Method for correcting deformation of large irregular casting
Through 3D scanning and design data model comparison, combined with the thermal correction method, the problem of difficulty in finding the deformation position of large irregular castings was solved, and the correction accuracy and cost-effectiveness were achieved.
Patent Information
- Application Number
- CN202410993251.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Large irregular castings are deformed during shrinkage or heat treatment. Traditional manual measurement and machine tool marking are difficult to accurately identify the location and degree of deformation, making correction difficult.
Obtain the three-dimensional data of the workpiece through 3D scanning, compare it with the design data model to find out the theoretical deformation position, make a conformal template and perform longitudinal slicing processing, combine the thermal correction method to correct the deformation position, and use the reference slice and measurement surface to determine the template size. Adjust the workpiece step by step until standard tolerances are reached.
It achieves the accurate identification and correction of deformation of large irregular castings, reduces production costs, avoids scrapping of workpieces due to insufficient correction or over-correction, and improves the accuracy and reliability of correction.
Smart Images

Figure CN118768474A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of shipbuilding, and in particular to a method for correcting deformation of large irregular castings. Background Art
[0002] Castings often deform during shrinkage or heat treatment, which can be corrected by heating, welding or pressure correction. For regular products, the deformation position and degree can be marked by manual measurement or marking. However, for large irregular castings, such as marine parts, the parts are irregular and asymmetrical in shape, have no reference or the reference is more than 10 meters away, and the faces are not vertical or parallel. Once a casting is deformed, it is impossible to use traditional manual measurement, marking or even machine tool dotting to find the deformation position and degree. Therefore, how to find the problem, land it on the correction site, and accurately correct it has become a difficulty in correction technology. Summary of the invention
[0003] In view of the problems and shortcomings in the prior art, the present invention provides a method for correcting deformation of large irregular castings.
[0004] The technical solution of the present invention is as follows:
[0005] A method for correcting deformation of large irregular castings, characterized by comprising the following steps:
[0006] S1, scanning the workpiece to obtain three-dimensional data of the workpiece;
[0007] S2, compare the workpiece 3D data with the design data model to find out the theoretical deformation position;
[0008] S3, longitudinally slicing the theoretical deformation position, setting the slice at the position with the largest deformation as the reference slice, and making a conformal template at the reference slice, including the following steps:
[0009] S31: Perform longitudinal slicing at the theoretical deformation position, compare the difference between the longitudinal slice and the intersection line of the workpiece 3D data and the design data model contour, take the longitudinal slice with the largest difference as the reference slice O, take the outer contour surface of the design data model that intersects with the reference slice O and corresponds to the theoretical deformation position as the measurement surface N, and define any surface of the design data model that intersects with the reference slice O and is not deformed as the reference surface M;
[0010] S32: Obtain the intersection lines m and n of the reference slice, the reference surface M and the measuring surface N, and then determine the reference side a and the measuring side b of the conformal template according to the positions and sizes of the intersection lines m and n, and make the conformal template according to the size of the workpiece;
[0011] S4, placing the conformal template at the deformed position on the workpiece for comparison, and calculating the actual deformation value of the deformed position of the workpiece;
[0012] S5, correcting the deformation position of the workpiece by using a thermal correction method according to the actual deformation value of the workpiece;
[0013] S6, comparing the conformal template with the corrected workpiece, if the actual deformation value after correction is less than the standard tolerance value T, then executing step S7, otherwise executing step S5;
[0014] S7, scan the corrected workpiece to obtain the corrected three-dimensional data of the workpiece, and compare it with the design data model. If the deformation is less than the standard tolerance value, the correction is completed, otherwise repeat steps S2-S6 until the deformation of the workpiece is less than the standard tolerance value.
[0015] In step S32, the sizes of the reference side a and the measuring side b of the conformal template are respectively larger than the corresponding sizes of the reference surface M and the measuring surface N of the workpiece matched therewith.
[0016] The step S4 is implemented by the following specific operations:
[0017] S41: matching the reference side a of the conformable template with the reference surface A of the workpiece, and matching the measuring side b with the deformation surface B of the workpiece, wherein the reference surface A is the surface on the workpiece opposite to the reference surface M in the design data model, and the deformation surface B is the surface opposite to the measurement surface N in the design data model;
[0018] S42: Measure the longitudinal difference between the deformation surface B and the measurement edge b, mark the position beyond the tolerance as the actual deformation position, and record the actual deformation value δ1.
[0019] The step S5 is implemented by the following specific operations:
[0020] S51: Calculating a correction value δ2 of the workpiece according to an actual deformation value δ1 of the workpiece;
[0021] S52: Place the special correction platform on the kiln car of the heat treatment kiln and level it with a level;
[0022] S53: stably placing the workpiece on a special correction platform, and setting a steel pad under the non-deformed position of the workpiece, and setting a wooden pad with a height greater than the correction value under the deformed position of the workpiece;
[0023] S54: two weights are arranged above the workpiece, one is a fixed weight, which is placed above the side opposite to the deformed position of the workpiece and fixedly connected to the dedicated platform, and the other is a correcting weight, which is placed just above the deformed position of the workpiece;
[0024] Among them, the weight calculation formula of the correction weight is: G J =k*S min*σS / g, where k represents the adjustment coefficient, and the value range is: 0.01 to 0.015; S min represents the minimum value of the cross-sectional area at the deformation position; σ S represents the yield stress of the workpiece material; g represents the acceleration due to gravity;
[0025] S55: Push the kiln car into the heat treatment kiln for heating and straightening until it reaches the plastic softening state as a whole, and then perform slow cooling in the furnace.
[0026] The height of the wooden cushion block in step S53 is 2 - 10 mm larger than the straightening value δ2. The weight of the fixed iron weight in step S54 is not less than 3 times the weight of the workpiece.
[0027] The above step S55 is realized through the following specific operations:
[0028] Heat the heat treatment kiln to 50°C - 100°C above the plastic deformation temperature of the workpiece, keep it warm for 4 - 7 hours, perform slow cooling in the furnace after reaching the plastic softening state as a whole, and take it out of the kiln when the temperature drops below 300°C. The heating rate of the heat treatment kiln during heating is controlled at 30 - 50°C / h.
[0029] The above step S6 is realized through the following specific operations:
[0030] S61: Cool the workpiece to below 100°C and shot blast the iron oxide on the surface of the workpiece;
[0031] S62: Place the profiling template at the deformed position of the straightened workpiece, measure the actual deformation value δ'1 after straightening and compare it with the standard tolerance T to judge the straightening result. If δ'1 < T, then execute step S7; otherwise, execute step S5.
[0032] The beneficial effects of the present invention are:
[0033] This method solves the problem that the deformed position of irregular workpieces cannot be accurately found and accurately straightened, reduces the situation that the workpieces do not meet the manufacturing tolerance requirements due to workpiece deformation, inaccurate straightening or over-straightening, resulting in workpiece scrapping. Moreover, this method is accurate, reliable, easy to operate, and has an extremely low production process cost, which can effectively reduce the production cost. Description of the Drawings
[0034] Figure 1 It is a comparison diagram of the three-dimensional data of the workpiece and the design data model and a slicing schematic diagram;
[0035] Figure 2 It is a schematic diagram of the comparison between the profiling template and the workpiece;
[0036] Figure 3 It is a process setting diagram of the workpiece before entering the cooling kiln;
[0037] 1. Design data model; 2. Workpiece three-dimensional data; 3. Workpiece; 4. Random sample; 5. Special correction platform; 6. Correction pressure iron; 7. Fixed pressure iron. DETAILED DESCRIPTION
[0038] The technical means adopted to achieve the predetermined inventive objectives of the present invention will be further described below in conjunction with the accompanying drawings in the embodiments of the present invention.
[0039] S1, scanning the workpiece to obtain three-dimensional data of the workpiece;
[0040] In the specific implementation, the workpiece is first placed on the workpiece platform, and then the operator uses a handheld 3D laser scanner to scan the workpiece to obtain the complete three-dimensional data of the workpiece, including geometric information and dimensional information, and transmit and view it through a computer.
[0041] Specifically, taking a marine bracket as an example, it is placed horizontally on the workpiece platform, and a handheld 3D laser scanner is used to scan it to obtain the three-dimensional data of the bracket, and the obtained data is uploaded to the CAD software module on the computer for viewing.
[0042] S2, compare the workpiece 3D data with the design data model to find out the theoretical deformation position;
[0043] The three-dimensional data of the workpiece obtained in the previous step is called and compared with the designed three-dimensional model of the workpiece to find the theoretical deformation position.
[0044] In practice, the workpiece 3D data and design data model obtained after the previous scan are imported into the software for comparison. The specific comparison method is to set the tolerance range in the software according to the standard tolerance T. When the deformation difference exceeds the standard tolerance range, it is determined as the theoretical deformation position and the color changes to indicate. Specifically, the standard tolerance value T is determined according to the casting size tolerance table in GB / T 6414-2017.
[0045] For example, the three-dimensional data of the marine bracket obtained above is compared with the design data model of the marine bracket in the CAD software module, and the standard tolerance is set to 10 mm in the software. When the three-dimensional data of the marine bracket is deformed by more than 10 mm compared with the design data model, the corresponding deformed position will be automatically highlighted.
[0046] S3, making a conformal template at the deformation position according to the theoretical deformation position;
[0047] S31: Perform longitudinal slicing at the theoretical deformation position, compare the difference between the longitudinal slice and the intersection line of the workpiece three-dimensional data and the design data model contour, take the longitudinal slice with the largest difference as the reference slice O, take the outer contour surface of the design data model that intersects with the reference slice O and corresponds to the theoretical deformation position as the measurement surface N, and define any surface of the design data model that intersects with the reference slice O and is not deformed as the reference surface M;
[0048] S32: Obtain intersection lines m and n between the reference slice and the reference surface M and the measurement surface N of the workpiece design data model, and then determine the reference side a and the measurement side b of the conformal template according to the positions and sizes of the intersection lines m and n;
[0049] S33: making a conformable template according to the size of the workpiece. Specifically, the sizes of the reference side a and the measuring side b of the conformable template are slightly larger than the corresponding sizes of the reference surface and the deformation surface of the workpiece matched therewith.
[0050] For example, the length of the reference side a of the conformable template is 5-10 mm greater than the extension length of the reference surface M of the ship support, and the length of the measuring side b is 10-15 mm greater than the extension length of the deformation surface of the ship support. The size of the side of the conformable template can be determined based on the principle of using space and saving materials. In this embodiment, the height of the side of the conformable template close to the reference side is greater than the height of the side away from the reference side, the purpose is to ensure that the reference side is completely in contact with the reference surface of the workpiece, and the side away from the reference side only needs the measuring side at the bottom to match the deformation surface of the workpiece, so the height size is not limited, and the high pressure is designed to be half of the height of the side adjacent to the reference side to save materials.
[0051] S4, placing the conformal template at the deformed position on the workpiece for comparison, and calculating the actual deformation value of the deformed position of the workpiece;
[0052] S41: placing the conformal template at the reference slice position of the workpiece, and making its reference side a match with the reference surface A of the workpiece, and the measuring side b match with the deformation surface B of the workpiece, wherein the reference surface A is the surface on the workpiece opposite to the reference surface M in the design data model, and the deformation surface B is the surface opposite to the measuring surface N in the design data model;
[0053] Specifically, it is necessary to ensure that the reference edge a is completely in contact with the reference surface A of the workpiece, the measuring edge b is in contact with the non-deformed position of the deformation surface B of the workpiece, and a gap appears at the deformed position, which is the actual deformation height difference.
[0054] S42: Then measure the longitudinal difference between the deformation surface B and the measurement edge b, mark the position beyond the tolerance as the actual deformation position, and record the actual deformation value δ1.
[0055] S5, correcting the deformation position of the workpiece by using a thermal correction method according to the actual deformation value of the workpiece;
[0056] S51: Calculating a correction value δ2 of the workpiece according to an actual deformation value δ1 of the workpiece;
[0057] S52: Place the special correction platform on the kiln car of the heat treatment kiln and level it with a level;
[0058] S53: stably placing the workpiece on a special correction platform, and setting a steel pad under the non-deformed position of the workpiece, and setting a wooden pad under the deformed position of the workpiece, and the height of the wooden pad is 2 to 10 mm greater than the correction value;
[0059] S54: two weights are arranged above the workpiece, one is a fixed weight, which is placed above the opposite side of the deformation position of the workpiece and fixedly connected to the dedicated platform to ensure the stability of the workpiece when it expands due to heat, and the other is a correcting weight, which is placed directly above the deformation position of the workpiece;
[0060] Among them, the weight of the fixed weight shall not be less than 3 times the weight of the workpiece; the weight calculation formula of the correction weight is: G J =k*S min *σ S / g, where k represents the adjustment coefficient, with a value range of 0.01 to 0.015; S min Indicates the minimum value of the cross-sectional area at the deformation position; σ S represents the yield stress of the workpiece material; g represents the acceleration due to gravity.
[0061] S55: Push the kiln car into the heat treatment kiln for heating correction. Heat the heat treatment kiln to 50℃-100℃ above the plastic deformation temperature of the workpiece. Control the heating rate at 30-50℃ / h. Keep warm for 4-7 hours to ensure that the temperature inside and outside the workpiece is consistent and the whole workpiece reaches a plastic softening state. Then slowly cool it in the furnace to release the stress caused by the correction deformation. Take it out of the kiln when the temperature drops below 300℃.
[0062] After the kiln car enters the heat treatment kiln, as the temperature rises, the wooden pad set below the deformation position burns, the workpiece loses its support point below the deformation position and is affected by the downward gravity of the correction pressure iron. At the same time, as the temperature rises, the workpiece reaches a plastic softening state, and the workpiece deforms in the opposite direction to gradually offset the deformation value, so that the deformation position of the workpiece is corrected. After correction, the workpiece is slowly cooled in the furnace to release the stress caused by the correction deformation, eliminate residual stress, and ensure that there is no rebound after leaving the kiln.
[0063] S6, compare the conformal template with the corrected workpiece. If the actual deformation value after correction is less than the standard tolerance value, execute step S7, otherwise execute step S5.
[0064] S61: After leaving the kiln, the workpiece is cooled to below 100°C and the iron oxide on the surface of the workpiece is cleaned by shot blasting;
[0065] S62: Place the conforming template at the sliced position of the corrected workpiece, measure the actual deformation value δ'1 after correction and compare it with the standard tolerance T to judge the correction result. If δ'1 < T, execute step S7; otherwise, execute step S5.
[0066] S7: Scan the corrected workpiece with a scanner to obtain the three-dimensional data of the workpiece after correction, and compare it with the design data model. If the deformation amount is less than the standard tolerance value T, the correction is completed; otherwise, repeat steps S2 - S6 until the deformation amount of the workpiece is less than the standard tolerance value.
[0067] The above is the preferred embodiment of the present invention. However, the present invention is not limited to the above embodiments and examples. All changes, equivalent substitutions, improvements, etc. made within the knowledge scope of those skilled in the art without departing from the concept of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for correcting deformation of large irregular castings, characterized in that: The following steps are involved: S1, scanning the workpiece to obtain three-dimensional data of the workpiece; S2, compare the workpiece 3D data with the design data model to find out the theoretical deformation position; S3, longitudinally slicing the theoretical deformation position, setting the slice at the position with the largest deformation as the reference slice, and making a conformal template at the reference slice, including the following steps: S31: Perform longitudinal slicing at the theoretical deformation position, compare the difference between the longitudinal slice and the intersection line of the workpiece 3D data and the design data model contour, take the longitudinal slice with the largest difference as the reference slice O, take the outer contour surface of the design data model that intersects with the reference slice O and corresponds to the theoretical deformation position as the measurement surface N, and define any surface of the design data model that intersects with the reference slice O and is not deformed as the reference surface M; S32: Obtain the intersection lines m and n of the reference slice, the reference surface M and the measuring surface N, and then determine the reference side a and the measuring side b of the conformal template according to the positions and sizes of the intersection lines m and n, and make the conformal template according to the size of the workpiece; S4, placing the conformal template at the deformed position on the workpiece for comparison, and calculating the actual deformation value of the deformed position of the workpiece; S5, correcting the deformation position of the workpiece by using a thermal correction method according to the actual deformation value of the workpiece; S6, comparing the conformal template with the corrected workpiece, if the actual deformation value after correction is less than the standard tolerance value T, then executing step S7, otherwise executing step S5; S7, scan the corrected workpiece to obtain the corrected three-dimensional data of the workpiece, and compare it with the design data model. If the deformation is less than the standard tolerance value, the correction is completed, otherwise repeat steps S2-S6 until the deformation of the workpiece is less than the standard tolerance value.
2. The correction method according to claim 1, characterized in that: In step S32, the sizes of the reference side a and the measuring side b of the conformal template are respectively larger than the corresponding sizes of the reference surface M and the measuring surface N of the workpiece matched therewith.
3. The correction method according to claim 1, characterized in that: The step S4 is implemented by the following specific operations: S41: matching the reference side a of the conformable template with the reference surface A of the workpiece, and matching the measuring side b with the deformation surface B of the workpiece, wherein the reference surface A is the surface on the workpiece opposite to the reference surface M in the design data model, and the deformation surface B is the surface opposite to the measurement surface N in the design data model; S42: Measure the longitudinal difference between the deformation surface B and the measurement edge b, mark the position beyond the tolerance as the actual deformation position, and record the actual deformation value δ1.
4. The correction method according to claim 3, characterized in that: The step S5 is implemented by the following specific operations: S51: Calculating a correction value δ2 of the workpiece according to an actual deformation value δ1 of the workpiece; S52: Place the special correction platform on the kiln car of the heat treatment kiln and level it with a level; S53: stably placing the workpiece on a special correction platform, and setting a steel pad under the non-deformed position of the workpiece, and setting a wooden pad with a height greater than the correction value under the deformed position of the workpiece; S54: two weights are arranged above the workpiece, one is a fixed weight, which is placed above the side opposite to the deformed position of the workpiece and fixedly connected to the dedicated platform, and the other is a correcting weight, which is placed just above the deformed position of the workpiece; Among them, the weight calculation formula of the correction weight is: G J =k*S min *σ S / g, where k represents the adjustment coefficient, with a value range of 0.01 to 0.015; S min Indicates the minimum value of the cross-sectional area at the deformation position; σ S represents the yield stress of the workpiece material; g represents the acceleration of gravity; S55: Push the kiln car into the heat treatment kiln for heating and straightening until the whole reaches the plastic softening state, and then perform slow cooling in the furnace.
5. The correction method according to claim 4, characterized in that: The height of the wooden spacer block in step S53 is 2 - 10 mm larger than the straightening value δ2.
6. The correction method according to claim 4, characterized in that: The weight of the fixed iron weight in step S54 is not less than 3 times the weight of the workpiece.
7. The correction method according to claim 4, characterized in that: Step S55 is realized through the following specific operations: Heat the heat treatment kiln to 50℃ - 100℃ above the plastic deformation temperature of the workpiece, keep it warm for 4 - 7 hours, perform slow cooling in the furnace after the whole reaches the plastic softening state, and take the workpiece out of the kiln when the temperature drops below 300℃.
8. The correction method according to claim 7, characterized in that: The heating rate of the heat treatment kiln is controlled at 30 - 50℃ / h.
9. The correction method according to claim 1, characterized in that: Step S6 is realized through the following specific operations: S61: Cool the workpiece to below 100℃, and shot blast the iron oxide on the surface of the workpiece; S62: Place the profiling template at the deformed position of the straightened workpiece, measure the actual deformation value δ'1 after straightening and compare it with the standard tolerance T to judge the straightening result. If δ'1 < T, then execute step S7; otherwise, execute step S5.
Citation Information
Patent Citations
Method of detecting inner type surface and curved surface errors of wind tunnel contraction section
CN107389293A
Detection device for surface profile of guider vane channel face
CN110440674A
Forming and correcting manufacturing method for aluminum alloy vehicle head skin of urban railway vehicle
CN112191708A
Spherical surface shape detection method of hemispherical resonator
CN112729159A
Profiling method for steel plate with spatial distortion structure