Manufacturing method of high-content copper-silver alloy microwire

By setting up a filter device and adopting cascade spinning processing in the oxygen-free smelting process, the problem of impurities brought in during downcasting is solved, the molding quality and production efficiency of copper-silver alloy fine wires are improved, and the cost is reduced. Realized the production of high-strength micro-wires.

CN118768461AActive Publication Date: 2024-10-15HUZHOU JIN TAI CONDUCTOR TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411073690.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-08
Publication Date
2024-10-15
Estimated Expiration
2043-03-08

AI Technical Summary

Technical Problem

In the existing high-content copper-silver alloy micro-wire manufacturing method, downward continuous casting may cause impurities from the furnace bottom to be brought into the casting rod, causing material breakage, waste of raw material silver, and high processing costs.

Method used

In the anaerobic smelting process, a filtering device is installed at the lower outlet of the crucible in the smelting furnace, and the diversion filter holes are used to reduce impurities from entering the casting rod, and a cascade spinning process is adopted, including straightening, twisting and ring pressure reduction. diameter, combined with surface treatment and heat treatment, to prepare high-content copper-silver alloy micro-wires.

Benefits of technology

It effectively reduces impurities entering the cast rod, improves the molding quality of the cast rod, saves raw materials, reduces production costs, and improves the strength and toughness of the material. It is suitable for the manufacture of high-strength copper alloy micro-wires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768461A_ABST
    Figure CN118768461A_ABST
Patent Text Reader

Abstract

The invention relates to a manufacturing method of a high-content copper-silver alloy microwire, which comprises an oxygen-free smelting process, an oxygen-free continuous casting process, a cascade spinning processing process, a surface treatment process, a heat treatment process and a drawing process, in the oxygen-free smelting process, a filter device is arranged at a lower water outlet of a crucible in a smelting furnace; a flow guide filtering hole higher than the bottom of the crucible is formed in the side wall of the filtering device; the technical problems that due to the fact that impurities at the bottom of a furnace are brought into a casting rod sometimes through downward continuous casting, material line breakage is caused, waste products are formed, a large amount of raw material silver is wasted, and the machining cost is high are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nonferrous metal processing, and in particular to a method for manufacturing a high-content copper-silver alloy fine wire. Background Art

[0002] Copper-silver alloys with a silver content of 1% to 4% are widely used in the field of high-strength, high-conductivity and high-toughness coils. They are resistant to fatigue and vibration. High-content copper-silver alloys have high strength, and the finished product can reach more than 1000 MPa. Therefore, they are difficult to process. Traditional high-silver copper continuous rod billet manufacturing methods include upward continuous casting, horizontal continuous casting or downward continuous casting. The rod billet is cold rolled and then drawn. Due to the existence of casting structure, it is difficult to draw it into a fine wire. Upward and horizontal continuous casting often have a large amount of copper-silver alloy retained at the bottom of the furnace, resulting in waste. Downward continuous casting can effectively solve the problem of alloy retention.

[0003] The patent document with patent number CN2021113022136 discloses a method for preparing high-strength and high-conductivity Cu-Ag alloy fine wire. The steps of the preparation method are: preparing a Cu-Ag alloy cast rod by a downward vacuum melting and casting method; continuously extruding the obtained Cu-Ag alloy cast rod to obtain a rod blank with a diameter greater than or equal to 4 mm; multi-mode cold drawing of the rod blank, annealing, and then drawing to finally prepare a Cu-Ag alloy fine wire of 0.016 to 0.055 mm.

[0004] However, in actual use, the inventors found that the down-draw continuous casting sometimes causes impurities from the furnace bottom to be brought into the casting rod, causing the material to break, forming scrap, wasting a large amount of raw material silver, and increasing processing costs. Summary of the invention

[0005] The purpose of the present invention is to address the deficiencies of the prior art and provide a method for manufacturing high-content copper-silver alloy fine wires. During the oxygen-free smelting process, a filtering device is used to be arranged at the lower outlet of the crucible in the smelting furnace, and a diversion filtering hole is opened on the side wall of the filtering device to be higher than the bottom of the crucible, so as to reduce the impurities from being washed into the casting rod through the copper water, thereby improving the molding quality of the casting rod, thereby solving the technical problem that impurities from the bottom of the furnace are sometimes brought into the casting rod during the lower continuous casting, causing the material to break, forming waste, wasting a large amount of raw material silver, and high processing costs.

[0006] In view of the above technical problems, the following technical solutions are adopted: a method for manufacturing high-content copper-silver alloy fine wires, comprising an oxygen-free smelting process, an oxygen-free continuous casting process, a cascade spinning process, a surface treatment process, a heat treatment process and a drawing process. In the oxygen-free smelting process, a filtering device is provided at the lower water outlet of the crucible in the smelting furnace, and a side wall of the filtering device is provided with a diversion filtering hole higher than the bottom of the crucible.

[0007] Preferably, the oxygen-free continuous casting process adopts a continuous downward casting method.

[0008] Preferably, the filtering device is inserted above the lower water outlet at the bottom of the crucible.

[0009] Preferably, the filtering device comprises a plurality of graphite mesh sleeves which are nested, each graphite mesh sleeve having a plurality of the guide and filter holes, and the heights from the guide and filter holes on the graphite mesh sleeves to the bottom of the crucible increase sequentially from the inner to the outer.

[0010] Preferably, the cascade spinning process comprises two or more spinning mechanisms connected in series, specifically comprising the following steps: S1: Straightening process, after straightening the continuous casting rod billet with high content of copper and silver alloy, it is continuously and automatically output under the traction of the traction machine; S2: Spinning and reducing diameter process. The straightened continuous casting rod billet passes through multiple groups of spinning mechanisms. Each group of spinning mechanisms first presses the continuous casting rod billet and continuously twists it. After twisting, the continuous casting rod billet is immediately subjected to continuous ring pressing and reducing diameter. Each group of spinning mechanisms completes the same action, and continuous cascade spinning and reducing diameter is achieved through the traction machine. S3: Cooling process, cooling the deformed rod blank to obtain a fine-grained rod blank.

[0011] Preferably, each group of the spinning mechanism comprises a guide wheel, a torsion assembly and a ring pressing assembly which are sequentially arranged along the pulling and output direction of the continuous casting rod billet; The torsion assembly comprises a plurality of engaging parts which are arranged in a ring on the circumference of the continuous casting rod blank and rotate synchronously with the first rotating part, and a first control part which is used to control the plurality of engaging parts to move synchronously to continuously clamp the continuously transported continuous casting rod blank; The ring pressing assembly is coaxially arranged with the torsion assembly, and comprises a plurality of ring pressing parts which rotate synchronously with the second rotating part, and a device for controlling the plurality of ring pressing parts to intermittently reduce the diameter of the continuous casting rod blank by ring pressing during the synchronous rotation. The continuously casting rod blank after the diameter reduction is transmitted backward by traction after the ring pressing parts are released.

[0012] Preferably, the torsion angle of the torsion assembly is 90°~180°, and the downward deformation amount of each group of spinning mechanisms is 10%~20%.

[0013] Preferably, from the input direction to the output direction of the traction machine, the force of the torsion component of any group of spinning mechanisms is smaller than the force of the ring pressing component, and the diameter of the continuous casting rod billet gradually decreases under the spinning treatment of multiple groups of spinning mechanisms.

[0014] Preferably, in the oxygen-free smelting process, the oxygen-free smelting equipment includes an electromagnetic induction heating smelting furnace that is isolated from oxygen.

[0015] As another preferred embodiment, the high-content copper-silver alloy has the following components by weight: 0.5% to 50% silver, the remainder being copper and inevitable trace impurities, and the oxygen content being less than 20PP.

[0016] Beneficial effects of the present invention: (1) The purpose of using spinning instead of continuous extrusion in the processing of the high-content copper-silver alloy fine wire of the present invention is that continuous extrusion or horizontal extrusion will produce a large amount of overflow and waste, which will waste a lot of silver, while spinning can also refine the grains without any waste, saving silver raw materials and improving the utilization rate of raw materials; (2) The present invention reduces the copper-silver alloy residue in the furnace by vacuum continuous casting, and then uses the filter device with a guide filter hole higher than the bottom of the crucible to block the impurities precipitated at the bottom of the crucible, thereby reducing the impurities entering the casting rod, improving the molding quality of the casting rod, and meeting the processing requirements of fine lines; (2) The continuous casting rod blank of the present invention realizes continuous grain refinement of high-content copper-silver alloy through continuous multi-stage torsion pressure processing technology. Combined with surface treatment, drawing, annealing and other processes, the hard high-content copper-silver alloy material can be processed into fine wires. Combined with high-content copper-silver alloy technology, fine wires with excellent performance can be produced. The new continuous grain refinement technology and spinning mechanism of high-strength materials help to improve production flexibility and reduce production costs, and can be applied to the manufacture of various other high-strength copper alloy fine wire materials. The grain refinement of the material structure can increase toughness and eliminate casting defects, meeting the processing requirements of fine wires. (3) The present invention adopts a deformation method of torsion combined with ring pressing, and the transmission of the continuous casting rod blank is continuous. The torsion, spinning and transmission are all continuous, so the continuous casting rod blank can be continuously output. By using the continuous method, the work efficiency is greatly improved. At the same time, the bite part bites the continuous casting rod blank and drives the continuous casting rod blank to rotate. After loosening, the ring pressing part immediately continues to compact it to achieve the diameter change and flattening of the continuous casting rod blank. The torsion combined with spinning method can keep the continuous casting rod blank consistent in diameter reduction. In addition, the deformation method has good versatility, is suitable for both soft and hard alloys, and does not produce waste and overflow, and is more suitable for continuous fine wire processing.

[0017] In summary, the equipment has the advantages of strong versatility and high strength of copper-silver alloy microwires, and is particularly suitable for the field of non-ferrous metal processing technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0019] Figure 1 The figure is a schematic diagram of the process flow of the method for manufacturing high-content copper-silver alloy fine wires.

[0020] Figure 2 A schematic diagram of the structure of the filtering device.

[0021] Figure 3 This is the cross-sectional crystal phase diagram of the first-level twisting process of the continuous casting rod billet.

[0022] Figure 4 This is the cross-sectional crystal phase diagram of the first stage of the continuous casting rod billet ring pressing process.

[0023] Figure 5 This is the cross-sectional crystal phase diagram of the second stage torsion process of the continuous casting rod billet.

[0024] Figure 6 This is the cross-sectional crystal phase diagram of the second stage ring pressing process of the continuous casting rod billet.

[0025] Figure 7 It is a schematic diagram of the transmission status of the torsion component and the ring pressure component.

[0026] Figure 8 It is a schematic diagram of the internal structure of a ring compression component or a torsion component.

[0027] Fig. 9 It is a schematic diagram of the structure of the biting part or the ring pressing part. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention are clearly and completely described below in conjunction with the accompanying drawings.

[0029] Embodiment 1 like Figure 1 As shown, a method for manufacturing high-content copper-silver alloy fine wires includes an oxygen-free smelting process, an oxygen-free continuous casting process, a cascade spinning process, a surface treatment process, a heat treatment process and a drawing process. In the oxygen-free smelting process, a filtering device 4 is provided at the lower water outlet 31 of the crucible 3 in the smelting furnace, and a side wall of the filtering device 4 is provided with a guide filter hole 41 higher than the bottom of the crucible 3.

[0030] Furthermore, the high-content copper-silver alloy has the following composition by weight: 0.5% to 50% silver, the remainder being copper and inevitable trace impurities, and the oxygen content being less than 20 PPM.

[0031] Further, if Figure 2 As shown, the oxygen-free continuous casting process adopts a continuous downward casting method.

[0032] It should be noted that oxygen-free continuous casting also includes upward continuous casting and horizontal continuous casting. The reason why this example prefers downward casting is that downward casting can effectively avoid a large amount of copper-silver alloy from being retained at the bottom of the furnace and causing waste.

[0033] Further, if Figure 2 As shown, the filtering device 4 is inserted above the lower water outlet 31 at the bottom of the crucible 3 .

[0034] In detail, vacuum induction downward continuous casting is used to melt the copper-silver alloy. The crucible 3 is a graphite crucible. Graphite powder and smelting agent adhere to the inner wall of the crucible and are not easy to float. They will flow out under the scouring of copper water, causing the continuous casting wire to break. The bottom is provided with a three-layer graphite cylindrical filter device. Each layer of the filter sleeve has a guide filter side hole 41 on the side. At the same time, the upper end of the sleeve is higher than the liquid level of the lower outlet 31 of the crucible furnace, that is, the liquid outlet a through the sleeve is higher than the traditional liquid outlet b at the bottom of the crucible furnace. Impurities flow through the filter sleeve and float up and stay at the top of the sleeve. After the copper water is melted, silver blocks are added to the copper water according to the weight ratio. After the composition is uniform, downward continuous casting is performed to obtain a copper-silver rod blank with a diameter of 12 mm. The remaining small amount of alloy is very convenient to take out.

[0035] Further, if Figure 2 As shown, the filtering device 4 includes multiple nested graphite mesh sleeves 42, each graphite mesh sleeve 42 has a plurality of guide filter holes 41, and the heights of the guide filter holes 41 on the graphite mesh sleeves increase from the inside to the outside to the bottom of the crucible 3, and there is a distance between two adjacent graphite mesh sleeves 42 in the horizontal direction.

[0036] In this embodiment, the height of the guide filter holes 41 on the graphite mesh sleeve to the bottom of the crucible 3 is increased sequentially from the inside to the outside, so as to achieve multi-level isolation of impurities remaining at the bottom of the crucible 3, thereby further improving the continuous casting quality.

[0037] Furthermore, in the oxygen-free smelting process, the oxygen-free smelting equipment includes an electromagnetic induction heating smelting furnace that is isolated from oxygen.

[0038] Furthermore, in the oxygen-free smelting process, the high-content copper-silver alloy has the following composition by weight: 0.5% to 50% silver, the remainder being copper and inevitable trace impurities, and the oxygen content being less than 20 PPM.

[0039] It should be noted that the composition of the high-content copper-silver alloy fine wire is 4% silver by weight, and the balance is oxygen-free copper.

[0040] Furthermore, the surface treatment is performed to remove surface defects and oxides.

[0041] It should be noted that the surface treatment process is used to remove surface defects and oxides of the rod blank. The outer surface of the continuous casting rod blank after torsional ring pressing has a threaded shape. However, in the traditional manufacturing method of high-content copper-silver alloy fine wire, a surface treatment process is originally provided in the diameter reduction process. Therefore, no other difficulty and cumbersome processes are added to the process itself. However, a surface treatment process can also be provided before the heat treatment process, and annealing treatment can be performed by adopting inert gas protection.

[0042] Furthermore, the method also includes a heat treatment process, in which an inert gas protection heat treatment is used, and the annealing temperature of the copper-silver alloy after rough drawing is 250° C. to 500° C., and the alloy is kept warm for 2 hours and then cooled naturally.

[0043] Furthermore, it also includes cold drawing and fine drawing processes. During the processing, wire drawing equipment with cooling lubricating fluid is used to reduce the diameter and draw to obtain a finished copper-silver fine wire with a diameter of 0.02~0.2 mm and a conductivity of not less than 70% IACS.

[0044] Embodiment 2 like Figure 1 , Figures 3 to 9 As shown, the components identical or corresponding to those in the first embodiment are marked with the corresponding reference numerals in the first embodiment. For the sake of simplicity, only the differences from the first embodiment are described below. The second embodiment differs from the first embodiment in that: Further, if Figure 1 As shown, the cascade spinning process includes two or more spinning mechanisms 2 connected in series, specifically including the following steps: S1: straightening process, after straightening the continuous casting rod blank 100 with high content of copper-silver alloy, it is continuously and automatically output under the traction of a traction machine; S2: Spinning and reducing diameter process, the straightened continuous casting rod blank 100 passes through multiple groups of spinning mechanisms 2, each group of spinning mechanisms 2 first presses the continuous casting rod blank 100, and continuously twists it, and immediately performs continuous ring pressing and reducing diameter on the continuous casting rod blank 100 after twisting, and each group of spinning mechanisms 2 completes the same action, and realizes continuous cascade spinning and reducing diameter through the traction machine; S3: Cooling process, cooling the deformed rod blank to obtain a fine-grained rod blank.

[0045] In this embodiment, by setting up cascade spinning technology and cascade spinning mechanism, the deformation heat of the material is fully utilized to achieve continuous grain refinement of the material, which is beneficial to the processing of fine wires and reduces material waste. The method has simple equipment, flexibility and reliability, strong versatility, and convenient mold replacement, and can realize the production of various high-strength copper alloy fine wires at low cost.

[0046] In addition, the spinning mechanism 2 is used to feed the continuous casting rod blank into the first group of twisting components 2 through the traction mechanism. The bite portion 22 bites the rod blank to twist the rod blank by 120°. The twisting causes the grains of the rod blank material to break and recrystallize. The twisted billet is then pulled to the ring pressing for diameter reduction. The ring pressing portion 32 rotates synchronously and presses down reciprocatingly. The pressing deformation amount is 20%, which makes the rod blank thinner. The material deformation generates a large amount of deformation heat, so that the material temperature reaches about 250°C. The continuous casting rod blank 100 deformed in the first pass then enters the second pass unit and repeats the above deformation process. The material temperature can continue to rise to about 500°C. Recrystallization occurs under the spinning deformation. The ring pressing can further weld the internal defects of the material and increase the material density. The continuous casting rod blank 100 after diameter reduction is cooled by a water tank. Then, by replacing the bite portion 22 and the ring pressing portion 32 of different specifications, the diameter of the rod blank can be reduced to 8 mm after repeated cascade spinning, and high-precision fine wire production is completed.

[0047] Among them, the spinning and reducing process includes: a: twisting process, the continuous casting rod blank 100 is clamped by the twisting assembly 2 and twisted continuously while being pulled and transmitted backward, and each twisting angle is 90° to 180°; b: Ring pressing process, the twisted continuous casting rod blank 100 is brought to the ring pressing assembly 3 by a traction belt and immediately subjected to continuous ring pressing and diameter reduction, so that the diameter of the continuous casting rod blank 100 is reduced; In this embodiment, the first rotating part 21 drives the plurality of the bite parts 22 to rotate synchronously, and the continuous casting rod blank 100 before being pulled to the ring pressing assembly 3 is intermittently clamped under the action of the first control part 23. The continuous casting rod blank 100 is continuously twisted synchronously when it is clamped by the bite parts 22. For the continuous refinement process of the continuous casting rod blank in the cascade spinning process, the internal grain changes refer to Figure 3-6 shown.

[0048] It should be noted that when clamping the continuous casting rod blank 100, the diameter of the clamping space at the feeding end of the plurality of the bite parts 22 is larger than the diameter of the clamping space at the discharging end thereof.

[0049] Furthermore, the continuous casting rod blank 100 is continuously twisted synchronously when clamped by the ring pressing part 32, and the ring pressing parts are arranged in pairs opposite to each other, so as to ensure that the force is more stable and uniform during the extrusion deformation process. In addition, the first rotating part 21 and the second rotating part 31 rotate continuously during operation. Since the continuous casting rod blank 100 becomes slender during the ring pressing and diameter reduction process under the action of the ring pressing assembly 3, the rotation speed of the second rotating part 31 is not less than the rotation speed of the first rotating part 21. On the one hand, it is beneficial to ensure the quality of the section of the continuous casting rod blank between the torsion assembly 2 and the ring pressing assembly 3 to avoid fracture; on the other hand, it improves the continuous casting rod blank to enter the ring pressing assembly 3 for ring pressing and diameter reduction immediately after torsional deformation and grain refinement by the torsion assembly 3, and maximizes the use of the heat generated by the torsional deformation, thereby further improving the quality of the ring pressing and grain refinement.

[0050] Further, if Figures 7 to 9 As shown, each group of the spinning mechanism 2 comprises a guide wheel 21, a twisting assembly 22 and a ring pressing assembly 23 which are sequentially arranged along the pulling and output direction of the continuous casting rod blank 100; The torsion assembly 22 includes a plurality of engaging parts which are arranged around the circumference of the continuous casting rod blank and rotate synchronously with the first rotating part, and a first control part for controlling the synchronous movement of the plurality of engaging parts to continuously clamp the continuously transported continuous casting rod blank; The ring pressing assembly 23 is coaxially arranged with the torsion assembly, and comprises a plurality of ring pressing parts which rotate synchronously with the second rotating part, and a device for controlling the plurality of ring pressing parts to intermittently reduce the diameter of the continuous casting rod blank by ring pressing during the synchronous rotation. The continuously casting rod blank after the diameter reduction is transmitted backward by traction after the ring pressing parts are released.

[0051] The working principle of the torsion assembly 2 is as follows: the motor drives the bite part 22 to rotate through the belt, and twists it to loosen it, the bite part 22 opens and closes, and twists instantly when the bite part 22 is closed, and the travel size of the continuous casting rod billet each time it is twisted is not less than the traction travel distance in the same time, thereby achieving torsional deformation and grain refinement in the torsion process; It is worth noting that the torsion assembly 2 and the ring pressing assembly 3 are combined to form a mold tooling. The first rotating part 21 of the torsion assembly 2 can adopt a circular ring disk structure, and the bite part 22 is set in a plurality of groups along the circumferential direction of the first rotating part 21. The bite part 22 rotates synchronously under the drive of the first rotating part 21. During the rotation process, the bite part 22 is guided by the first control part 23 to gather toward the axis to complete the embracing and clamping work of the continuous casting rod blank 100; wherein, Fig. 9As shown, in order to improve the stability of the transmission, an elastic structure can also be provided in the first rotating part to support and guide the correspondingly installed bite part 22; the structure and working principle of the ring pressing assembly 3 are the same or similar to those of the torsion assembly, and are not described in detail here. However, the pressure F1 exerted by the torsion assembly 2 on the continuous casting rod blank 100 is less than the pressure F2 exerted by the ring pressing assembly 3 on the continuous casting rod blank 100 in the ring pressing process. The ring pressing assembly 3 further performs continuous ring pressing and diameter reduction on the continuous casting rod blank 100 after the primary grain refinement by the torsion assembly 2, so as to achieve secondary grain refinement, which is beneficial to the processing of fine wires.

[0052] The specific structure of the torsion assembly 2 and the ring pressing assembly 3 in this embodiment is the preferred structure of this technical solution for realizing the process, but is not limited to this structure. The protection scope of the present invention is not limited to this. Any changes or replacements that can be easily thought of by technicians familiar with this technical field under the technical prompts of the present invention should be covered within the protection scope of the present invention.

[0053] In addition, a guide wheel 1 is provided at the front end of the continuous casting rod billet to position and guide the transmission of the continuous casting rod billet. After the biting part bites the continuous casting rod billet, it drives the continuous casting rod billet to rotate. After loosening, the ring pressing part immediately continues to press it, that is, press down and rotate synchronously, to achieve diameter change and flattening of the continuous casting rod billet. Compared with the traditional diameter change method of pure drawing or pure extrusion, this torsion combined with ring pressing method has consistent product surface quality and consistent diameter reduction.

[0054] Furthermore, the torsion angle of the torsion assembly 22 is 90° to 180°, and the downward deformation amount of each group of spinning mechanisms 2 is 10% to 20%.

[0055] Further, if Figure 7 As shown, from the input direction to the output direction of the traction machine, the force of the torsion assembly 22 of any group of spinning mechanisms 2 is smaller than the force of the ring pressing assembly 23, and the diameter of the continuous casting rod blank 100 gradually decreases under the spinning treatment of multiple groups of spinning mechanisms 2.

[0056] Embodiment 3 A method for manufacturing a high-content copper-silver alloy fine wire, wherein the high-content copper-silver alloy has a composition by weight of: 0.5% to 50% silver, the remainder is copper and inevitable trace impurities, and the oxygen content is less than 20PPM. The specific steps of the processing technology are: Step A: straightening the continuous casting rod billet of high-content copper-silver alloy; Step B: The cascade structure is composed of two or more spinning machines connected in series. The cascade spinning machines respectively press the rod blank and twist it continuously. The twisting angle of each spinning machine is 120°~180°. After twisting, the rod blank is immediately subjected to ring pressing and diameter reduction. The downward deformation amount of each spinning machine is 10%~20%; each spinning machine completes the same action, and continuous cascade spinning diameter reduction is achieved through the traction mechanism.

[0057] Step C: continuously pulling the deformed rod blank to a water tank for cooling to obtain a fine-grained rod blank; The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for producing a high-content copper-silver alloy fine wire, characterized in that: The method comprises an oxygen-free smelting process, an oxygen-free continuous casting process, a cascade spinning process, a surface treatment process, a heat treatment process and a drawing process. In the oxygen-free smelting process, a filtering device is provided at the lower outlet of the crucible in the smelting furnace, and a flow guide filtering hole higher than the bottom of the crucible is provided on the side wall of the filtering device. The oxygen-free continuous casting process adopts a continuous downcasting method; The filtering device is inserted above the lower water outlet at the bottom of the crucible; The filtering device includes multiple nested graphite mesh sleeves, each of which has a plurality of guide and filter holes. The heights of the guide and filter holes on the graphite mesh sleeves to the bottom of the crucible increase sequentially from the inside to the outside, thereby performing multi-level isolation on impurities remaining at the bottom of the crucible.

2. The method for manufacturing a high-content copper-silver alloy fine wire according to claim 1, characterized in that: The continuous downcasting and melting of the copper-silver alloy adopts a vacuum induction method.

3. The method for manufacturing a high-content copper-silver alloy fine wire according to claim 2, characterized in that: In the oxygen-free smelting process, the oxygen-free smelting equipment includes an electromagnetic induction heating smelting furnace that is isolated from oxygen.

4. The method for manufacturing a high-content copper-silver alloy fine wire according to claim 1, characterized in that: The crucible is a graphite crucible, and graphite powder and a smelting agent are bonded to the inner wall of the crucible.

5. The method for manufacturing a high-content copper-silver alloy fine wire according to claim 1, characterized in that: The graphite mesh sleeves are arranged in three groups, and there is a gap between two adjacent graphite mesh sleeves in the horizontal direction.

6. The method for manufacturing a high-content copper-silver alloy fine wire according to claim 1, characterized in that: The upper end of the graphite mesh sleeve is higher than the liquid level of the lower outlet of the crucible. Impurities flow through the graphite mesh sleeve and float up to the top of the sleeve. After the copper water is melted, silver blocks are added to the copper water according to weight proportion. After the composition is uniform, the lower continuous casting is carried out to obtain the copper-silver rod blank.

7. A method for manufacturing a high-content copper-silver alloy fine wire according to any one of claims 1 to 6, characterized in that: The cascade spinning process includes two or more spinning mechanisms connected in series, and specifically includes the following steps: S1: Straightening process, after straightening the continuous casting rod billet with high content of copper and silver alloy, it is continuously and automatically output under the traction of the traction machine; S2: Spinning and reducing diameter process. The straightened continuous casting rod billet passes through multiple groups of spinning mechanisms. Each group of spinning mechanisms first presses the continuous casting rod billet and continuously twists it. After twisting, the continuous casting rod billet is immediately subjected to continuous ring pressing and reducing diameter. Each group of spinning mechanisms completes the same action, and continuous cascade spinning and reducing diameter is achieved through the traction machine. S3: Cooling process, cooling the deformed rod blank to obtain a fine-grained rod blank.

8. The method for manufacturing a high-content copper-silver alloy fine wire according to claim 7, characterized in that: Each group of the spinning mechanism comprises a guide wheel, a twisting assembly and a ring pressing assembly which are sequentially arranged along the pulling and output direction of the continuous casting rod blank; The torsion assembly comprises a plurality of engaging parts which are arranged in a ring on the circumference of the continuous casting rod blank and rotate synchronously with the first rotating part, and a first control part which is used to control the plurality of engaging parts to move synchronously to continuously clamp the continuously transported continuous casting rod blank; The ring pressing assembly is coaxially arranged with the torsion assembly, and comprises a plurality of ring pressing parts which rotate synchronously with the second rotating part, and a device for controlling the plurality of ring pressing parts to intermittently reduce the diameter of the continuous casting rod blank by ring pressing during the synchronous rotation. The continuously casting rod blank after the diameter reduction is transmitted backward by traction after the ring pressing parts are released.

9. The method for manufacturing a high-content copper-silver alloy fine wire according to claim 7, characterized in that: From the input direction to the output direction of the traction machine, the force of the torsion component of any group of spinning mechanisms is smaller than the force of the ring pressing component, and the diameter of the continuous casting rod billet gradually decreases under the spinning treatment of multiple groups of spinning mechanisms.

10. A method for manufacturing a high-content copper-silver alloy fine wire according to any one of claims 1 to 9, characterized in that: The high-content copper-silver alloy has the following components by weight: 0.5% to 50% silver, the remainder copper and inevitable trace impurities, and an oxygen content of less than 20 PPM.

Citation Information

Patent Citations

  • A continuous casting device and a continuous casting method for continuously casting castings formed by magnesium or magnesium alloys

    CN103286286A

  • Superfine copper, silver and rare earth alloy wire and production method thereof

    CN106282651A

  • Production process of copper-chromium-zirconium rod material

    CN113981258A

  • Molten metal supply pipe and continuous casting device

    JP2013169589A

  • Pressure slip casting apparatus and method for casting a molded article

    WO2009106061A2

Cited By

  • Continuous casting system and continuous casting method for silver alloy

    CN119407122A