Sodium removal method in bulk phase hydrogenation catalyst preparation process
The sodium removal method that combines vacuum filtration and curing treatment solves the molding and pore structure problems caused by residual sodium ions in the co-precipitation method, improves the molding strength and pore structure of the bulk hydrogenation catalyst, simplifies the process and saves money. of water resources.
Patent Information
- Application Number
- CN202310357194.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-06
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-04-06
AI Technical Summary
In the process of preparing bulk hydrogenation catalysts by co-precipitation method, the residual sodium ions make the catalyst difficult to form, have poor pore structure and affect the hydrogenation activity. It is difficult to completely remove sodium ions with existing technology, affecting the performance of the catalyst.
Adopting a sodium removal method that combines vacuum filtration and health treatment, the sodium content in the catalyst is gradually reduced through multiple vacuum filtration and deionized water treatments, and the pore structure is optimized during the temperature-controlled drying process to reduce the adsorption and absorption of sodium ions. Precipitate.
It effectively improves the molding strength and pore structure properties of the catalyst, reduces the residual sodium ions, improves the hydrogenation activity and pore volume of the catalyst, simplifies the process, and saves water resources.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of bulk hydrogenation catalyst preparation, and in particular relates to a method for removing impurity sodium during the process of preparing bulk catalyst by coprecipitation method. Background Art
[0002] The most effective means to meet the requirements of oil quality upgrade is to use high hydrogenation activity catalysts. As one of the most active hydrogenation catalysts currently available, bulk catalysts are very suitable for diesel quality upgrades in refineries due to their excellent hydrogenation performance.
[0003] Bulk hydrogenation catalysts are usually prepared by kneading or coprecipitation. Due to the difficulty of molding, it is difficult to obtain a catalyst with a high metal content by kneading. At the same time, due to the limitations of the preparation method, it is difficult to evenly mix the active metal components, which cannot promote the synergistic effect between the active metals, making it difficult for the catalyst to fully exert its activity.
[0004] Due to the characteristics of ionic reactions, the components of the co-precipitation method can be evenly mixed during the reaction. At the same time, the co-precipitation method determines that the selection range of preparation raw materials is relatively wide, and raw materials that cannot be used by the impregnation method and kneading method can be used, which broadens the range of raw material selection. Cheap and clean raw materials can be selected to produce bulk catalysts, thereby achieving the purpose of reducing the cost of bulk catalyst raw materials and realizing green production. These are also the two main problems faced by bulk catalyst research and development and industrial applications.
[0005] The co-precipitation method mostly uses ammonia water as a precipitant and nitrogen-containing soluble salts as raw materials. The current research on bulk catalysts shows that compared with ammonium metatungstate, ammonium molybdate, ammonium thiomolybdate, nickel nitrate, etc. as active metal raw materials, or using ammonia water as an alkaline precipitant, using relatively low-priced sodium-containing raw materials such as sodium tungstate, sodium molybdate, nickel chloride, sodium hydroxide, sodium carbonate, sodium bicarbonate, etc., can not only reduce the raw material cost of bulk catalysts, but also solve the "ammonia nitrogen" pollution problem in the production process of bulk catalysts from the source because the raw materials do not contain "ammonia nitrogen".
[0006] However, as the research progressed, it was found that the introduction of a large amount of sodium ions in the raw materials would lead to an increase in the sodium content in the bulk catalyst. It is difficult to completely remove sodium ions during the catalyst preparation process, and a large amount of sodium ions in the precipitated material leads to poor material adhesion, which affects the difficulty of catalyst extrusion molding. Not only is it difficult to mold, but it also affects the strength of the catalyst; and the sodium content of the finished catalyst increases, and the remaining sodium ions are not conducive to the formation of the catalyst pore structure, which will lead to more small pores in the catalyst, and will also cause changes in other physical and chemical properties of the catalyst, affecting the catalyst hydrogenation activity.
[0007] CN101172261A discloses a method for preparing a catalyst composition by co-precipitation reaction using sodium aluminate solution and a mixed solution of nickel and tungsten component salts in parallel; CN110038581B discloses a method for preparing a hydrogenation refining catalyst. The preparation method adopts a co-precipitation method, and two co-precipitation processes are respectively precipitated using sodium tungstate alkaline solution and sodium molybdate alkaline solution as precipitants. In the above two invention patents, sodium-containing active metal salts are introduced as precipitants during the co-precipitation reaction, but no targeted sodium removal treatment is performed during the process, resulting in a certain amount of sodium ions in the co-precipitation product, poor material adhesion, relatively low crushing strength, and residual sodium ions also make the pore volume and specific surface area of the catalyst small.
[0008] CN114471593A and CN114471594A both disclose a method for preparing a hydrorefining catalyst. The method adopts coprecipitation method to prepare and remove sodium salt. The sodium salt removal method selects to remove sodium salt after catalyst extrusion molding. The method has certain requirements for the total amount of sodium content of catalyst preparation raw materials. If the sodium content in the coprecipitation slurry filter cake exceeds 10wt%, the material will be relatively loose, and the material cannot be extruded or the strength after molding is small. In addition to this situation, a large amount of sodium ions exist in the coprecipitation product, and part of the sodium chloride crystals will be precipitated and attached to its internal pores during the drying process before its molding, affecting the pore expansion of the catalyst. In addition, sodium salt removal is selected after catalyst extrusion molding, and the drying, extrusion and other treatments performed on the material before molding increase the degree of adsorption of sodium ions to the catalyst, resulting in sodium salt being more difficult to remove, that is, the desalination treatment after molding is not thorough. Summary of the invention
[0009] In view of the problems existing in the prior art, the present invention provides a method for removing sodium in the process of preparing a bulk hydrogenation catalyst. The method solves the adverse effects of sodium-containing raw materials on catalyst molding, pore structure, other physical and chemical properties and hydrogenation activity, and at the same time improves the catalyst strength and pore structure properties, and is particularly suitable for the process of preparing a bulk hydrogenation catalyst by co-precipitation of raw materials with high sodium content.
[0010] The method for removing sodium in the preparation process of the bulk hydrogenation catalyst of the present invention comprises the following contents: (1) vacuum filtering the sodium-containing slurry obtained by preparing the bulk hydrogenation catalyst by the co-precipitation method to obtain a slurry filter cake, and then performing a first curing treatment; (2) adding deionized water to the filter cake obtained in step (1), performing a first vacuum filtration desalination, and then performing a second curing treatment; (3) adding deionized water onto the filter cake obtained in step (2) to perform a second vacuum filtration and desalination; (4) The deionized water and the filter cake obtained in step (3) are mixed evenly, and vacuum filtration is performed for the third time for desalination, followed by temperature-controlled drying to obtain a de-sodiumized catalyst precursor.
[0011] In the method of the present invention, at least one of the raw materials for preparing the bulk hydrogenation catalyst by the co-precipitation method in step (1) is a sodium-containing raw material, generally comprising an acidic working solution and an alkaline precipitant, wherein: the acidic working solution is a soluble salt solution of an active metal (one or any combination of tungsten, molybdenum, nickel, and cobalt) and other components, such as sodium tungstate, sodium molybdate, and sodium aluminate; the alkaline precipitant is a solution of an alkali and / or an alkaline salt, such as sodium hydroxide, sodium carbonate, and sodium bicarbonate; the sodium-containing slurry in step (1) needs to use one or any combination of the above-mentioned sodium-containing or other sodium-containing raw materials as the co-precipitation reaction raw material.
[0012] In the method of the present invention, the sodium content of the sodium-containing slurry filter cake in step (1), calculated as the sodium content in the solid after the slurry filter cake is calcined at 500° C. in air for 4 hours, is 1.0 wt % to 18 wt %, preferably 2 wt % to 16 wt %.
[0013] In the method of the present invention, the filter cake base obtained by vacuum filtration in step (1) is in the range of 15wt% to 25wt%, preferably 18wt% to 23wt%.
[0014] In the method of the present invention, the first curing treatment conditions in step (1) are as follows: curing temperature of 28°C to 45°C, preferably 35°C to 40°C; curing time of 0.4 to 2 hours, preferably 0.5 to 1 hour; curing environment humidity of greater than 80%, preferably greater than 85%; and preventing the filter cake from being excessively dehydrated or dehydrated at a fast rate due to low environmental humidity and high temperature during the curing process, resulting in the precipitated sodium salt rapidly crystallizing into larger grains, thereby affecting the subsequent sodium salt removal efficiency.
[0015] In the method of the present invention, after the curing process in step (1) is completed: the dry basis range of filter cake A is 20% to 33%, preferably 23% to 28%; the curing process causes most of the hydrated sodium ions in the filter cake A to precipitate from its pores and retain vacancies, thereby increasing the pore volume of the filter cake.
[0016] In the method of the present invention, the first vacuum filtration desalination conditions in step (2) are as follows: the liquid-to-solid mass ratio is greater than 2, preferably 3-4:1, wherein the solid mass is based on the final catalyst mass; the deionized water temperature is 28°C-45°C, preferably the same as the curing temperature.
[0017] In the method of the present invention, the second curing treatment conditions in step (2) are as follows: curing temperature of 40°C to 70°C, preferably 50°C to 60°C; curing time of 0.5 to 2 hours, preferably 0.8 to 1.2 hours; and curing environment humidity of greater than 80%, preferably greater than 85%. In addition to preventing the rapid crystallization of sodium salt into larger grains due to low environmental humidity during the curing process, the pores left by the removal of most of the sodium impurities in step (2) allow water in the filter cake to diffuse rapidly outward in the form of water vapor under the higher temperature and humidity environment of the second curing, thereby producing a pore expansion effect.
[0018] In the method of the present invention, the filter cake base obtained after the second curing treatment is 28wt%~38wt%, preferably 30wt%~35wt%.
[0019] In the method of the present invention, the second vacuum filtration desalination conditions in step (3) are as follows: the liquid-to-solid mass ratio is greater than 0.5, preferably 2-3:1, wherein the solid mass is based on the final catalyst mass; the deionized water temperature is 40°C-70°C, preferably the same as the curing temperature.
[0020] In the method of the present invention, the third vacuum filtration desalination conditions in step (4) are as follows: liquid-to-solid mass ratio>0.3, preferably 0.5-0.8:1, wherein the solid mass is based on the final catalyst mass; and the deionized water temperature is 30°C-60°C.
[0021] In the method of the present invention, the vacuum filtration described in steps (1) to (4) is generally carried out in a vacuum filtration device.
[0022] In the method of the present invention, the curing treatment process described in steps (1) and (2) can be carried out in any environment that meets the curing treatment conditions. Preferably, it is carried out directly in a vacuum filtration device without moving the filter cake, thereby simplifying the operation process.
[0023] In the method of the present invention, the temperature-controlled drying conditions in step (4) are: the temperature is 45-95°C, preferably 50-70°C; and the filter cake base is controlled to be 40wt%-68wt%, preferably 43wt%-55wt%.
[0024] The catalyst precursor in step (4) of the method of the present invention is further subjected to processes such as extrusion, molding, drying and calcination to finally prepare a bulk hydrogenation catalyst, and this process is well known to those skilled in the art.
[0025] The method of the present invention directly removes the sodium impurity from the coprecipitation product obtained when preparing the bulk catalyst by the coprecipitation method. The process is simple, water resources are saved, and the impurity removal efficiency is high. It is not limited by the sodium content in the raw material. The advantages of the method of the present invention can be better reflected for raw materials with high sodium content.
[0026] This method combines vacuum filtration desalination with curing treatment to remove impurity sodium in a short time after the coprecipitation reaction ends, reducing the degree of adsorption of sodium ions on the catalyst due to subsequent drying and extrusion treatment, making it easier to remove. At the same time, compared with traditional coprecipitation product pulping and washing to remove impurities, or water washing to remove sodium after molding, this method can remove a large amount of impurity sodium in the filter cake with a small amount of water, achieving the requirement that the sodium content in the filter cake (catalyst molding material) is ≯0.1%, reducing the number of washing times and significantly reducing the water consumption in the catalyst preparation process, thereby achieving the purpose of saving water.
[0027] After vacuum filtration and desalination, the filter cake is obtained, and then the temperature-controlled drying treatment in step (4) is carried out. Due to the removal of the sodium impurity, the sodium chloride crystals precipitated during drying and adhering to the internal pores of the filter cake to affect the pore expansion are eliminated. During the drying process, the water in the filter cake diffuses outward rapidly in the form of water vapor, causing a secondary impact on the pore structure, further optimizing the pore structure of the catalyst and increasing the pore volume. Implementation
[0028] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0029] The specific surface area and pore volume of the catalyst were measured on an American ASAP-2405 BET nitrogen adsorption instrument. The crushing strength of the catalyst was measured on a particle strength tester. The sodium contents of the catalyst, catalyst precursor and slurry filter cake were measured on an inductively coupled plasma spectrometer. The sodium contents of the catalyst precursor and slurry filter cake were measured based on the sodium content in the solid after the sample was calcined at 500°C in air for 4 hours.
[0030] The coprecipitation reaction slurry used in the examples and comparative examples is the reaction slurry commonly used in preparing bulk hydrogenation catalysts using sodium-containing raw materials. For example, the slurry can be prepared using the following process: Prepare a mixed solution A of aluminum chloride and nickel chloride (the mass concentration of aluminum chloride calculated as Al2O3 is 15g / L, and the mass concentration of nickel chloride calculated as NiO is 30g / L); prepare a mixed solution B of sodium tungstate and sodium molybdate (the mass concentration of sodium tungstate calculated as WO3 is 45g / L, and the mass concentration of sodium molybdate calculated as MoO3 is 15g / L); solution A is used as the bottom water of the coprecipitation reaction, and under high-speed stirring conditions, the mixed solution B and alkaline precipitant sodium hydroxide solution (NaOH mass concentration 10g / L) are co-flowed and dripped into the mixed solution A to obtain a coprecipitation product slurry①.
[0031] Prepare a mixed solution A of sodium aluminate and nickel chloride (the mass concentration of sodium aluminate calculated as Al2O3 is 15 g / L, and the mass concentration of nickel chloride calculated as NiO is 30 g / L); prepare a mixed solution B of sodium tungstate and sodium molybdate (the mass concentration of sodium tungstate calculated as WO3 is 45 g / L, and the mass concentration of sodium molybdate calculated as MoO3 is 15 g / L); solution A is used as the bottom water of the coprecipitation reaction, and under high-speed stirring conditions, the mixed solution B and the alkaline precipitant sodium hydroxide solution (NaOH mass concentration 10 g / L) are co-flowed and dripped into the mixed solution A to obtain a coprecipitation product slurry②.
[0032] According to the different sodium contents in the raw materials, coprecipitation product slurry ① and slurry ② were selected to carry out the embodiments of the present invention and the comparative examples, wherein the elemental sodium content in the filter cake of slurry ① was 8.32wt%, and the elemental sodium content in the filter cake of slurry ② was 11.32wt%. Example 1
[0033] The slurry ① is vacuum filtered to obtain a coprecipitated product filter cake with a dry basis of 20.3wt%; the filter cake is cured, and the curing process is directly carried out in a vacuum filter, maintaining the curing environment humidity at 86%, the curing temperature at 35°C, the time for 0.75 hour, and the filter cake base is 26wt% after the curing; deionized water in a mass ratio of 4:1 to the catalyst preparation is added to the upper layer of the filter cake, the deionized water temperature is 35°C, and vacuum filtration is performed until there is no suspension on the surface of the filter cake.
[0034] Continue to perform secondary curing on the filter cake in the vacuum filter, maintain the curing environment humidity at 88%, the curing temperature at 52°C, the time for 1.0 hour, and at the end of curing, the filter cake base is 32wt%; add deionized water in a mass ratio of 2:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 52°C, and vacuum filter until there is no suspension on the surface of the filter cake.
[0035] Add 50°C deionized water in a mass ratio of 0.5:1 to the catalyst preparation to the filter cake again, mix well with the filter cake, and then vacuum filter until there is no filtrate dripping from the filter cake, and the washing is completed.
[0036] The filter cake was dried at 70° C. to obtain a catalyst precursor with a dry basis weight of 50 wt %.
[0037] The material was subjected to conventional bulk catalyst extrusion molding treatment and then dried and calcined to obtain bulk catalyst A1-1. The main properties are shown in Table 1. Example 2
[0038] The slurry ① is vacuum filtered to obtain a coprecipitated product filter cake with a dry basis of 22.5wt%; the filter cake is cured, and the curing process is directly carried out in a vacuum filter, maintaining the curing environment humidity at 89%, the curing temperature at 40°C, and the time for 0.5 hour. After the curing, the filter cake base is 29wt%; deionized water in a mass ratio of 3.5:1 to the catalyst preparation is added to the upper layer of the filter cake, the deionized water temperature is 43°C, and vacuum filtration is performed until there is no suspension on the surface of the filter cake.
[0039] Continue to perform secondary curing on the filter cake in the vacuum filter, maintain the curing environment humidity at 85%, the curing temperature at 58°C, and the time for 1.2 hours. At the end of curing, the filter cake base is 36wt%. Add deionized water in a mass ratio of 2.5:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 58°C, and vacuum filter until there is no suspension on the surface of the filter cake.
[0040] Add 30°C deionized water in a mass ratio of 1.0:1 to the catalyst preparation to the filter cake again, mix well with the filter cake, and then vacuum filter until there is no filtrate dripping from the filter cake, and the washing is completed.
[0041] The filter cake was dried at 60° C. to obtain a catalyst precursor having a dry basis weight of 46 wt %.
[0042] The material was subjected to conventional bulk catalyst extrusion molding treatment and then dried and calcined to obtain bulk catalyst A2-1. The main properties are shown in Table 1. Example 3
[0043] The slurry ① is vacuum filtered to obtain a coprecipitation product filter cake with a dry basis of 25.0wt%; the filter cake is cured, and the curing process is directly carried out in a vacuum filter, maintaining the curing environment humidity at 82%, the curing temperature at 45°C, the time for 1.0 hour, and the filter cake base is 32wt% after the curing; deionized water in a mass ratio of 3:1 to the catalyst preparation is added to the upper layer of the filter cake, the deionized water temperature is 28°C, and vacuum filtration is performed until there is no suspension on the surface of the filter cake.
[0044] Continue to perform secondary curing on the filter cake in the vacuum filter, maintain the curing environment humidity at 82%, the curing temperature at 65°C, and the time for 1.5 hours. At the end of curing, the filter cake base is 34wt%. Add deionized water in a mass ratio of 3:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 65°C, and vacuum filter until there is no suspension on the surface of the filter cake.
[0045] Add 60°C deionized water in a mass ratio of 0.7:1 to the catalyst preparation to the filter cake again, mix well with the filter cake, and then vacuum filter until there is no filtrate dripping from the filter cake, and the washing is completed.
[0046] The filter cake was dried at 50° C. to obtain a catalyst precursor having a dry basis weight of 42 wt %.
[0047] The material was subjected to conventional bulk catalyst extrusion molding treatment and then dried and calcined to obtain bulk catalyst A3. The main properties are shown in Table 1. Example 4
[0048] The slurry ① is vacuum filtered to obtain a coprecipitation product filter cake with a dry basis of 17.2wt%; the filter cake is cured, and the curing process is directly carried out in a vacuum filter, maintaining the curing environment humidity at 93%, the curing temperature at 30°C, the time for 1.8 hours, and the filter cake base is 22wt% after the curing; deionized water in a mass ratio of 2.5:1 to the catalyst preparation is added to the upper layer of the filter cake, the deionized water temperature is 30°C, and vacuum filtration is performed until there is no suspension on the surface of the filter cake.
[0049] Continue to perform secondary curing on the filter cake in the vacuum filter, maintain the curing environment humidity at 94%, the curing temperature at 45°C, the time for 2.0 hours, and the filter cake base is 29wt% at the end of curing; add deionized water in a mass ratio of 1:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature is 45°C, and vacuum filter until there is no suspension on the surface of the filter cake.
[0050] Add 40°C deionized water in a mass ratio of 0.35:1 to the catalyst preparation to the filter cake again, mix evenly with the filter cake, and then vacuum filter until there is no filtrate dripping from the filter cake, and the washing is completed.
[0051] The filter cake was dried at 80° C. to obtain a catalyst precursor with a dry basis weight of 55 wt %.
[0052] The material was subjected to conventional bulk catalyst extrusion molding treatment and then dried and calcined to obtain bulk catalyst A4. The main properties are shown in Table 1. Example 5
[0053] The slurry ① is vacuum filtered to obtain a coprecipitation product filter cake with a dry basis of 19.4wt%; the filter cake is cured in an insulated box, the curing environment humidity is maintained at 95%, the curing temperature is 37°C, the time is 1.2 hours, and the filter cake base is 24wt% after the curing; the filter cake is placed flat and seamlessly on a vacuum filter cloth, and deionized water is added to the upper layer of the filter cake in a mass ratio of 4.5:1 to the catalyst preparation. The deionized water temperature is 37°C, and vacuum filtration is performed until there is no suspension on the surface of the filter cake.
[0054] Continue to perform secondary curing on the filter cake in the vacuum filter. The secondary curing process is carried out in the above-mentioned incubator, maintaining the curing environment humidity at 90%, the curing temperature at 60°C, the time at 1.7 hours, and the filter cake base is 33wt% at the end of curing; place the filter cake flat and seamlessly on the filter cloth of the vacuum filter, add deionized water in a mass ratio of 4:1 to the catalyst preparation to the upper layer of the filter cake, the deionized water temperature at 60°C, and vacuum filter until there is no suspension on the surface of the filter cake.
[0055] Add 50°C deionized water in a mass ratio of 0.8:1 to the catalyst preparation to the filter cake again, mix evenly with the filter cake, and then vacuum filter until there is no filtrate dripping from the filter cake, and the washing is completed.
[0056] The filter cake was dried at 65° C. to obtain a catalyst precursor having a dry basis weight of 48 wt %.
[0057] The material was subjected to conventional bulk catalyst extrusion molding treatment and then dried and calcined to obtain bulk catalyst A5. The main properties are shown in Table 1. Example 6
[0058] The other steps of this example are the same as those of Example 1, except that slurry ② is used to carry out this example to obtain catalyst B1, the main properties of which are shown in Table 1.
[0059] Comparative Example 1 The slurry ② was vacuum filtered to obtain a coprecipitation product cake with a dry basis of 20.6 wt%; the filter cake was dried at 70° C. to obtain a material with a dry basis of 50 wt%.
[0060] The material was subjected to conventional bulk catalyst extrusion molding treatment, but due to the excessively high sodium content, the material became loose, the molding material became powdery, and the catalyst could not be molded.
[0061] Comparative Example 2 The slurry ① was vacuum filtered to obtain a coprecipitated product cake with a dry basis of 20.5 wt%; the filter cake was dried at 70° C. to obtain a catalyst precursor with a dry basis of 50 wt%.
[0062] After the material is subjected to conventional bulk catalyst extrusion molding treatment, the impurity sodium is removed according to the method disclosed in CN114471593A: the molded product is cured at 85°C for 48 hours, then cooled to 28°C, and cured for another 30 hours, and washed twice with deionized water, with the ratio of deionized water to catalyst preparation mass being 5:1.
[0063] Then, the catalyst was dried and calcined to obtain bulk catalyst C1, the main properties of which are shown in Table 1.
[0064] Comparative Example 3 The slurry ① was vacuum filtered to obtain a coprecipitated product cake with a dry basis of 20.3 wt%.
[0065] Deionized water was added to the filter cake, the mass ratio of deionized water to catalyst preparation was 10:1, and the slurry was beaten and washed for 1.5 hours. The slurry was vacuum filtered to obtain a filter cake with a dry basis of 20.7 wt%.
[0066] The filter cake was dried at 70°C to obtain a catalyst precursor with a dry basis of 50 wt%. The material was subjected to conventional bulk catalyst extrusion molding treatment, and the molded material was washed 3 times with deionized water, with a deionized water to catalyst preparation mass ratio of 5:1, and then dried and calcined to obtain bulk catalyst C2. The main properties are shown in Table 1.
[0067] Comparative Example 4 The other steps of this example are the same as those of Example 1, except that in step (1), the first curing treatment conditions of this comparative example are as follows: the curing environment humidity is maintained at 70%, the curing temperature is 60°C, the curing time is 2.5 hours, and the filter cake base is 36wt% at the end of the curing.
[0068] Finally, bulk catalyst A1-2 was obtained, and its main properties are shown in Table 1.
[0069] Comparative Example 5 The other steps of this example are the same as those of Example 1, except that in step (2), the first vacuum filtration desalination conditions of this comparative example are as follows: deionized water in a mass ratio of 1:1 to the catalyst preparation is added to the upper layer of the filter cake, the deionized water temperature is 35°C, and vacuum filtration is performed until there is no suspension on the surface of the filter cake.
[0070] Finally, bulk catalyst A1-3 was obtained, and its main properties are shown in Table 1.
[0071] Comparative Example 6 The other steps of this example are the same as those of Example 2, except that the second curing treatment conditions in step (2) of this comparative example are as follows: the curing environment humidity is maintained at 65%, the curing temperature is 25°C, the time is 0.4 hours, and the filter cake base is 30wt% at the end of the curing.
[0072] Finally, bulk catalyst A2-2 was obtained, and its main properties are shown in Table 1.
[0073] Comparative Example 7 The other steps of this example are the same as those of Example 2, except that in step (3), this comparative example performs a second vacuum filtration desalination: deionized water is added to the upper layer of the filter cake in a mass ratio of 0.3:1 to the catalyst preparation, the temperature of the deionized water is 50°C, and vacuum filtration is performed until there is no suspension on the surface of the filter cake.
[0074] Finally, bulk catalyst A2-3 was obtained, and its main properties are shown in Table 1.
[0075] Comparative Example 8 The other steps of this example are the same as those of Example 2, except that in step (3) of this comparative example, the second vacuum filtration desalination is directly performed until no filtrate drips, and step (4) of the third vacuum filtration desalination is not performed.
[0076] Finally, bulk catalyst A2-4 was obtained, and its main properties are shown in Table 1.
[0077] Table 1 Properties of catalysts prepared in Examples and Comparative Examples A1-1 A2-1 A3 A4 A5 B1 Catalyst precursor sodium content, ppm 148 106 522 431 337 350 Catalyst products Pore volume, mL / g 0.479 0.463 0.447 0.443 0.466 0.441 <![CDATA[Specific surface area, m 2 / g]]> 356 353 341 338 347 350 Mechanical strength, N / mm 19.4 20.9 18.5 18.7 19.3 20.2 Sodium content, ppm, 101 83 501 408 286 321 Table 1 (Continued) Properties of Catalysts Prepared in Examples and Comparative Examples C1 C2 A1-2 A1-3 A2-2 A2-3 A2-4 Catalyst precursor sodium content, ppm 83219 21837 1242 1093 769 884 312 Catalyst products Pore volume, mL / g 0.423 0.394 0.434 0.441 0.446 0.453 0.459 <![CDATA[Specific surface area, m 2 / g]]> 322 310 331 335 342 342 347 Mechanical strength, N / mm 12.6 14.8 18.6 18.5 19.1 20.1 19.7 Sodium content, ppm, 1436 2904 1279 1017 706 821 285
Claims
1. A method for removing sodium in the preparation process of a bulk hydrogenation catalyst, characterized in that The method comprises the following contents: (1) vacuum filtering the sodium-containing slurry obtained by preparing the bulk hydrogenation catalyst by the coprecipitation method to obtain the slurry filter cake, and then performing the first curing treatment; (2) adding deionized water to the filter cake obtained in step (1), performing the first vacuum filtration desalination, and then performing the second curing treatment; (3) adding deionized water to the filter cake obtained in step (2), performing the second vacuum filtration desalination; (4) uniformly mixing the deionized water and the filter cake obtained in step (3), performing the third vacuum filtration desalination, and then performing the temperature-controlled drying treatment to obtain a de-sodiumized catalyst precursor.
2. The sodium removal method according to claim 1, characterized in that: At least one of the raw materials for preparing the bulk hydrogenation catalyst by the co-precipitation method in step (1) is a sodium-containing raw material.
3. The sodium removal method according to claim 1, characterized in that: The sodium content of the sodium-containing slurry filter cake in step (1) is 1.0 wt% to 18 wt%, preferably 2 wt% to 16 wt%, calculated as the sodium content in the solid after the slurry filter cake is calcined at 500° C. in air for 4 hours.
4. The sodium removal method according to claim 1, characterized in that: The filter cake base content obtained by vacuum filtration in step (1) is 15wt%~25wt%, preferably 18wt%~23wt%.
5. The sodium removal method according to claim 1, characterized in that: The first curing treatment conditions in step (1) are as follows: curing temperature of 28°C to 45°C, preferably 35°C to 40°C; curing time of 0.4 to 2 hours, preferably 0.5 to 1 hour; and curing environment humidity of greater than 80%, preferably greater than 85%.
6. The sodium removal method according to claim 1, characterized in that: After the curing process in step (1) is completed: the dry basis content of the filter cake A is 20% to 33%, preferably 23% to 28%.
7. The sodium removal method according to claim 1, characterized in that: The first vacuum filtration desalination conditions in step (2) are as follows: the liquid-to-solid mass ratio is greater than 2, preferably 3-4:1, wherein the solid mass is based on the final catalyst mass; and the deionized water temperature is 28°C-45°C.
8. The sodium removal method according to claim 1, characterized in that: The second curing treatment conditions in step (2) are as follows: curing temperature of 40°C to 70°C, preferably 50°C to 60°C; curing time of 0.5 to 2 hours, preferably 0.8 to 1.2 hours; and curing environment humidity of greater than 80%, preferably greater than 85%.
9. The sodium removal method according to claim 1, characterized in that: The filter cake base content obtained after the second curing treatment is 28wt%~38wt%, preferably 30wt%~35wt%.
10. The sodium removal method according to claim 1, characterized in that: The second vacuum filtration desalination conditions in step (3) are as follows: the liquid-to-solid mass ratio is greater than 0.5, preferably 2-3:1, wherein the solid mass is based on the final catalyst mass; and the deionized water temperature is 40°C-70°C.
11. The sodium removal method according to claim 1, characterized in that: The third vacuum filtration desalination conditions in step (4) are as follows: liquid-to-solid mass ratio>0.3, preferably 0.5-0.8:1, wherein the solid mass is based on the final catalyst mass; and the deionized water temperature is 30°C-60°C.
12. The sodium removal method according to claim 1, characterized in that: The health treatment process described in steps (1) and (2) is directly carried out in the vacuum filtration equipment.
13. The sodium removal method according to claim 1, characterized in that: The temperature-controlled drying conditions in step (4) are as follows: the temperature is 45-95° C., preferably 50-70° C.; the filter cake base content is controlled to be 40wt%-68wt%, preferably 43wt%-55wt%.
14. The sodium removal method according to claim 1, characterized in that: The catalyst precursor of step (4) is then subjected to extrusion, molding, drying and calcination processes to finally prepare a bulk hydrogenation catalyst.
Citation Information
Patent Citations
Hydrogenation catalyst and preparation method and application thereof
CN105536808A