Preparation method and application of nano-bismuth selenium oxide
Nanose bismuth oxide is prepared by mixing selenium urea, bismuth compound and alkali, and reacting with sacrificial agent under ultrasonic wave, the efficiency and environmental protection problems of nanoselenium bismuth oxide preparation and hydrogen production are solved, achieving efficient and simple nanoselenium Bismuth oxide preparation and efficient hydrogen production.
Patent Information
- Application Number
- CN202111669948.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-12-31
AI Technical Summary
The prior art is difficult to efficiently, simply and reproducibly prepare nanoselenium bismuth oxide, and realize efficient and easy-to-use, green and environmentally friendly processes in the preparation of hydrogen.
By mixing selenium urea, bismuth compound, chelating agent and water, precipitating after adding alkali, sheet-like nanoselenium bismuth oxide is prepared, and mixed with the sacrificial agent under ultrasonic action to prepare hydrogen gas, catalyzed by decomposition of water.
The possibility of efficient preparation and industrial production of nanoselenium bismuth oxide is achieved, and under ultrasonic waves of 45kHz and 100W, the hydrogen production efficiency reaches 648μmol/g/h, which is significantly better than other piezoelectric material catalysts, and the process is green and environmentally friendly.
Smart Images

Figure CN114505083B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of piezoelectric catalysts, and in particular to a preparation method of nano-bismuth selenium oxide and an application thereof. Background Art
[0002] Piezoelectric materials can convert mechanical energy into electrical energy. Currently, they are widely used in many fields such as electroacoustic transducers and pressure sensors. Compared with the mature piezoelectric ceramic material conversion technology, piezoelectric catalysis technology was not discovered until the 1990s. The charge generated by piezoelectric action can also generate h with water. + 、e - , OH, O2 - Active species such as carbon dioxide, carbon dioxide, and carbon dioxide can further react to decompose water and degrade pollutants, thereby realizing the conversion of mechanical energy into electrical / chemical energy. Piezoelectric catalysis technology can not only enrich small mechanical energy in nature such as sound, water waves, vibrations, etc., but is also efficient, easy to operate, non-toxic and environmentally friendly, making piezoelectric catalysis research extremely promising.
[0003] Bi2O2Se material is a typical ferroelectric perovskite oxide. Ferroelectric semiconductor catalysts can generate internal spontaneous polarization electric fields, which can effectively drive electrons and photogenerated holes to quickly migrate to different locations on the surface of ferroelectric catalysts, thereby achieving separation and directional migration of electrons and holes on a spatial scale. In addition, Bi2O2Se has an extremely high carrier mobility (>20,000cm 2 V -1 s -1 at 2K) and a very small bandgap (~0.8eV). Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing nano-bismuth selenium oxide, which has a simple process, a short cycle and high repeatability.
[0005] The technical problem that the present invention needs to solve is to provide a nano-bismuth selenium oxide.
[0006] The technical problem that the present invention needs to solve is to provide an application of nano-bismuth selenium oxide in the preparation of hydrogen, which is efficient, easy to operate, and green and environmentally friendly.
[0007] In order to solve the above technical problems, the present invention provides a method for preparing nano-bismuth selenium oxide, which comprises:
[0008] (1) mixing selenourea, a bismuth compound, a chelating agent and water to obtain a precursor solution;
[0009] (2) adding a base to the precursor solution, reacting for a preset time, and separating the resulting precipitate to obtain a finished product of nano-selenium bismuth oxide;
[0010] Wherein, the molar ratio of Bi in the bismuth compound to Se in the selenourea is (1.8-5):1.
[0011] As an improvement of the above technical solution, the bismuth compound is selected from one or more of BiCl3, Bi2(SO4)3, and Bi(NO3)3·5H2O.
[0012] As an improvement of the above technical solution, the chelating agent is EDTA and / or disodium EDTA, and the molar ratio of EDTA and selenourea is (5-10):1.
[0013] As an improvement of the above technical solution, the base is selected from one or more of NaOH, KOH, and LiOH, and the molar ratio of the base to the thiourea is (8-15):1.
[0014] As an improvement of the above technical solution, the components are selected from NaOH and KOH, and the molar ratio of NaOH to KOH is (3-5):1.
[0015] Correspondingly, the present invention also discloses a nano-bismuth selenium oxide, which is prepared by the above-mentioned preparation method.
[0016] As an improvement of the above technical solution, it is in the form of a sheet with a thickness of 1 to 3 nm and a width of 100 to 500 nm.
[0017] Correspondingly, the present invention also discloses the use of the above-mentioned nano-bismuth selenium oxide in preparing hydrogen, wherein the nano-bismuth selenium oxide, a sacrificial agent and water are mixed to obtain a reaction system; and the reaction system is subjected to ultrasonic treatment to obtain hydrogen.
[0018] As an improvement of the above technical solution, the sacrificial agent is selected from one or more of ferrous sulfate, triethanolamine, and methanol;
[0019] In the reaction system, the concentration of the sacrificial agent is 0.001-0.01 mol / L.
[0020] As an improvement of the above technical solution, the power of the ultrasonic treatment is 40-100 W and the frequency is 20-100 kHz.
[0021] The implementation of the present invention has the following beneficial effects:
[0022] 1. The present invention prepares nano-bismuth selenide oxide by a coprecipitation method, which has a simple operation process, a short experimental cycle, high repeatability, and is suitable for industrial production.
[0023] 2. The nano-bismuth selenide oxide in the present invention is a ferroelectric perovskite oxide. The ferroelectric semiconductor catalyst can generate an internal spontaneous polarization electric field, which can effectively drive electrons and photogenerated holes to quickly migrate to different positions on the surface of the ferroelectric catalyst, thereby realizing the separation and directional migration of electrons and holes on a spatial scale, thereby enhancing the piezoelectric catalytic water splitting performance; in addition, by controlling the types and concentrations of the reactants in the present invention, the flaky nano-bismuth selenide oxide with a thickness of 1 to 3 nm can be obtained, which is easier to respond to acoustic vibrations and produce deformation, and is therefore more conducive to its enrichment and conversion of sound waves.
[0024] 3. The present invention catalytically decomposes nano-bismuth selenium oxide under the action of ultrasound to produce hydrogen. This process is green and environmentally friendly, and has high hydrogen production efficiency. Specifically, under 45kHz, 100W ultrasound, the hydrogen production efficiency can reach 648μmol / g / h, which is significantly better than other types of piezoelectric material catalysts. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a SEM image of nano-bismuth selenium oxide obtained in Example 1 of the present invention;
[0026] Figure 2 is the XRD pattern of nano-bismuth selenium oxide obtained in Example 2 of the present invention;
[0027] Figure 3 is a SEM image of nano-bismuth selenium oxide obtained in Example 2 of the present invention;
[0028] Figure 4 This is the ultraviolet-visible light spectrum of the nano-bismuth selenium oxide obtained in Example 2 of the present invention;
[0029] Figure 5 This is a comparison chart of the results of the hydrogen preparation test of Example 3 of the present invention and Comparative Example 1;
[0030] Figure 6 This is a graph showing the results of the hydrogen preparation test in Comparative Example 2. DETAILED DESCRIPTION
[0031] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.
[0032] As a first aspect of the present invention, the present invention provides a method for preparing nano-bismuth selenium oxide, which comprises the following steps:
[0033] (1) mixing selenourea, a bismuth compound, a chelating agent and water to obtain a precursor solution;
[0034] The bismuth compound is selected from one or more of BiCl3, Bi2(SO4)3, Bi(NO3)3·5H2O, but is not limited thereto. Preferably, the bismuth compound is BiCl3. In the precursor solution, the concentration of the bismuth compound is 5 to 10 mmol / L, exemplified by 5 mmol / L, 5.5 mmol / L, 6 mmol / L, 6.5 mmol / L, 7 mmol / L, 7.5 mmol / L, 8 mmol / L, 8.5 mmol / L, 9 mmol / L or 9.5 mmol / L, but is not limited thereto. Preferably, it is 6 to 9 mmol / L, and more preferably, it is 8 mmol / L.
[0035] Wherein, in the precursor solution, the concentration of selenourea is 2-8 mmol / L, exemplified by 2.5 mmol / L, 3 mmol / L, 3.5 mmol / L, 4 mmol / L, 4.5 mmol / L, 5 mmol / L, 5.5 mmol / L, 6 mmol / L, 6.5 mmol / L, 7 mmol / L or 7.5 mmol / L, but not limited thereto. Preferably, it is 3-5 mmol / L, and more preferably, it is 4 mmol / L.
[0036] Further, the molar ratio of Bi in the bismuth compound to Se in the selenourea is controlled to be (1.8-5):1, exemplarily 2:1, 3:1 or 4:1, but not limited thereto, preferably 2:1.
[0037] Wherein, the chelating agent is selected from EDTA and / or disodium EDTA, but not limited thereto. Disodium EDTA is preferred. In the precursor solution, the concentration of the chelating agent is 20 to 40 mmol / L, exemplified by 22 mmol / L, 24 mmol / L, 26 mmol / L, 28 mmol / L, 30 mmol / L, 32 mmol / L, 34 mmol / L or 38 mmol / L, but not limited thereto. Preferably, it is 30 to 40 mmol / L, and more preferably, it is 36 mmol / L.
[0038] Furthermore, the molar ratio of selenourea to chelating agent is controlled to be 1:(5-10), exemplarily 1:6, 1:7, 1:8, 1:9, preferably 1:9.
[0039] (2) adding a base to the precursor solution, reacting for a preset time, and separating the resulting precipitate to obtain a finished product of nano-selenium bismuth oxide;
[0040] The base is selected from one or more of NaOH, KOH, and LiOH, but is not limited thereto. Preferably, the base is selected from NaOH and KOH, and the molar ratio of NaOH to KOH is (3-5):1. By controlling the type and amount ratio of the base, sheet-like nano-bismuth selenium oxide can be prepared. Exemplarily, the molar ratio of NaOH to KOH is 3.5:1, 4:1 or 4.5:1, but is not limited thereto. Preferably, it is 4:1.
[0041] Specifically, the molar ratio of the base to the thiourea is (8-15):1, exemplified by 9:1, 10:1, 11:1, 12:1, 13:1 or 14:1, but not limited thereto, and preferably 10:1.
[0042] Furthermore, after adding the alkali, stirring is performed for 10 to 40 minutes, and then standing for 50 to 80 minutes, and then solid-liquid separation is performed, and the obtained precipitate is washed with alcohol and water in turn, and then dried to obtain the finished product of nano-selenium bismuth oxide.
[0043] The nano-bismuth selenide oxide prepared based on the above preparation method is in the form of a sheet, with a thickness of 1 to 3 nm and a width of 100 to 500 nm (specifically, the width refers to its maximum width in a non-thickness direction).
[0044] Correspondingly, the present invention also discloses a method for preparing hydrogen based on nano-bismuth selenide oxide, which comprises mixing nano-bismuth selenide oxide, a sacrificial agent and water to obtain a reaction system, and subjecting the reaction system to ultrasonic treatment to obtain hydrogen. Specifically, nano-bismuth selenide oxide is a ferroelectric perovskite oxide, which can generate a spontaneous polarization electric field inside, and the electric field can effectively drive electrons and photogenerated holes to quickly migrate to different positions on the surface of nano-bismuth selenide oxide; furthermore, the electric field is enhanced by the action of ultrasonic waves, thereby promoting the redox reaction at the solid-liquid interface, so that water decomposes to produce hydrogen.
[0045] The sacrificial agent can consume holes during the reaction, promote the separation of electron-hole pairs, and promote the decomposition of water, thereby improving the efficiency of hydrogen production. Specifically, the sacrificial agent is selected from one or more of triethanolamine, ferrous sulfate, and methanol. Triethanolamine is preferred.
[0046] In the reaction system, the concentration of the sacrificial agent is 0.001 to 0.01 mol / L, preferably 0.002 to 0.006 mol / L, and more preferably 0.005 mol / L.
[0047] The power of the ultrasonic treatment is 40-100W, and the frequency is 20-100kHz, but not limited thereto.
[0048] The nano-bismuth selenide oxide may be in the form of a sheet. Specifically, the sheet-shaped nano-bismuth selenide oxide has a thickness of 1 to 3 nm and a width of 100 to 500 nm.
[0049] The present invention is described below with specific embodiments:
[0050] Example 1
[0051] This embodiment provides a method for preparing nano-bismuth selenium oxide, which comprises:
[0052] (1) 0.25 mmol Bi(NO3)3·5H2O, 0.08 mmol SeC(NH2)2 and 0.8 mmol EDTA were added sequentially to 25 ml water in a glass beaker to obtain solution A;
[0053] (2) 8 mmol NaOH was added to solution A. After stirring for 30 min, the solution was allowed to stand for 1 h, washed with alcohol and water in sequence, and then the obtained powder was dried in a vacuum oven at 105 °C.
[0054] Example 2
[0055] This embodiment provides a method for preparing nano-bismuth selenium oxide, which comprises:
[0056] (1) 0.2 mmol BiCl3, 0.1 mmol SeC(NH2)2 and 0.9 mmol disodium EDTA were added sequentially into 25 ml of water in a glass beaker to obtain solution A;
[0057] (2) 2 mmol KOH and 8 mmol NaOH were added to solution A. After stirring for 30 min, the solution was allowed to stand for 1 h, washed with alcohol and water in sequence, and then the obtained powder was dried in a vacuum oven at 105 °C.
[0058] The nano-bismuth selenium oxide obtained in Example 2 was analyzed by X-ray diffractometer, and the results are as follows: Figure 2 As shown, it can be seen from the figure that the prepared product is bismuth selenide oxide.
[0059] The nano-bismuth selenium oxide obtained in Example 2 was analyzed using a scanning electron microscope, and the results are as follows: Figure 3 As shown in the figure, it can be seen that the thickness of nano-bismuth selenide oxide is 1 to 2 nm, and its width is 100 to 500 nm.
[0060] The nano-bismuth selenium oxide obtained in Example 2 was analyzed using an ultraviolet-visible spectrometer, and the results are as follows: Figure 4 As shown in the figure, it can be seen that the band gap of nano-bismuth selenide oxide is relatively small, which is 0.8eV.
[0061] Example 3
[0062] This embodiment provides a method for preparing hydrogen, which comprises placing 10 mg of nano-bismuth selenide oxide prepared in Example 2 into 100 mL of deionized water containing 0.005 mol / L of triethanolamine, and applying 45 kHz, 100 W ultrasound for 0 h, 1 h, 2 h, 3 h, 4 h and 5 h, respectively, and using a gas chromatograph (Techcomp GC-7900) with Ar as the carrier to analyze the amount of precipitated H2.
[0063] Figure 5 3 is an analysis chart of the amount of hydrogen produced. It can be seen from the chart that the nano-bismuth selenium oxide of Example 2 can assist in catalytic decomposition of water to produce hydrogen under the action of ultrasound. In an ultrasound wave of 45kHz and a power of 100W, the hydrogen production efficiency can reach 648μmol / g / h.
[0064] Example 4
[0065] This embodiment provides a method for preparing hydrogen, which comprises placing 10 mg of nano-bismuth selenide oxide prepared in Example 2 into 100 mL of deionized water containing 0.005 mol / L of triethanolamine, and applying 45 kHz, 100 W ultrasound for 0 h, 1 h, 2 h, 3 h, 4 h and 5 h, respectively, and using a gas chromatograph (Techcomp GC-7900) with Ar as the carrier to analyze the amount of precipitated H2.
[0066] Figure 5 3 is an analysis chart of the amount of hydrogen produced. It can be seen from the chart that the nano-bismuth selenium oxide of Example 1 can assist in catalytic decomposition of water to produce hydrogen under the action of ultrasound. In an ultrasound wave of 45kHz and a power of 100W, the hydrogen production efficiency can reach 186μmol / g / h.
[0067] Comparative Example 1
[0068] In this comparative example, 10 mg of nano-bismuth selenide oxide prepared in Example 2 was placed in 100 mL of deionized water and treated with 45 kHz, 100 W ultrasound for 0 h, 1 h, 2 h, 3 h, 4 h and 5 h, respectively, and the amount of precipitated H2 was analyzed using a gas chromatograph (Techcomp GC-7900) with Ar as the carrier.
[0069] The test results are as follows Figure 5 As shown, from Figure 5 It can be seen that without adding a sacrificial agent, hydrogen cannot be produced.
[0070] Comparative Example 2
[0071] In this comparative example, 10 mg of nano-bismuth selenide oxide prepared in Example 2 was placed in 100 mL of deionized water containing 0.005 mol / L of triethanolamine without ultrasonic treatment, and the amount of precipitated H2 was analyzed using a gas chromatograph (Techcomp GC-7900) with Ar as the carrier.
[0072] The test results are as follows Figure 6 As shown, from Figure 6 It can be seen that without ultrasonic treatment, hydrogen gas cannot be generated.
[0073] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. Application of nano-bismuth selenium oxide in the preparation of hydrogen, characterized in that: Mixing nano-bismuth selenium oxide, a sacrificial agent and water to obtain a reaction system; subjecting the reaction system to ultrasonic treatment to obtain hydrogen; Among them, the nano-bismuth selenide oxide is in the form of flakes, with a thickness of 1-3 nm and a width of 100-500 nm; The sacrificial agent is selected from one or more of ferrous sulfate, triethanolamine, and methanol; the concentration of the sacrificial agent in the reaction system is 0.001-0.01 mol / L; The power of the ultrasonic treatment is 40-100W and the frequency is 20-100kHz; Wherein, the preparation method of the nano-bismuth selenium oxide comprises: (1) mixing selenourea, a bismuth compound, a chelating agent and water to obtain a precursor solution; (2) adding a base to the precursor solution, reacting for a preset time, and separating the resulting precipitate to obtain a finished product of nano-selenium bismuth oxide; The bismuth compound is selected from one or more of BiCl3, Bi2(SO4)3, and Bi(NO3)3•5H2O, and the molar ratio of Bi in the bismuth compound to Se in selenourea is (1.8-5):1; The chelating agent is EDTA and / or EDTA disodium, and the molar ratio of EDTA and selenourea is (5-10):1; The base is selected from one or more of NaOH, KOH, and LiOH, and the molar ratio of the base to the selenourea is (8-15):
1.
2. The use according to claim 1, characterized in that The bismuth compound is selected from BiCl3.
3. The use according to claim 1, characterized in that The alkali is selected from NaOH and KOH, and the molar ratio of NaOH to KOH is 4:
1.
4. The use according to claim 1, characterized in that The nano-bismuth selenium oxide has a thickness of 1-2 nm and a width of 100-500 nm.
5. The use according to claim 1, characterized in that The sacrificial agent is triethanolamine; In the reaction system, the concentration of the sacrificial agent is 0.005 mol / L.
6. The use according to claim 1, characterized in that The power of the ultrasonic treatment was 100 W and the frequency was 45 kHz.