Bimetal cluster catalyst as well as preparation method and application thereof
Patent Information
- Application Number
- CN202310356753.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure BDA0004165921570000021 
Figure BDA0004165921570000071 
Figure BDA0004165921570000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical materials, and in particular relates to a bimetallic cluster catalyst and a preparation method and application thereof. Background Art
[0002] As fossil energy depletion and ecological environment become increasingly serious, the deep development of renewable biomass resources and their further substitution for traditional energy or petrochemical raw materials are widely recognized. The use of efficient catalytic technology to convert biomass resources into high-value-added platform compounds is expected to derive a large number of green chemicals with novel structures and functions.
[0003] As one of the important biomass-based platform compounds, 2,5-furandicarboxylic acid (FDCA) has great market application value. Among them, because it has a very similar chemical structure to fossil-based terephthalic acid (PTA), FDCA has attracted much attention as a synthetic monomer to replace PTA in the preparation of bulk polymers. The method of preparing FDCA by selective oxidation using 5-hydroxymethylfurfural (HMF) as a raw material and a heterogeneous catalytic system (mainly precious metal catalysts) is currently widely used.
[0004] [Modern Chemical Industry, 2019, 39(09): 135-140.] It was reported that nano copper oxide was used as a catalyst to catalyze the oxidation of 5-hydroxymethylfurfural to FDCA in a sodium hypochlorite reaction system, and the FDCA selectivity could reach up to 99.8%. However, this route will result in HMF in an alkaline reaction medium, which usually gives the intermediate 5-hydroxymethyl-2-furancarboxylic acid (HMFCA) with preferential oxidation of the aldehyde group. However, due to the presence of the carboxyl functional group in the HMFCA structure, further oxidation of the hydroxyl group is difficult, and it is usually necessary to increase the alkali concentration, temperature or pressure to improve the conversion efficiency. Therefore, it is urgent to develop a catalyst with good stability that can efficiently catalyze HMF to prepare 2,5-furandicarboxylic acid FDCA and reduce the amount of alkaline medium, which is of great significance for subsequent treatment. Summary of the invention
[0005] The present invention provides a bimetallic cluster catalyst, a preparation method and application thereof, the main purpose of which is to solve the technical problems of low efficiency and large amount of alkaline medium used in catalyzing HMF to prepare 2,5-furandicarboxylic acid FDCA.
[0006] In a first aspect, the present invention provides a bimetallic cluster catalyst, wherein the chemical formula of the bimetallic cluster catalyst is Cu 12-x Co x L, wherein L is 1,2-bis((E)-2-(1H-pyrazol-3-yl)benzylidene)hydrazine, and its chemical structure is Formula I:
[0007]
[0008] Among them, x=0.5-1.7.
[0009] Preferably, the Cu ions are divalent; and the Co ions are divalent.
[0010] In a second aspect, the present invention provides a method for preparing the above-mentioned bimetallic cluster catalyst, the method comprising the following steps:
[0011] (S1) obtaining 1,2-bis((E)-2-(1H-pyrazol-3-yl)benzylidene)hydrazine as ligand L;
[0012] (S2) the ligand L reacts with a metal copper salt to obtain a Cu pre-ligand;
[0013] (S3) the ligand L reacts with a metal cobalt salt to obtain a Co pre-ligand;
[0014] (S4) the Cu pre-ligand and the Co pre-ligand are mixed in the presence of a solvent to obtain a bimetallic cluster catalyst Cu 12-x Co x L crystal; wherein x=0.5-1.7.
[0015] Preferably, x is selected from any value among 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7 or any range therebetween.
[0016] Preferably, in step (S2), the mixing ratio of the ligand L to the metal copper salt is 0.022-0.026 mmol: 0.016-0.022 mmol.
[0017] Preferably, the mixing ratio of the ligand L to the metal copper salt is selected from any value among 0.022, 0.023, 0.024, 0.025, 0.026 or any range value between two mmol: any value among 0.016, 0.017, 0.018, 0.019, 0.020, 0.021, 0.022 or any range value between two mmol.
[0018] Preferably, in step (S3), the mixing ratio of the ligand L to the metal cobalt salt is 0.022-0.026 mmol: 0.016-0.022 mmol.
[0019] Preferably, the mixing ratio of the ligand L to the metal cobalt salt is selected from any value among 0.022, 0.023, 0.024, 0.025, 0.026 or any range value between two mmol: any value among 0.016, 0.017, 0.018, 0.019, 0.020, 0.021, 0.022 or any range value between two mmol.
[0020] Preferably, the ligand L, copper salt and solvent in step (S2) are kept at 130° C. to 150° C. for 48 to 96 hours in a vacuum sealed environment, and then cooled to room temperature to obtain the Cu pre-ligand; the solvent is ethanol and pyridine.
[0021] Preferably, the temperature in step (S2) is selected from any value among 130°C, 135°C, 140°C, 142°C, 145°C, 150°C or any range between two thereof.
[0022] Preferably, the time in step (S2) is selected from any value of 48h, 55h, 60h, 65h, 70h, 72h, 75h, 80h, 85h, 90h, 95h, 96h, or a range between any two of them.
[0023] Preferably, the ligand L, cobalt salt and solvent in step (S3) are kept at 130-150° C. for 48-96 hours in a vacuum sealed environment, and then cooled to room temperature to obtain Co pre-ligand; the solvent is ethanol and pyridine.
[0024] Preferably, the temperature in step (S3) is selected from any value among 130°C, 135°C, 140°C, 142°C, 145°C, 150°C or any range between two thereof.
[0025] Preferably, the time in step (S3) is selected from any value among 48h, 55h, 60h, 65h, 70h, 72h, 75h, 80h, 85h, 90h, 95h, 96h, or any range between two of them.
[0026] Preferably, in step (S4), the mass ratio of the Cu precursor ligand to the Co precursor ligand is 15:0.5-2.9.
[0027] Preferably, the mass ratio of the Cu pre-ligand to the Co pre-ligand in step (S4) is 15:1-2.9; preferably 15:1.5-2.9; preferably 15:2.0-2.9; preferably 15:2.5-2.9.
[0028] Preferably, the mass ratio of the Cu pre-ligand to the Co pre-ligand is 15 to any value among 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or the range value between any two of them.
[0029] Preferably, the metal copper salt is a divalent copper salt; and the metal cobalt salt is a divalent cobalt salt.
[0030] Preferably, the metal copper salt is CuCl2; and the metal cobalt salt is Co(OH)2.
[0031] Preferably, in step (S4), the Cu pre-ligand and the Co pre-ligand are mixed in the presence of a benzene solution and phenylacetylene, and are diffused using triethylamine and n-hexane as diffusion agents to obtain a bimetallic cluster catalyst Cu 12-x Co x L crystal; wherein x=0.5-1.7.
[0032] In a third aspect, the present invention provides use of the bimetallic cluster catalyst or the bimetallic cluster catalyst prepared by the above method in the preparation of 2,5-furandicarboxylic acid.
[0033] In a fourth aspect, the present invention provides a method for preparing 2,5-furandicarboxylic acid, the method comprising: synthesizing the 2,5-furandicarboxylic acid from 5-hydroxymethylfurfural through the action of a catalyst under alkaline medium conditions; wherein the catalyst is the above-mentioned bimetallic cluster catalyst or the bimetallic cluster catalyst prepared by the above-mentioned method.
[0034] Preferably, the method comprises: mixing sodium hydroxide, 5-hydroxymethylfurfural, a catalyst and sodium hypochlorite, and reacting to obtain 2,5-furandicarboxylic acid.
[0035] Preferably, the mixing ratio of the 5-hydroxymethylfurfural to the catalyst is 3 to 4:1, by weight.
[0036] Preferably, the mixing ratio of the 5-hydroxymethylfurfural to the catalyst is selected from any value of 3:1, 3.1:1, 3.2:1, 3.3:1, 3.4:1, 3.5:1, 3.6:1, 3.7:1, 3.8:1, 3.9:1, 4.0:1 or any range value between two of them.
[0037] Preferably, the mixing ratio of the 5-hydroxymethylfurfural, the catalyst, sodium hydroxide and sodium hypochlorite is 3-4 g: 1 g: 0.5-1 g: 20-40 mL, calculated by weight.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] 1) The bimetallic cluster catalyst prepared by the present invention has stable catalytic performance. As a non-precious metal catalyst, it can efficiently catalyze 5-hydroxymethylfurfural (HMF) to prepare 2,5-furandicarboxylic acid (FDCA) in an alkaline reaction medium; wherein the conversion rate of the 5-hydroxymethylfurfural is 100%, the yield of the 2,5-furandicarboxylic acid is 98.8-99.6%, and the purity is 99.8% to 99.9%.
[0040] 2) The non-precious metal catalyst prepared by the present invention is applied to the oxidation synthesis of FDCA by HMF, which can reduce the amount of alkaline medium used.
[0041] 3) The catalyst prepared by the present invention can be recycled and reused at least 10 times after being repeatedly washed with clean water and ethanol for multiple times. DETAILED DESCRIPTION
[0042] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0043] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0044] The following examples 1-6 are the processes for preparing the catalyst.
[0045] Example 1
[0046] (1) 4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-1H-pyrazole (11.6 g, 60 mmol) and 150 mL of CH2Cl2 were placed in a 500 mL two-necked flask under stirring at 45°C. Triethylamine (15 mL) was then added dropwise to the reaction mixture, and a water condenser was connected to the flask. The mixture was stirred for 30 minutes to obtain a clear colorless solution. Trityl chloride (16.7 g, 60 mmol) was dissolved in 100 mL of CH2Cl2 and added dropwise to the solution. After stirring for another 2 hours, the solvent was removed. The solid was washed with a small amount of methanol and an appropriate amount of petroleum ether, and then filtered to obtain 4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-1-tritylpyrazole.
[0047] (2) Pd(PPh3)4 (0.58 g, 0.5 mmol) was added to a mixture of 2-iodobenzaldehyde (2.32 g, 10 mmol), 4-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-1-tritylpyrazole (6.54 g, 15 mmol) and Cs2CO3 (2.00 g, 6 mmol), and 30 mL of 1,4-dioxane and 6 mL of H2O were added. The resulting mixture was stirred at 100°C under N2 atmosphere for another 24 hours. After the reaction solution was cooled to room temperature, it was extracted with CH2Cl2, the combined organic layers (CH2Cl2) were washed with saturated NaHCO3 aqueous solution, and the solvent was removed in vacuo to obtain the product 2-(1-trityl-1H-pyrazol-3-yl)-benzaldehyde.
[0048] (3) In a 250 mL flask, 2.82 g (6.81 mmol) of 2-(1-trityl-1H-pyrazol-3-yl)-benzaldehyde and 50 mL of MeOH, 50 mL of CH2Cl2 and 10 mL of HCl were added. The mixture was stirred at 45°C for 3 h, and then NaOH solution was slowly added to adjust the pH to 7-8. After extraction with CH2Cl2, the combined organic layers were dried over Na2SO4 and filtered. After the solvent was removed in vacuo, hydrazine hydrate (98% aqueous solution) (200 μL, 4 mmol) and 50 mL of EtOH were added. The resulting mixture was stirred at 90°C for 3 h. After the solvent was removed in vacuo, the ligand H2L1 was purified by ethyl acetate.
[0049] (4) Weigh the ligand H2L1 (8.5 mg, 0.025 mmol) and CuCl2 (2 mg, 0.02 mmol) into a thick-walled hard glass tube, then add 4 mL of anhydrous ethanol and 0.1 mL of pyridine, and then seal the tube with an oxyhydrogen flame machine and place it in a constant temperature oven. Raise the temperature to 140°C within 10 minutes and maintain it for 72 hours, then lower it to room temperature at a rate of 5°C per hour. After opening the glass tube, a colorless and transparent needle-shaped crystal Cu preligand is obtained.
[0050] (5) Weigh the ligand H2L1 (8.5 mg, 0.025 mmol) and Co(OH)2 (2 mg, 0.02 mmol) into a thick-walled hard glass tube, then add 4 mL of anhydrous ethanol and 0.1 mL of pyridine, and then seal the tube with an oxyhydrogen flame machine and place it in a constant temperature oven. Raise the temperature to 140°C within 10 minutes and maintain it for 72 hours, then lower it to room temperature at a rate of 5°C per hour. After opening the glass tube, a colorless and transparent needle-shaped crystal Co pre-ligand is obtained.
[0051] (6) Using a 5 mL transparent glass bottle without a lid, the Cu pre-ligand and the Co pre-ligand were dissolved in 1 mL of benzene solution in a ratio of 15:0.5, and then 0.01 mL of phenylacetylene was added to obtain a clear light yellow solution. The solution was placed in a sealed diffusion bottle with a mixed solution of triethylamine and n-hexane (volume ratio of 1:100) as a diffusion agent, kept away from light overnight, and the bimetallic cluster catalyst Cu was obtained after slow diffusion. 12-x Co x Ligand (x=0.5) crystals.
[0052] Embodiment 2-6
[0053] The difference between Example 2-6 and Example 1 is that the mixing ratio of the Cu pre-ligand and the Co pre-ligand is different, see Table 1 for details.
[0054] Comparative Example 1
[0055] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 is a copper single metal ligand catalyst.
[0056] Table 1. Proportion of pre-catalyst ligands and mixed metal clusters
[0057] catalyst Cu preligand / ㎎ Co preligand / ㎎ Bimetallic cluster catalysts <![CDATA[1 # ]]> 15 0.5 <![CDATA[Cu 12-x Co x Ligand (x = 0.5)]]> <![CDATA[2 # ]]> 15 1 <![CDATA[Cu 12-x Co x Ligand (x=0.7)]]> <![CDATA[3 # ]]> 15 1.5 <![CDATA[Cu 12-x Co x Ligand (x=1)]]> <![CDATA[4 # ]]> 15 2 <![CDATA[Cu 12-x Co x Ligand (x=1.2)]]> <![CDATA[5 # ]]> 15 2.5 <![CDATA[Cu 12-x Co x Ligand (x=1.5)]]> <![CDATA[6 # ]]> 15 2.9 <![CDATA[Cu 12-x Co x Ligand (x=1.7)]]> <![CDATA[7 # ]]> 15 / <![CDATA[Cu 12 Ligand]]>
[0058] The following Examples 7-14 use the catalysts prepared in Examples 1-6 and Comparative Example 1 to synthesize FDCA.
[0059] Example 7
[0060] Weigh 0.2 g of sodium hydroxide and add it to 100 mL of deionized water. Place the reactor in a water bath, stir at 120 rpm and turn on the heating. After heating to 35° C., add a certain amount of 5-hydroxymethylfurfural 1.26 g and a certain mass of catalyst in sequence. Add 10 mL of sodium hypochlorite (effective chlorine content 11%). Start timing, react for 0.5 h to 2 h, and take samples for analysis. See Table 2 for details.
[0061] Embodiment 8-14
[0062] The difference between Examples 8-14 and Example 7 is that the catalysts are different or the amounts of alkali solution or catalysts are different, as shown in Table 2.
[0063] Comparative Example 2
[0064] The difference between Comparative Example 2 and Example 7 is that the catalyst used is the catalyst of Comparative Example 1.
[0065] Comparative Example 3
[0066] The difference between Comparative Example 3 and Example 7 is that no catalyst is added.
[0067] Comparative Example 4
[0068] The difference between Comparative Example 4 and Example 7 is that the catalyst used is commercial nano copper oxide.
[0069] Table 2. Catalytic performance of different catalysts for the oxidation of 5-hydroxymethylfurfural to 2,5-furandicarboxylic acid
[0070]
[0071]
[0072] The data in Table 2 show that the HMF conversion rate in Examples 7-14 of the present invention is 100%, the FDCA yield is 99-99.6%, and the FDCA product purity can reach 99.8% to 99.9%. Comparative Example 2 uses a single copper metal catalyst, and the FDCA yield is 95%. Comparative Example 3 does not use a catalyst, and the FDCA yield is 1.1%. Comparative Example 4 uses commercial nano copper oxide, and the FDCA yield is 83%.
[0073] By comparing Example 7 and Example 8, both use 1# catalyst. After the amount of sodium hypochlorite in Example 8 is increased compared with Example 7, the yield of FDCA in Example 8 does not change, indicating that when the amount of the catalyst used in the present invention is reasonable, increasing the amount of alkaline medium does not affect the yield of FDCA. It further illustrates that the catalyst of the present invention has the ability to catalyze the synthesis of FDCA with a yield of 99%, has higher selectivity, and does not need to increase the amount of alkali solution to increase the FDCA yield. Under the condition of the presence of the catalyst of the present invention, increasing the amount of alkali solution has no obvious effect on the FDCA yield.
[0074] By comparing Example 7 and Example 9, both use 1# catalyst, but the amount of catalyst used in Example 8 is 0.8g, and the amount of catalyst used in Example 7 is 0.4g. After the amount of catalyst is increased, the FDCA yield does not change, indicating that when the amount of the catalyst used in the present invention is reasonable, the FDCA yield can reach 99% without more catalyst, further indicating that the catalyst of the present invention has high selectivity and excellent catalytic effect. When the ratio of the amount of reactants to the amount of catalyst is reasonable, increasing the amount of catalyst has no obvious effect on the FDCA yield.
[0075] By comparing Example 7 and Examples 10-14 with Comparative Example 4, under the conditions of the same catalyst dosage, the same reaction conditions, and the same reactant dosage, the yield of FDCA synthesized by the bimetallic cluster catalyst of the present invention is increased from 83% to 99% to 99.6% compared with the yield of FDCA synthesized by nano-copper oxide in the prior art; directly proving that the catalyst of the present invention has a stable and efficient effect on the catalytic synthesis of FDCA by HMF; indirectly proving that the use of the bimetallic cluster catalyst of the present invention to synthesize FDCA reduces the amount of alkaline medium.
[0076] By comparing Example 7 and Examples 10-14 with Comparative Example 2, under the same reaction conditions, the yield of FDCA synthesized using the bimetallic cluster catalyst of the present invention is increased from 95% to 99% compared with the yield of FDCA synthesized using a single copper catalyst, indicating that the catalytic efficiency of the copper-cobalt bimetallic catalyst is higher than that of the copper single metal catalyst.
[0077] By comparing Example 7 and Examples 10-14 with Comparative Example 3, under the same reaction conditions, the yield of FDCA synthesized by the bimetallic cluster catalyst of the present invention is increased from 1.1% to 99% compared with the yield of FDCA synthesized without any catalyst; this indicates that when FDCA is synthesized from HMF, the synthesis reaction is basically unable to successfully synthesize FDCA without the action of a catalyst, further proving that the bimetallic cluster catalyst of the present invention has the advantages of being stable and efficient for the catalytic synthesis of FDCA by HMF, and also provides a new and efficient catalyst for the catalytic synthesis of FDCA by HMF, thereby increasing the selectivity of the catalyst.
[0078] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A bimetallic cluster catalyst, characterized in that: The chemical formula of the bimetallic cluster catalyst is Cu 12-x Co x L, wherein L is 1,2-bis((E)-2-(1H-pyrazol-3-yl)benzylidene)hydrazine, and its chemical structure is Formula I: Among them, x=0.5-1.
7.
2. A bimetallic cluster catalyst as claimed in claim 1, characterized in that: The Cu ions are divalent; the Co ions are divalent.
3. The method for preparing the bimetallic cluster catalyst according to claim 1 or 2, characterized in that: The method comprises the following steps: (S1) obtaining 1,2-bis((E)-2-(1H-pyrazol-3-yl)benzylidene)hydrazine as ligand L; (S2) the ligand L reacts with a metal copper salt to obtain a Cu pre-ligand; (S3) the ligand L reacts with a metal cobalt salt to obtain a Co pre-ligand; (S4) the Cu precursor ligand and the Co precursor ligand are mixed in the presence of a solvent to obtain a bimetallic cluster catalyst Cu 12-x Co x L crystal; wherein x=0.5-1.
7.
4. The method for preparing a bimetallic cluster catalyst according to claim 3, characterized in that: In step (S2), the mixing ratio of the ligand L to the metal copper salt is 0.022-0.026 mmol: 0.016-0.022 mmol; Preferably, in step (S3), the mixing ratio of the ligand L to the metal cobalt salt is 0.022-0.026 mmol: 0.016-0.022 mmol; Preferably, the ligand L, copper salt and solvent in step (S2) are kept at 130° C. to 150° C. for 48 to 96 hours in a vacuum sealed environment, and then cooled to room temperature to obtain a Cu pre-ligand; the solvent is ethanol and pyridine; Preferably, the ligand L, cobalt salt and solvent in step (S3) are kept at 130-150° C. for 48-96 hours in a vacuum sealed environment, and then cooled to room temperature to obtain Co pre-ligand; the solvent is ethanol and pyridine.
5. The method for preparing a bimetallic cluster catalyst according to claim 3, characterized in that: The mass ratio of the Cu pre-ligand to the Co pre-ligand in step (S4) is 15:0.5-2.9; Preferably, in step (S4), the mass ratio of the Cu precursor to the Co precursor is 15:1 to 2.
9.
6. The method for preparing a bimetallic cluster catalyst according to claim 3, characterized in that: The metal copper salt is a divalent copper salt; the metal cobalt salt is a divalent cobalt salt; Preferably, the metal copper salt is CuCl2; and the metal cobalt salt is Co(OH)2.
7. The method for preparing a bimetallic cluster catalyst according to claim 3, characterized in that: In step (S4), the Cu pre-ligand and the Co pre-ligand are mixed in the presence of a benzene solution and phenylacetylene, and are diffused using triethylamine and n-hexane as diffusion agents to obtain a bimetallic cluster catalyst Cu 12-x Co x L crystal; wherein x=0.5-1.
7.
8. Use of the bimetallic cluster catalyst according to claim 1 or 2 or the bimetallic cluster catalyst prepared by the method according to any one of claims 3 to 7 in the preparation of 2,5-furandicarboxylic acid.
9. A method for preparing 2,5-furandicarboxylic acid, characterized in that: The method comprises: synthesizing the 2,5-furandicarboxylic acid from 5-hydroxymethylfurfural by the action of a catalyst under alkaline medium conditions; wherein the catalyst is the bimetallic cluster catalyst according to claim 1 or 2 or the bimetallic cluster catalyst prepared by the method according to any one of claims 3-7.
10. The method for preparing 2,5-furandicarboxylic acid according to claim 8, characterized in that: The method comprises: mixing sodium hydroxide, 5-hydroxymethylfurfural, a catalyst and sodium hypochlorite, and reacting to obtain 2,5-furandicarboxylic acid; Preferably, the mixing ratio of the 5-hydroxymethylfurfural to the catalyst is 3 to 4:1, by weight; Preferably, the mixing ratio of the 5-hydroxymethylfurfural, the catalyst, sodium hydroxide and sodium hypochlorite is 3-4 g: 1 g: 0.5-1 g: 20-40 mL.
Citation Information
Patent Citations
Preparation method of transition metal catalyst and application of transition metal catalyst in preparation of furandicarboxylic acid
CN114618496A
Catalyst for preparing 2, 5-furandicarboxylic acid through catalytic oxidation of 5-hydroxymethylfurfural and preparation method of catalyst
CN115739093A