight, the aluminum chlorine mass ratio of the aluminum sol is above 1.5, and the aluminum sol 27 In the Al NMR spectrum, there are characteristic peaks at chemical shifts of 62.5 and 64.5, and no characteristic peak at chemical shift 0.
[0010] Preferably, the method for preparing the aluminum sol comprises the following steps:
[0011] S1. Under the condition of temperature of 65-90° C., a first aluminum source and an acid are subjected to a first contact reaction;
[0012] S2, adjusting the pH value of the reaction product obtained in step S1 to 2-3;
[0013] S3, contacting the slurry obtained in step S2 with a second aluminum source to perform a second contact reaction, wherein the temperature of the second contact reaction is 60-80° C. to obtain aluminum sol.
[0014] Preferably, in step (1), based on the total amount of the molecular sieve used, the mass ratio of the Y-type molecular sieve to the ZSM-5 type molecular sieve is 5-10:1, more preferably 5-7:1.
[0015] The second aspect of the present invention provides a catalytic cracking catalyst prepared by the preparation method described in the first aspect.
[0016] The third aspect of the present invention provides a use of the catalytic cracking catalyst described in the second aspect in a heavy oil hydrocatalytic cracking reaction.
[0017] The preparation method provided by the present invention uses aluminum sol as one of the binders, and the Al element in the aluminum sol is mainly Al 13 The aluminum sol is present in the form of tetracoordinate aluminum, and the aluminum sol substantially does not contain monomer aluminum. The presence of tetracoordinate aluminum makes the aluminum sol have better adhesion, thereby improving the wear resistance of the catalyst, the heavy oil conversion capacity and the yield of light olefins.
[0018] The preparation method provided by the present invention selects the aluminum sol provided by the present invention to cooperate with the Y-type molecular sieve and the ZSM-5 type molecular sieve, thereby improving the macromolecular cracking ability of the catalyst and simultaneously improving the yield of light olefins. For example, the Y-type molecular sieve has a larger pore structure and is prone to bimolecular reaction, but the yield of light olefins is low; when the ZSM-5 type molecular sieve has a smaller pore size, the cracking performance of heavy oil macromolecules is reduced, but the yield of light olefins is higher. When only the Y-type molecular sieve or the ZSM-5 type molecular sieve is selected, the heavy oil conversion ability and the light olefin yield of the catalyst cannot be improved simultaneously. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is the aluminum sol in Example 1 of the present invention 27 Al NMR spectrum.
[0020] Figure 2 is the aluminum sol in Comparative Example 1 of the present invention 27 Al NMR spectrum. DETAILED DESCRIPTION
[0021] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0022] A first aspect of the present invention provides a method for preparing a catalytic cracking catalyst, wherein the method comprises the following steps:
[0023] (1) mixing aluminum sol with clay, molecular sieve, water and optionally a binder to obtain a catalyst slurry; the molecular sieve includes a Y-type molecular sieve and a ZSM-5 type molecular sieve;
[0024] (2) drying and calcining the catalyst slurry obtained in step (1) to obtain a catalytic cracking catalyst;
[0025] Among them, in the aluminum sol, Al 2 O 3 The aluminum content is 19-24% by weight, the aluminum chlorine mass ratio of the aluminum sol is above 1.5, and the aluminum sol 27 In the Al NMR spectrum, there are characteristic peaks at chemical shifts of 62.5 and 64.5, and no characteristic peak at chemical shift 0.
[0026] In the preparation method provided by the present invention, aluminum sol mainly containing Al element in medium and high polymer states is selected as one of the binders for preparing the catalytic cracking catalyst, and is combined with Y-type molecular sieve, ZSM-5 type molecular sieve and other raw materials, which can significantly improve the wear resistance and heavy oil conversion capacity of the catalytic cracking catalyst.
[0027] Usually, in the aluminum sol 27 In the Al NMR spectrum, the δ (chemical shift) of 60-70 corresponds to the characteristic peak of the tetracoordinated aluminum species of medium and high polymer aluminum, and the δ of 0 corresponds to the characteristic peak of monomer aluminum. The existence form of the Al element can be determined based on the peak area of the characteristic peak.
[0028] In the preparation method provided by the present invention, in the aluminum sol, one of the binders 27 In the Al NMR spectrum, there are characteristic peaks at δ of 62.5 and 64.5, and there is no characteristic peak at δ of 0, which indicates that the Al element in the aluminum sol is mainly in medium and high polymer states, and basically does not contain monomer aluminum. The presence of tetracoordinated aluminum makes the aluminum sol have better adhesion. When used to prepare catalytic cracking catalysts, it can better retain the pore volume of the catalyst, overcome the pore blocking phenomenon existing in the traditional aluminum sol used in the catalyst, and thus improve the catalytic cracking performance of the catalytic cracking catalyst.
[0029] In the present invention, it can be understood that the Al element being mainly in medium and high polymer states means that more than 60% of the Al element exists in the form of medium and high polymer states. The aluminum sol substantially does not contain monomer aluminum, which means that the content of Al element in the form of monomer aluminum is less than 10%. By reducing the content of monomer aluminum and increasing the degree of polymerization of aluminum species, the bonding performance of the aluminum sol is significantly improved, thereby improving the wear resistance and catalytic cracking performance of the catalytic cracking catalyst.
[0030] According to the present invention, preferably, the aluminum-chlorine mass ratio of the aluminum sol is 1.5-1.8. A higher aluminum-chlorine mass ratio increases the degree of polymerization of aluminum species in the aluminum sol and reduces the content of free chlorine; preferably, the pH of the aluminum sol is above 3.5, and more preferably 3.5-3.7. Within this pH value range, the influence of the aluminum sol on the molecular sieve framework during the preparation of the catalyst can be reduced, thereby making the prepared catalytic cracking catalyst have better wear resistance and mechanical strength.
[0031] According to the present invention, preferably, the total acid content of the aluminum sol is 0.4-0.7 mmol / g, and more preferably 0.5-0.6 mmol / g. Aluminum sol has a higher acid content, and using it as one of the raw material binders for preparing the catalyst can increase the acidity of the matrix, which is beneficial to improving the heavy oil cracking ability of the catalytic cracking catalyst.
[0032] According to the present invention, preferably, the aluminum sol has a specific surface area of 105-200m after being calcined at 500°C for 1.5h. 2 / g, pore volume is 0.14-0.2cm 3 / g; preferably, the aluminum sol is calcined at 500°C for 1.5h and then hydrothermally aged at 800°C for 17h to have a specific surface area of 60-120m 2 / g, pore volume is 0.18-0.2cm 3 / g. The aluminum sol provided by the present invention still has a good pore structure after aging treatment, which is more conducive to improving the heavy oil hydrocracking performance of the catalytic cracking catalyst.
[0033] According to the present invention, preferably, the method for preparing the aluminum sol comprises the following steps:
[0034] S1. Under the condition of temperature of 65-90° C., a first aluminum source and an acid are subjected to a first contact reaction;
[0035] S2, adjusting the pH value of the reaction product obtained in step S1 to 2-3;
[0036] S3, contacting the slurry obtained in step S2 with a second aluminum source to perform a second contact reaction, wherein the temperature of the second contact reaction is 60-80° C. to obtain aluminum sol.
[0037] According to the present invention, preferably, the first aluminum source and the second aluminum source are each independently selected from at least one of aluminum hydroxide, aluminum ingots, aluminum flakes, aluminum chips, aluminum powder, aluminum chloride, aluminum nitrate, pseudo-boehmite, boehmite, bauxite and aluminum isopropoxide; further preferably, the first aluminum source and the second aluminum source are each independently selected from at least one of aluminum hydroxide, aluminum flakes, aluminum chips, aluminum powder, aluminum isopropoxide and aluminum chloride.
[0038] According to the present invention, preferably, the added amount of the second aluminum source is 0.2-0.6 times of the first aluminum source, and more preferably 0.2-0.5 times.
[0039] According to the present invention, in step S1, from the perspective of improving the uniformity of the contact reaction, preferably, in step S1, the first contact reaction is carried out under stirring conditions, and the stirring can be carried out in a conventional manner, which is not particularly limited in the present invention, for example, mechanical stirring, magnetic stirring, etc. can be used. Preferably, the stirring speed is 300-500 rpm.
[0040] According to the present invention, in step S1, preferably, the time of the first contact reaction is 6-20 hours, and more preferably 8-20 hours.
[0041] According to the present invention, in step S1, preferably, the mass ratio of the amount of the acid added to the amount of the aluminum element added is 0.6-1.5:1, and more preferably 0.6-1.2:1, wherein the acid is calculated as acid radical, and the aluminum element here refers to total aluminum, that is, the sum of the aluminum elements in the first aluminum source and the second aluminum source.
[0042] In the present invention, in step S1, the acid can be added all at once or in steps, preferably in steps, and more preferably in two steps. In the embodiment where the acid is added in two steps, preferably, the amount of acid added in the first step is 40-70% by weight of the total acid amount, stirred for 2-10 hours, and then the remaining acid is added to continue and complete the first contact reaction.
[0043] According to the present invention, in step S1, preferably, the acid is selected from organic acid and / or inorganic acid, and more preferably a mixture of organic acid and inorganic acid. The aluminum sol prepared by this preferred embodiment is used as one of the raw material binders for preparing the catalyst, which is more conducive to increasing the pore volume of the matrix. When the acid is an organic acid and an inorganic acid, the ratio of the two is selected in a wide range. Preferably, the weight ratio of the organic acid: inorganic acid is 0.02-0.2:1.
[0044] According to the present invention, preferably, the inorganic acid is selected from at least one of hydrochloric acid, sulfuric acid and phosphoric acid, and more preferably hydrochloric acid.
[0045] According to the present invention, preferably, the organic acid is selected from at least one of formic acid, acetic acid, propionic acid, oxalic acid and citric acid.
[0046] In the present invention, the acid is preferably in the form of an aqueous solution of the acid. In the embodiment where the acid is an inorganic acid, preferably, the concentration of the acid is 5-20% by weight, more preferably 12-18% by weight; in the embodiment where the acid is an organic acid, preferably, the concentration of the acid is 10-12% by weight, more preferably 10-11% by weight; in the embodiment where the acid is a mixture of an organic acid and an inorganic acid, preferably, the concentration of the acid is 5-25% by weight, more preferably 12-20% by weight.
[0047] According to the present invention, in step S2, as long as the pH value of the reaction product obtained in step S1 can be adjusted to 2-3, the range of selection of the added regulator is relatively wide. Preferably, at least one of ammonium salt, inorganic base and organic base is used to adjust the pH value of the reaction product obtained in step S1. The inorganic base is preferably selected from at least one of ammonia water, sodium hydroxide and potassium hydroxide. The organic base is preferably selected from quaternary ammonium salts, and more preferably at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide and tetrapropylammonium hydroxide.
[0048] Preferably, the pH value of the reaction product obtained in step S1 is adjusted to 2.1-2.8, which is beneficial to improving the yield of medium and high polymer aluminum species in the obtained aluminum sol, thereby improving the bonding performance of the aluminum sol and further improving the heavy oil conversion capacity of the catalytic cracking catalyst.
[0049] According to the present invention, in step S3, the slurry obtained in step S2 is contacted with a second aluminum source to carry out a second contact reaction. From the perspective of improving the uniformity of the contact reaction, preferably, the second contact reaction is carried out under stirring conditions. The stirring method and parameters can refer to the method in step S1, which will not be repeated here.
[0050] According to the present invention, in step S3, preferably, the time of the second contact reaction is 5-20 hours, and more preferably 5-16 hours.
[0051] According to the present invention, step S3 further comprises cooling the product system obtained by the second contact reaction, and then filtering to obtain the aluminum sol. The present invention has no particular limitation on the cooling and filtering, and can be performed in a conventional manner.
[0052] In the present invention, the type of clay is not particularly limited, and clays conventionally defined in the art are applicable to the present invention. Preferably, in step (1), the clay is selected from at least one of kaolin, montmorillonite, diatomaceous earth, halloysite, saponite, rectorite, sepiolite, attapulgite, hydrotalcite and bentonite, preferably kaolin.
[0053] In the present invention, the type of binder is not particularly limited, and the binders conventionally defined in the art are applicable to the present invention. Preferably, in step (1), the binder is selected from at least one of pseudo-boehmite, silica sol and boehmite, preferably pseudo-boehmite. In the present invention, pseudo-boehmite is usually acidified before use, and the pseudo-boehmite acidification process uses hydrochloric acid and an acidification method well known to those skilled in the art.
[0054] According to the present invention, preferably, the amount of the aluminum sol, clay, molecular sieve, water and optionally the binder is such that in the prepared catalyst, based on the dry weight of the catalyst slurry, the content of the aluminum sol is 6-20% by weight, for example, it can be 6% by weight, 7% by weight, 8% by weight, 9% by weight, 10% by weight, 11% by weight, 12% by weight, 13% by weight, 14% by weight, 15% by weight, 16% by weight, 17% by weight, 18% by weight, 19% by weight, 20% by weight and values between any two groups, and the content of the clay is 20-40% by weight, for example, it can be 20% by weight, 25% by weight, 30% by weight, 35% by weight, 40% by weight and values between any two groups. The content of the binder is 10-30% by weight, for example, it can be 10% by weight, 15% by weight, 20% by weight, 25% by weight, 30% by weight and any values between two groups; the content of the molecular sieve is 20-50% by weight, for example, it can be 20% by weight, 25% by weight, 30% by weight, 35% by weight, 40% by weight, 45% by weight, 50% by weight and any values between two groups; further preferably, the content of the aluminum sol is 6-15% by weight, the content of the clay is 20-35% by weight, the content of the binder is 10-20% by weight, and the content of the molecular sieve is 20-45% by weight; wherein the aluminum sol is calculated as alumina. The present invention adopts a material rich in ε-Al 13 Sol can improve the mechanical strength of the catalyst and effectively retain the micropore specific surface area and micropore volume.
[0055] According to the present invention, preferably, in step (1), Y-type molecular sieve and ZSM-5 molecular sieve are added in sequence for mixing and slurrying. The advantage of adopting this preferred embodiment is that the yield of light olefins is increased while the macromolecular cracking ability of the material is increased.
[0056] According to the present invention, preferably, in step (1), the silicon-aluminum molar ratio of the Y-type molecular sieve is 2.5-5, and the silicon-aluminum molar ratio of the ZSM-5 type molecular sieve is 20-50.
[0057] According to the present invention, preferably, in step (1), based on the total amount of the molecular sieve, the mass ratio of the Y-type molecular sieve to the ZSM-5 type molecular sieve is 5-10:1, for example, it can be 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1, 10:1 and values between any two groups, further preferably 5-7:1, and even more preferably 5-6:1.
[0058] According to the present invention, preferably, in step (1), the solid content of the catalyst slurry is 20-50% by weight, preferably 20-40% by weight.
[0059] In the present invention, the drying conditions in step (2) can be selected in a wide range. Preferably, in step (2), the drying conditions include: a temperature of 100-150° C. and a time of 2-12 hours.
[0060] In the present invention, the range of selection of the calcination conditions in step (2) is relatively wide. Preferably, in step (2), the calcination conditions include: a temperature of 500-600°C and a time of 1-6 hours. More preferably, in step (2), the calcination conditions include: a temperature of 500-550°C and a time of 1-4 hours.
[0061] According to a specific preferred embodiment of the present invention, the preparation method of the catalytic cracking catalyst comprises the following steps:
[0062] (1) Clay and water are slurried, and acidified pseudo-boehmite is added (pseudo-boehmite is mixed with water, and then hydrochloric acid is added thereto under stirring to acidify until it is in a peptized state), and stirred to obtain slurry A; Y-type molecular sieve is then added and stirred for 30-60 minutes to obtain slurry B; ZSM-5 molecular sieve and aluminum sol are then added and stirred for 20-40 minutes to obtain a catalyst slurry (solid content is 20-40% by weight). Based on the total amount of the molecular sieve, the Y-type molecular sieve (silicon-aluminum molar ratio The mass ratio of the aluminum sol, the clay, the molecular sieve water and the optional binder is 5-7:1; the amount of the aluminum sol, the clay, the molecular sieve water and the optional binder is such that, in the prepared catalyst, the content of the aluminum sol is 6-15% by weight, the content of the clay is 20-35% by weight, the content of the binder is 10-20% by weight, and the content of the molecular sieve is 20-45% by weight, based on the dry weight of the catalyst slurry; wherein the aluminum sol is calculated as aluminum oxide;
[0063] (2) The catalyst slurry obtained in step (1) is spray dried and calcined at a drying temperature of 100-150° C. for 1-4 h and a calcination temperature of 500-550° C. for 1-4 h to obtain a catalytic cracking catalyst.
[0064] The second aspect of the present invention provides a catalytic cracking catalyst prepared by the preparation method described in the first aspect.
[0065] Using the aluminum sol provided by the present invention as a binder for a catalytic cracking catalyst has the advantages of low wear index, high mechanical strength, and high pore retention.
[0066] The third aspect of the present invention provides a use of the catalytic cracking catalyst described in the second aspect in a heavy oil hydrocatalytic cracking reaction.
[0067] The present invention will be described in detail below by way of examples, but the scope of the present invention is not limited thereby. In the following examples and comparative examples,
[0068] The aluminum content and aluminum-chlorine mass ratio in the prepared aluminum sol were determined by the method specified in RIPP34-90 of "Petrochemical Analysis Method (RIPP Test Method)";
[0069] The pH value of aluminum sol was measured using a pH meter (manufacturer: Mettler-Toledo);
[0070] Aluminum sol 27 Al NMR spectra were measured using a nuclear magnetic resonance spectrometer (manufacturer: Bruker, model: AVANCEⅢ600WB), and the existence form of Al element in aluminum sol was determined using a nuclear magnetic resonance spectrometer;
[0071] The pore structure of aluminum sol was measured using a static nitrogen adsorption instrument (manufacturer: Quantachrome Company, model: Autosorb6B);
[0072] The acid content of the aluminum sol was measured using a programmed temperature desorption instrument (manufacturer: Micromeritics, model: AutochemⅡ2920).
[0073] Example 1
[0074] (1) heating 360 g of a 16 wt % hydrochloric acid solution to 80° C., adding 67 g of an aluminum sheet, maintaining the temperature, and performing a first contact reaction at a stirring rate of 500 rpm for 18 h;
[0075] (2) cooling the reaction product obtained in step (1) to 65° C., slowly dropping ammonia water into the reaction product to adjust the pH value of the solution to 2.6;
[0076] (3) Slowly add 17 g of aluminum chips to the liquid obtained in step (2), control the temperature at 75°C, continue stirring, and carry out the second contact reaction for 10 hours. After the reaction is completed, wait for the product to cool to ambient temperature (25°C, the same below), filter, and obtain a 23.5 wt% (in terms of Al 2 O 3 Aluminum sol P1 (calculated).
[0077] The pH value of P1 is 3.5, the aluminum-chlorine mass ratio is 1.52, and the total acid content is 0.56 mmol / g. The BET specific surface area and pore volume of P1 after calcination at 500℃ for 1.5h and hydrothermal aging at 800℃ for 17h are shown in Table 1.
[0078] P1 27 Al NMR spectrum Figure 1 As shown, from Figure 1 It can be seen that there are characteristic peaks of tetracoordinate aluminum species of medium-polymerized aluminum at δ of 62.5 and 64.5, and a characteristic peak of tetracoordinate aluminum species of high-polymerized aluminum at δ of 70 (partially overlapping with the characteristic peak at δ of 65 in the figure), and there is no characteristic peak of monomeric aluminum at δ of 0. It can be seen that the Al element in P1 mainly exists in medium and high-polymerized forms, and basically does not contain monomeric aluminum.
[0079] 112g of kaolin and 100g of water were slurried, and then 430g of acidified pseudo-boehmite was added (the pseudo-boehmite was mixed with water, and then hydrochloric acid was added thereto under stirring to acidify until it was in a peptized state), and stirred to obtain slurry A; 103g of HRY-1 molecular sieve (silicon-aluminum molar ratio was 3.5) was added and stirred for 30min to obtain slurry B; 16.2g of ZSM-5 molecular sieve (silicon-aluminum molar ratio was 24) and 178g of aluminum sol were added, and stirred for 20min to obtain a catalyst slurry (solid content was 30% by weight), in which, based on the dry weight of the catalyst slurry, the content of HRY-1 molecular sieve was 30% by weight, the content of ZSM-5 molecular sieve was 5% by weight, the content of kaolin was 35% by weight, and the content of aluminum sol (based on Al 2 O 3 The content of pseudo-boehmite (in terms of Al 2 O 3 The catalyst slurry was spray dried at a temperature of 120° C., and the obtained catalyst microspheres were calcined at 550° C. for 2 h to obtain a catalytic cracking catalyst.
[0080] Comparative Example 1
[0081] 360 g of 16 wt% hydrochloric acid solution was heated to 80°C, 67 g of aluminum flakes were added, the temperature was maintained, and the contact reaction was carried out at a stirring rate of 500 rpm for 20 h. After the reaction was completed, the product was cooled to ambient temperature (25°C, the same below), filtered, and a 20 wt% (in terms of Al) concentration was obtained. 2 O 3 Aluminum sol D1 (calculated).
[0082] The pH value of D1 is 2.5, the aluminum-chlorine mass ratio is 1.2, and the total acid content is 0.33 mmol / g. The BET specific surface area and pore volume of D1 after calcination at 500℃ for 1.5h and hydrothermal aging at 800℃ for 17h are shown in Table 1.
[0083] D1 27 Al NMR spectrum Figure 2 As shown, from Figure 2 It can be seen that there is a characteristic peak of tetracoordinated aluminum species of mesopolymerized aluminum at δ of 64.5, and a characteristic peak of monomeric aluminum at δ of 0.
[0084] It can be seen from Table 1 that after calcination at 500℃ for 1.5h and hydrothermal aging at 800℃ for 17h, the BET specific surface area and pore volume of aluminum sol P1 are higher than those of aluminum sol D1. P1 can still maintain a relatively high pore structure after hydrothermal aging at 800℃ for 17h.
[0085] A catalytic cracking catalyst was prepared according to the method of Example 1.
[0086] Comparative Example 2
[0087] According to the method of Example 1, 112 g of kaolin and 100 g of water were slurried, and then 430 g of acidified pseudo-boehmite was added (the pseudo-boehmite was mixed with water, and then hydrochloric acid was added thereto under stirring to acidify until it was in a peptized state), and stirred to obtain slurry A; 120 g of HRY-1 molecular sieve (silicon-aluminum molar ratio was 3.5) was added and stirred for 30 min to obtain slurry B; and 178 g of the aluminum sol in Example 1 was added and stirred for 20 min to obtain a catalyst slurry (solid content was 30 wt %). In the catalyst slurry, the content of HRY-1 molecular sieve was 35 wt %, the content of kaolin was 35 wt %, and the content of aluminum sol (based on the dry weight of the catalyst slurry) was 1.34 wt %. 2 O 3 The content of pseudo-boehmite (in terms of Al 2 O 3 The catalyst slurry was spray dried at a temperature of 120° C., and the obtained catalyst microspheres were calcined at 550° C. for 2 h to obtain a catalytic cracking catalyst.
[0088] Table 1
[0089]
[0090] Example 2
[0091] The method of Example 1 is followed, except that in step (1), 360 g of 16 wt % hydrochloric acid is added in two steps, specifically, 180 g of 16 wt % hydrochloric acid solution is heated to 80° C., 67 g of aluminum flakes are added, and a first contact reaction is carried out at a stirring rate of 500 rpm for 10 h, and then 180 g of 16 wt % hydrochloric acid solution is added, and the first contact reaction is continued for 10 h. Other conditions are the same as those of Example 1, and a 23.2 wt % (in terms of Al) hydrochloric acid solution is obtained. 2 O 3 Aluminum sol P2 (calculated).
[0092] The pH value of P2 is 3.5, the aluminum-chlorine mass ratio is 1.54, and the total acid content is 0.57 mmol / g.
[0093] A catalytic cracking catalyst was prepared according to the method of Example 1.
[0094] Example 3
[0095] The method of Example 1 is followed, except that in step (2), tetrapropylammonium hydroxide solution is slowly added dropwise to adjust the pH value of the feed solution to 2.6. Other conditions are the same as in Example 1 to obtain a 23 wt% (in terms of Al 2 O 3 Aluminum sol P3 (calculated).
[0096] The pH value of P3 is 3.5, the aluminum-chlorine mass ratio is 1.52, and the total acid content is 0.52 mmol / g.
[0097] A catalytic cracking catalyst was prepared according to the method of Example 1.
[0098] Example 4
[0099] The catalyst was prepared according to the method of Example 1, except that in step (3), 17 g of aluminum flakes were added to the liquid obtained in step (2), and the time of the second contact reaction was controlled to be 16 h. Other conditions were the same as those of Example 1, and a catalyst with a concentration of 23.2 wt% (in terms of Al 2 O 3 Aluminum sol P4 (calculated).
[0100] The pH value of P4 is 3.5, the aluminum-chlorine mass ratio is 1.52, and the total acid content is 0.54 mmol / g.
[0101] A catalytic cracking catalyst was prepared according to the method of Example 1.
[0102] Example 5
[0103] The method of Example 1 is followed, except that in step (2), a mixture solution of ammonium chloride and ammonia water is slowly dripped to adjust the pH value of the feed solution to 2.6. Other conditions are the same as those of Example 1 to obtain a concentration of 23.8 wt % (in terms of Al 2 O 3 Aluminum sol P5 (calculated).
[0104] The pH value of P5 is 3.5, the aluminum-chlorine mass ratio is 1.5, and the total acid content is 0.5 mmol / g.
[0105] A catalytic cracking catalyst was prepared according to the method of Example 1.
[0106] Example 6
[0107] (1) heating a mixed solution of 350 g of 16 wt % hydrochloric acid and 55 g of 5 wt % acetic acid to 80° C., adding 67 g of aluminum chips, maintaining the temperature, and performing a first contact reaction at a stirring rate of 500 rpm for 15 h;
[0108] (2) cooling the reaction product obtained in step (1) to 60° C., slowly dropping ammonia water into the reaction product to adjust the pH value of the solution to 2.3;
[0109] (3) Add 17 g of aluminum chips to the liquid obtained in step (2), control the temperature at 75° C., continue stirring, and carry out the second contact reaction for 10 hours. After the reaction is completed, wait for the product to cool to ambient temperature (25° C., the same below), filter, and obtain a 23 wt% (in terms of Al 2 O 3 Aluminum sol P6 (calculated).
[0110] The pH value of P6 is 3.5, the aluminum-chlorine mass ratio is 1.56, and the total acid content is 0.58 mmol / g.
[0111] A catalytic cracking catalyst was prepared according to the method of Example 1.
[0112] Example 7
[0113] The alumina sol in Example 1 was selected and the method of Example 1 was followed, except that 109 g of kaolin and 100 g of water were slurried, and then 456 g of acidified pseudo-boehmite was added (the pseudo-boehmite was mixed with water, and then hydrochloric acid was added thereto under stirring to acidify until it was in a peptized state), and stirred to obtain slurry A; 110 g of HRY-1 molecular sieve (silicon-aluminum molar ratio of 3.5) was added and stirred for 30 min to obtain slurry B; 19.8 g of ZSM-5 molecular sieve (silicon-aluminum molar ratio of 24) and 147 g of alumina sol were added and stirred for 30 min to obtain a catalyst slurry (solid content of 30 wt %), in which, based on the dry weight of the catalyst slurry, the content of HRY-1 molecular sieve was 32 wt %, the content of ZSM-5 molecular sieve was 6 wt %, the content of kaolin was 34 wt %, and the content of alumina sol (based on Al 2 O 3 The content of pseudo-boehmite (in terms of Al 2 O 3 The catalyst slurry was spray dried at a drying temperature of 110° C., and the obtained catalyst microspheres were calcined at 500° C. for 2.5 h to obtain a catalytic cracking catalyst.
[0114] Test Case
[0115] The catalytic cracking catalysts prepared in the above-mentioned embodiments and comparative examples were subjected to heavy oil micro-reaction activity evaluation test and wear index test.
[0116] 1. Heavy oil micro-reactivity test
[0117] Before the heavy oil micro-reaction activity test, the catalytic cracking catalyst was subjected to hydrothermal aging treatment at 800°C and 100% steam for 17 h. The reaction raw material was Wu-mixed triple oil, the composition of which is shown in Table 2. The reaction conditions were: catalyst loading 5 g, temperature 500°C, weight space velocity 16 h -1 , agent-oil weight ratio is 3.2, and the reaction results are shown in Table 3.
[0118] Table 2
[0119] project data <![CDATA[Density (20 °C) / g / cm 3 > 0.8731 Refraction (70℃) 1.4682 <![CDATA[Viscosity (80 °C) / mm 2 / s]]> 17.56 Vacuum distillation range / ℃ Initial distillation point 189 5% 398 10% 418 30% 457 50% 497 70% 549 73.5% 560 Acid value / mgKOH / g 0.07 Residual carbon weight / % 0.7 Ash weight / % 0.05 S content weight / % 0.12 N content weight / % 0.11 C, H content weight / % C 86.43 H 13.53
[0120] Table 3
[0121]
[0122]
[0123] It can be seen from Table 3 that the use of Al-rich 13The catalyst composed of aluminum sol, Y-type molecular sieve and ZSM-5 molecular sieve has higher heavy oil cracking activity and higher ethylene and propylene yields.
[0124] 2. Wear index test
[0125] According to the method specified in RIPP29-90 of "Petrochemical Analysis Method (RIPP Test Method)", the 4h wear index of the catalytic cracking catalyst prepared above was evaluated. The results are shown in Table 4.
[0126] Table 4
[0127] catalyst Wear index / % Catalyst prepared by P1 0.91 Catalyst prepared by P2 0.85 Catalyst prepared by P3 0.82 Catalyst prepared by P4 0.93 Catalyst prepared by P5 0.97 Catalyst prepared by P6 0.78 Catalyst prepared by P7 1.01 Catalyst prepared by D1 1.75
[0128] As can be seen from Table 3 and Table 4, the aluminum sol of the present invention is selected by the method provided by the present invention. Compared with conventional industrial aluminum sol, the aluminum sol has better bonding performance and is used as a binder for preparing catalytic cracking catalysts, so that the prepared catalyst has a lower wear index and can obtain higher mechanical strength. It can be seen from Example 1 and Comparative Example 1 combined with Table 1 that the aluminum sol provided by the present application also has a higher pore retention.
[0129] In the preparation method provided by the present invention, aluminum sol is selected as one of the binders. In the process of preparing aluminum sol, the raw material price is low, more free chlorine is neutralized, so the raw material utilization rate is high, the whole preparation process conditions are mild, and high-quality aluminum sol products can be produced. The pH value of the prepared aluminum sol product is high, the Al element therein is mainly in medium and high polymer states, and basically does not contain monomer aluminum, the aluminum chlorine mass ratio is high, and the bonding performance is strong. After the catalyst is prepared, compared with the catalyst prepared by conventional aluminum sol, the catalyst has a low wear index, high mechanical strength and high pore retention under the same composition and colloidal solid content. It is used in combination with Y-type molecular sieve and ZSM-5 type molecular sieve, which can simultaneously improve the heavy oil conversion capacity of the catalytic cracking catalyst and the yield of light olefins.
[0130] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a catalytic cracking catalyst, characterized in that: The method comprises the following steps: (1) mixing aluminum sol with clay, molecular sieve, water and optionally a binder to obtain a catalyst slurry; the molecular sieve includes a Y-type molecular sieve and a ZSM-5 type molecular sieve; (2) drying and calcining the catalyst slurry obtained in step (1) to obtain a catalytic cracking catalyst; The aluminum sol has an aluminum content of 19-24% by weight in terms of Al2O3, an aluminum-chlorine mass ratio of more than 1.5, and a 27 In the Al NMR spectrum, there are characteristic peaks at chemical shifts of 62.5 and 64.5, and no characteristic peak at chemical shift 0.
2. The preparation method according to claim 1, wherein The aluminum sol has an aluminum-chlorine mass ratio of 1.5-1.8; and / or, the pH of the aluminum sol is above 3.5, preferably 3.5-3.7; and / or, the total acid content of the aluminum sol is 0.4-0.7 mmol / g, preferably 0.5-0.6 mmol / g; And / or, after the aluminum sol is calcined at 500°C for 1.5 hours, the specific surface area is 105-200m 2 / g, pore volume is 0.14-0.2cm 3 / g; preferably, the specific surface area is 60-120m 2 / g, pore volume is 0.18-0.2cm 3 / g.
3. The preparation method according to claim 1 or 2, wherein: The preparation method of the aluminum sol comprises the following steps: S1. Under the condition of temperature of 65-90° C., a first aluminum source and an acid are subjected to a first contact reaction; S2, adjusting the pH value of the reaction product obtained in step S1 to 2-3; S3, contacting the slurry obtained in step S2 with a second aluminum source to perform a second contact reaction, wherein the temperature of the second contact reaction is 60-80° C. to obtain aluminum sol.
4. The preparation method according to claim 3, wherein The first aluminum source and the second aluminum source are each independently selected from at least one of aluminum hydroxide, aluminum ingot, aluminum flake, aluminum chips, aluminum powder, aluminum chloride, aluminum nitrate, pseudo-boehmite, boehmite, bauxite, and aluminum isopropoxide; Preferably, the first aluminum source and the second aluminum source are each independently selected from at least one of aluminum hydroxide, aluminum flakes, aluminum chips, aluminum powder, aluminum isopropoxide and aluminum chloride; And / or, the added amount of the second aluminum source is 0.2-0.6 times of the first aluminum source, and more preferably 0.2-0.5 times.
5. The preparation method according to claim 3, wherein: In step S1, the first contact reaction is carried out under stirring conditions, and the stirring speed is 300-500 rpm; And / or, in step S1, the first contact reaction time is 6-20 hours, more preferably 8-20 hours; And / or, in step S1, the mass ratio of the amount of the acid added to the amount of the aluminum element added is 0.6-1.5:1, more preferably 0.6-1.2:1, wherein the acid is calculated as acid radical; And / or, in step S1, the acid is added in one step or in steps, more preferably in two steps, and more preferably in the first step, the amount of acid added is 40-70% by weight of the total acid, stirred for 2-10 hours, and then the remaining acid is added.
6. The preparation method according to claim 3, wherein: In step S1, the acid is selected from organic acid and / or inorganic acid, preferably organic acid and inorganic acid; Preferably, the inorganic acid is selected from at least one of hydrochloric acid, sulfuric acid and phosphoric acid, more preferably hydrochloric acid; Preferably, the organic acid is selected from at least one of formic acid, acetic acid, propionic acid, oxalic acid and citric acid.
7. The preparation method according to claim 3, wherein: In step S2, the pH value of the reaction product obtained in step S1 is adjusted to 2.1-2.8; Preferably, in step S2, at least one of an ammonium salt, an inorganic base and an organic base is used to adjust the pH value of the reaction product obtained in step S1; And / or, in step S3, the time of the second contact reaction is 5-20 hours, more preferably 5-16 hours.
8. The preparation method according to claim 1 or 2, wherein: In step (1), the clay is selected from at least one of kaolin, montmorillonite, diatomaceous earth, halloysite, saponite, rectorite, sepiolite, attapulgite, hydrotalcite and bentonite, preferably kaolin; And / or, in step (1), the binder is selected from at least one of pseudo-boehmite, silica sol and boehmite, preferably pseudo-boehmite.
9. The preparation method according to claim 1 or 2, wherein: The amounts of the aluminum sol, clay, molecular sieve, water and optionally the binder are such that, in the prepared catalyst, based on the dry weight of the catalyst slurry, the content of the aluminum sol is 6-20% by weight, the content of the clay is 20-40% by weight, the content of the binder is 10-30% by weight, and the content of the molecular sieve is 20-50% by weight; preferably, the content of the aluminum sol is 6-15% by weight, the content of the clay is 20-35% by weight, the content of the binder is 10-20% by weight, and the content of the molecular sieve is 20-45% by weight; wherein the aluminum sol is calculated as aluminum oxide; And / or, in step (1), Y-type molecular sieve and ZSM-5 molecular sieve are added in sequence for mixing and slurrying; And / or, in step (1), the silicon-aluminum molar ratio of the Y-type molecular sieve is 2.5-5, and the silicon-aluminum molar ratio of the ZSM-5 type molecular sieve is 20-50; Preferably, in step (1), based on the total amount of the molecular sieve, the mass ratio of the Y-type molecular sieve to the ZSM-5 type molecular sieve is 5-10:1, more preferably 5-7:1; And / or, in step (1), the solid content of the catalyst slurry is 20-50% by weight, preferably 20-40% by weight.
10. The preparation method according to claim 1 or 2, wherein: In step (2), the drying conditions include: temperature of 100-150° C. and time of 2-12 h; And / or, in step (2), the calcination conditions include: temperature of 500-600° C., time of 1-6 h; Preferably, in step (2), the calcination conditions include: temperature of 500-550° C. and time of 1-4 h.
11. The catalytic cracking catalyst obtained by the preparation method according to any one of claims 1 to 10.
12. Use of the catalytic cracking catalyst according to claim 11 in heavy oil hydrocatalytic cracking reaction.
Citation Information
Patent Citations
Preparation method for heavy oil catalytic cracking catalyst
CN105772074A
Alumina sol, preparation method and application thereof, catalytic cracking catalyst, preparation method of catalyst
CN107149917A
Adhesive, application of adhesive, catalytic cracking catalyst and preparation method of catalytic cracking catalyst
CN107297203A
Production process of aluminum sol and aluminum sol prepared by production process
CN112744847A
Prepn of catalytic cracking catalyst
CN1362472A
Cited By
Catalysts that include zeolites and related methods
US12779440B2