Economical high-boron steel sheath rolling process for nuclear power

Through the composite lamination rolling process in the form of cladding, combined with A36 carbon structural steel and aluminum foil isolation layers, the problem of cracking of high boron steel during the rolling process has been solved, the forming quality and preparation efficiency of high boron steel plates have been improved, and seamless Preparation of high boron steel plates with uniform cracks and structures.

CN118768385AActive Publication Date: 2024-10-15HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410928737.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-15
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

High boron steel is prone to edge cracking during the rolling process, resulting in reduced thermoplasticity and production efficiency and quality problems.

Method used

Adopting a composite lamination rolling process in the form of a cladding, the high boron steel blank is put into an A36 carbon structural steel cladding, an aluminum foil isolation layer is used, and through hot rolling and straightening treatments, the rolling temperature and deformation amount are controlled to reduce heat loss. and risk of cracking.

Benefits of technology

It effectively improves the forming quality and preparation efficiency of high boron steel plates, ensures no cracks on the surface and uniformity of the structure, reduces the difficulty of consumable use and heat preservation control, and solves the problem of cracking during the rolling process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768385A_ABST
    Figure CN118768385A_ABST
Patent Text Reader

Abstract

The invention discloses a high-boron steel sheath rolling process for economical nuclear power. The high-boron steel sheath rolling process comprises the following steps: (1) preparing a cuboid high-boron steel blank; (2) a wrapping sleeve for rolling is machined according to the size of the blank, the head end and the tail end of the wrapping sleeve are not blocked, the high-boron steel blank is loaded into the wrapping sleeve, the blank and the wrapping sleeve are separated through an isolation layer, and the thickness of the isolation layer is smaller than or equal to 1 mm; (3) hot rolling is conducted, specifically, the sheathed high-boron steel blank is placed in a resistance furnace to be heated, the heating temperature ranges from 1050 DEG C to 1250 DEG C, and heat preservation is conducted for 1-3 h; the initial rolling temperature is 950-1050 DEG C, and the final rolling temperature is higher than 900 DEG C; the total rolling deformation is controlled to be 70-80%; (4) the rolled plate is straightened through a straightening machine, and the straightening temperature is higher than 900 DEG C; and (5) removing the sheath, and milling and cutting the surface of the high-boron steel to obtain the required high-boron steel plate. The process provided by the invention solves the problem of rolling plate cracking in the rolling process of the high-boron steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel rolling, and in particular relates to an economical high-boron steel sheath rolling process for nuclear power. Background Art

[0002] Medium-high boron steel is made by adding boron to the existing stainless steel components. Stainless steel itself has a certain γ-ray shielding effect. After adding boron, it has a better ability to absorb thermal neutrons and γ-rays. It also has high strength and good toughness. Therefore, boron-containing stainless steel can be used not only as a shielding material but also as a structural material. However, because high-boron steel contains a large amount of compound brittle phases, the thermoplasticity is reduced, and edge cracking is prone to occur during the rolling process. Summary of the invention

[0003] The purpose of the present invention is to provide an economical high-boron steel sheath rolling process for nuclear power, in which a high-boron steel billet is loaded into a sheath with A36 as the sheath material for rolling, thereby reducing temperature loss during the rolling process, ensuring stable rolling, and improving the preparation efficiency and quality of high-boron steel plates.

[0004] To achieve the above object, the technical solution of the present invention is: An economical high-boron steel jacket rolling process for nuclear power includes the following steps: (1) Preparing a rectangular high-boron steel billet; (2) A sheath for rolling is processed according to the size of the billet, the head and tail ends of the sheath are not blocked, the high-boron steel billet is loaded into the sheath, and the billet and the sheath are separated by an isolation layer, and the thickness of the isolation layer is ≤1mm; (3) Hot rolling: The sheathed high-boron steel billet is heated in a resistance furnace at a temperature between 1050-1250°C for 1-3 hours; the starting rolling temperature is 950-1050°C, and the final rolling temperature is >900°C; the total rolling deformation is controlled between 70-80%; (4) Use a straightening machine to straighten the rolled plate, and the straightening temperature is greater than 900°C; (5) Remove the sheath, grind and cut the surface of the high-boron steel to obtain the required high-boron steel plate.

[0005] Furthermore, the material of the sheath in step (2) of the present invention is A36 carbon structural steel. A36 carbon structural steel has a low carbon content, good ductility, excellent weldability, and is easy to process.

[0006] Furthermore, the sheath in step (2) of the present invention is welded from a total of 4 A36 carbon steel plates on the top, bottom and sides.

[0007] Furthermore, the isolation layer in step (2) of the present invention is aluminum foil. Aluminum foil can fill the gap between the sheath and the rolled plate, and the material of aluminum foil is relatively soft and low in cost.

[0008] Furthermore, the hot rolling in step (3) of the present invention is performed 6 to 10 times.

[0009] Furthermore, in step (3) of the present invention, the reduction per pass during the rolling process is controlled within a range of 10% to 30%.

[0010] Furthermore, the high-boron steel composition of the present invention is: B: 1.5-2.0%; C: 0.04-0.08%, Si: 0.4-0.8%, Mn: 1.00-2.00%, Cr: 15-19%, V: 0.015-0.028%, Ti: 0.02-0.06%; Ni: 9-12%; N≤0.08%; P≤0.015%, S≤0.003%, and the balance is Fe and unavoidable impurity elements.

[0011] The present invention aims at the fact that high-boron steel has poor thermoplasticity and is prone to cracking during rolling. The present invention provides a method of using a sheathing form and composite rolling to efficiently and conveniently prepare a high-boron steel plate with no surface cracks and uniform structure. The invention principle and beneficial technical effects are: (1) The structural form of the combination of the sheath and the high-boron steel billet reduces the difficulty of thermal insulation control. The sheath structure provided increases the heat capacity and reduces the heat loss during the rolling process, which is beneficial to the improvement of the forming quality of the high-boron steel sheet. In addition, the sheath has a head-to-tail non-blocking structure, which reduces the use of consumables.

[0012] (2) A36 carbon structural steel has good ductility and weldability, and is easy to weld between sheathed plates, which can prevent high-boron steel plates from being crushed by the sheath during rolling and post-rolling cooling; the aluminum foil protective layer used between billets and between billets and sheaths is low in cost.

[0013] (3) The present invention straightens the rolled material after the high-boron steel plate is jacketed and rolled, thereby ensuring that the high-boron steel plate has a good plate shape after the jacket is removed.

[0014] (4) The high-boron steel of the present invention has a brittle phase. During the rolling process, a sheathing device is used for heat preservation. In combination with appropriate starting and final rolling temperatures, the problem of cracking of the rolled plate during the rolling process is solved. The steel has strong practicability and significant effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The package structure of the present invention; Figure 1 The ABCD surface and the EFGH surface are respectively the upper and lower surfaces of the package, and the ABEF surface and the CDGH surface are the side surfaces of the package.

[0016] Figure 2 This is the organizational morphology of the high-boron steel plate in Example 1. DETAILED DESCRIPTION

[0017] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example 1

[0018] The high-boron steel composition of this embodiment is: B: 1.5%; C: 0.04%, Si: 0.7%, Mn: 1.00%, Cr: 15%, V: 0.028%, Ti: 0.04%; Ni: 11%; N: 0.06%; P: 0.01%, S: 0.003%, and the balance is Fe and unavoidable impurity elements; its rolling process is as follows: (1) Preparation of rectangular high-boron steel billets: Ingots were prepared by vacuum consumable smelting, and high-boron steel slabs were prepared by 1100°C billet opening treatment. The high-boron steel slabs were processed into rectangular billets by mechanical processing, with a billet width of 210 mm, a length of 360 mm, and a thickness of 120 mm.

[0019] (2) According to the size of the billet, the sleeve for rolling is processed. A36 carbon structural steel is used to process the sleeve. The sleeve is welded from four plates, the upper and lower surfaces and the side surfaces. Figure 1 As shown, the inner cavity size of the sleeve is 211mm wide × 361mm long × 121mm thick; when welding the sleeve, first weld the two plates at the bottom and side of the sleeve, and put the milled high-boron steel billet into the sleeve. The billet and the sleeve are separated by a 0.5mm thick aluminum foil isolation layer. After the billet is completely loaded, the top and side of the sleeve are sealed by tungsten inert gas arc welding to ensure the strength and integrity of the weld. The overall thickness of the sleeve is 30mm.

[0020] (3) Hot rolling: The sheathed high-boron steel billet is placed in a resistance furnace for heating at a temperature of 1120°C for 2 hours; the hot rolling mill with a roll width of 550 mm is used for rolling, the starting rolling temperature is 950°C, and a total of 6 passes are rolled, with the reduction per pass controlled at 20-30%, and the final rolling temperature is 910°C; the thickness of the high-boron steel plate after rolling is 30 mm.

[0021] (4) Straightening: Straighten the steel bar immediately after rolling with a straightening machine at a temperature above 900°C.

[0022] (5) Remove the sheath by machining, take out the high-boron steel plate, and grind the high-boron steel plate to make the surface smooth.

[0023] The high-boron steel plate in this embodiment is of good quality and has no cracking phenomenon; its organizational morphology is as follows Figure 2 shown by Figure 2 It can be seen that the microstructure of high boron steel is mainly composed of austenite and FeCrB brittle phase. Example 2

[0024] The high-boron steel composition of this embodiment is: B: 1.8%; C: 0.08%, Si: 0.4%, Mn: 1.5%, Cr: 17%, V: 0.02%, Ti: 0.02%; Ni: 9%; N: 0.07%; P: 0.015%, S: 0.002%, and the remainder is Fe and unavoidable impurity elements.

[0025] Preparation of rectangular high-boron steel billet: First, a 50kg vacuum melting furnace is used to prepare an ingot, the ingot is milled for rolling, and the surface is coated with anti-rust paint. The billet is 150mm wide, 240mm long, and 145mm thick.

[0026] (2) According to the size of the billet, the sleeve for rolling is processed. A36 carbon structural steel is selected to process the sleeve. The sleeve is welded by four plates, the upper and lower plates and the side plates, such as Figure 1 As shown, the inner cavity size is 150.6mm wide × 240.6mm long × 145.6mm thick. When welding the sleeve, first weld the two plates on the bottom and side of the sleeve, and put the milled high-boron steel billet into the sleeve. The billet and the sleeve are separated by a 0.5mm thick aluminum foil isolation layer. After the billet is completely loaded, the top and side of the sleeve are sealed by tungsten inert gas arc welding to ensure the strength and integrity of the weld. The overall thickness of the sleeve is 20mm.

[0027] (3) Hot rolling: The high-boron steel billet after welding is placed in a resistance furnace for heating at a temperature of 1250°C and kept warm for 1 hour; a hot rolling mill with a roll width of 350 mm is used for rolling, the starting rolling temperature is 970°C, and a total of 10 passes are rolled, with the pass reduction controlled at 10-20%, and the final rolling temperature is 920°C; the thickness of the high-boron steel plate after rolling is 35 mm; (4) Straightening: Straighten the steel bar immediately after rolling with a straightening machine at a temperature above 900°C.

[0028] (5) Remove the sheath by machining, take out the high-boron steel plate, and grind the high-boron steel plate to make the surface smooth.

[0029] The high-boron steel plate in this embodiment is of good quality and has no cracking. Example 3

[0030] The high-boron steel of the present invention has the following components: B: 2.0%, C: 0.05%, Si: 0.6%, Mn: 1.3%, Cr: 16%, V: 0.015%, Ti: 0.04%, Ni: 10%, N: 0.08%, P: 0.01%, S: 0.003%, and the remainder is Fe and unavoidable impurity elements.

[0031] Preparation of rectangular high-boron steel billet: First, a vacuum melting furnace is used to prepare an ingot, and the ingot is milled for rolling. The smelted billet has a width of 350 mm, a length of 370 mm, and a thickness of 150 mm.

[0032] The sleeve for rolling is processed according to the size of the billet: A36 carbon structural steel is used to process the sleeve, which is welded by four plates in total, the upper, lower and side plates, and the inner cavity size is 150.2mm wide × 240.2mm long × 145.2mm thick; after the sleeve is welded, the high-boron steel billet is loaded into the sleeve, and the space between the billet and the sleeve is filled with 0.6mm thick aluminum foil. The overall thickness of the sleeve is 20mm Hot rolling: the high-boron steel billet after welding is placed in a resistance furnace for heating at a temperature of 1200°C for 3 hours; the starting rolling temperature is 1050°C, and a total of 10 passes are rolled, with the reduction per pass controlled at 10-20%, and the final rolling temperature is 940°C; the thickness of the high-boron steel plate after rolling is 30mm.

[0033] (4) Straightening: Straighten the steel bar immediately after rolling with a straightening machine at a temperature above 900°C.

[0034] (5) Machining and cutting to remove the sheath, take out the high-boron steel plate, and complete the grinding and milling of the high-boron steel plate to make the surface smooth.

[0035] The high-boron steel plate in this embodiment is of good quality and has no cracking. Example 4

[0036] The high-boron steel of the present invention has the following components: B: 1.9%; C: 0.06%; Si: 0.8%; Mn: 1.8%; Cr: 19%; V: 0.02%; Ti: 0.06%; Ni: 12%; N: 0.04%; P: 0.013%; S: 0.003%; the remainder is Fe and unavoidable impurity elements.

[0037] Preparation of rectangular high-boron steel billet: First, the ingot is prepared in a vacuum melting furnace, and then the ingot is electroslag treated to make the steel have better purity; the electroslag ingot is processed and milled. The resulting billet is 300mm wide, 410mm long, and 160mm thick.

[0038] According to the size of the billet, the sleeve for rolling is processed: A36 carbon structural steel is used to process the sleeve, which is welded by four plates, the upper and lower plates and the side plates. Figure 1 As shown, the inner cavity size is 300.8mm wide × 410.8mm long × 160.8mm thick; after the sleeve welding is completed, the high-boron steel billet is loaded into the sleeve, and the space between the billet and the sleeve is filled with 0.8mm thick aluminum foil, and the overall thickness of the sleeve is 25mm; Hot rolling: the high-boron steel billet after welding is placed in a resistance furnace for heating at a temperature of 1050°C for 2 hours; the rolling temperature is 1020°C, and a total of 7 passes are rolled, with the reduction of each pass controlled at 10-20%, and the final rolling temperature is 920°C; the thickness of the high-boron steel plate after rolling is 55mm; (4) Straightening: Straighten the steel bar immediately after rolling with a straightening machine at a temperature above 900°C.

[0039] (5) Remove the sheath by machining, take out the high-boron steel plate, and grind the high-boron steel plate to make the surface smooth.

[0040] The high-boron steel plate in this embodiment is of good quality and has no cracking.

Claims

1. An economical high-boron steel jacket rolling process for nuclear power, characterized in that: The following steps are involved: (1) Preparing a rectangular high-boron steel billet; (2) A sheath for rolling is processed according to the size of the billet, the head and tail ends of the sheath are not blocked, the high-boron steel billet is loaded into the sheath, and the billet and the sheath are separated by an isolation layer, and the thickness of the isolation layer is ≤1mm; (3) Hot rolling: The sheathed high-boron steel billet is heated in a resistance furnace at a temperature between 1050-1250°C for 1-3 hours; the starting rolling temperature is 950-1050°C, and the final rolling temperature is >900°C; the total rolling deformation is controlled between 70-80%; (4) Use a straightening machine to straighten the rolled plate, and the straightening temperature is greater than 900°C; (5) Remove the sheath, grind and cut the surface of the high-boron steel to obtain the required high-boron steel plate.

2. The economical high-boron steel jacket rolling process for nuclear power according to claim 1 is characterized in that: The material of the sheath in step (1) is A36 carbon structural steel.

3. The economical high-boron steel jacket rolling process for nuclear power according to claim 1, characterized in that: The package in step (2) is welded from 4 A36 carbon steel plates on the top, bottom and sides.

4. The economical high-boron steel jacket rolling process for nuclear power according to claim 1, characterized in that: The material of the isolation layer in step (2) is aluminum foil.

5. The economical high-boron steel jacket rolling process for nuclear power according to claim 1, characterized in that: The hot rolling in step (3) is performed 6 to 10 times.

6. The economical high-boron steel jacket rolling process for nuclear power according to claim 1, characterized in that: In step (3), the reduction per pass during the rolling process is controlled at 10% to 30%.

7. The economical high-boron steel jacket rolling process for nuclear power according to claim 1, characterized in that: The high-boron steel composition is: B: 1.5-2.0%; C: 0.04-0.08%, Si: 0.4-0.8%, Mn: 1.00-2.00%, Cr: 15-19%, V: 0.015-0.028, Ti: 0.02-0.06; Ni: 9-12%; N≤0.08; P≤0.015, S≤0.003%, the balance is Fe and unavoidable impurity elements.

Citation Information

Patent Citations

  • Short-flow high-efficiency preparation method of thin high-silicon electrical steel strip

    CN101886215A

  • Method for improving hot-working performance and room-temperature plasticity of high-boron stainless steel

    CN106702287A

  • Sheath suitable for TiAl alloy rolling and preparation method thereof

    CN112958626A

  • 370MPa-grade stainless steel composite plate and preparation method thereof

    CN116001380A

  • Material and method for hot-rolling austenitic stainless steel with high boron content

    JP1997269398A