Sand core structure for piston casting and piston casting process
By designing a sand core structure for piston casting that integrates the pouring and riser, and using inkjet printing and sequential solidification technology, the problems of mold complexity and assembly difficulty are solved, the process is simplified and the quality of castings is improved, which is suitable for industrial production. .
Patent Information
- Application Number
- CN202410751480.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing sand core casting piston process, the mold design is complex, the assembly is difficult, and the process is complicated, which affects product development efficiency and casting consistency, and the manufacturing cost is high.
A sand core structure for piston casting is used, including a bottom mold, an outer mold, a core mold and a top mold. The pouring and riser is designed to be an integrated runner and riser. The sand core structure is formed by inkjet printing, simplifying the assembly process and using Sequential solidification and gravity realize self-feeding of castings, reducing cold iron and multiple processes.
It simplifies the sand core structure design and casting process, improves production efficiency, reduces manufacturing costs, ensures the quality and consistency of castings, and is suitable for industrial production.
Smart Images

Figure CN118768520A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of piston casting, in particular to a sand core structure for piston casting and a piston casting process. Background Art
[0002] In the related art, in the sand core casting piston process, the sand core design is subject to the problems of mold parting and sand core demolding, and generally requires the setting of special runners, adding chillers, spraying paint, drying and other processes. For example, it is necessary to place chillers in thick and large parts or locations prone to shrinkage, or to set up multiple risers for shrinkage compensation to ensure the quality of the casting. This leads to: on the one hand, the structural design of the sand core is complex and the assembly is difficult; on the other hand, the piston manufacturing process is complicated, which seriously affects the efficiency of product development, the process consistency is difficult to guarantee, and the manufacturing cost is high. Summary of the invention
[0003] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.
[0004] To this end, the purpose of the present invention is to provide a sand core structure for piston casting and a piston casting process, which does not require the design of a separate runner and simplifies the sand core structure. At the same time, sequential solidification can be achieved without the need to set up a chiller, simplifying the casting process.
[0005] In order to achieve the above-mentioned purpose, the technical solution of the present invention provides a sand core structure for piston casting, including: a bottom mold, an outer mold, a core mold and a top mold that are arranged in coordination, the sand core structure as a whole is designed to correspond to the piston top facing upward, the wall thickness of the bottom mold and the outer mold are consistent, the top mold is located at the geometric center of the sand core structure, and the interior of the core mold is a hollow conformal design, wherein the core mold is assembled to the inside of the bottom mold, the outer mold is assembled above the bottom mold, and the top mold is assembled to the top of the outer mold; a pouring riser is arranged above the top mold, and the pouring riser coincides with the central axis of the top mold, and the pouring riser is communicated with the internal cavity of the top mold.
[0006] Preferably, the height of the pouring and riser is 1 / 5-1 / 3 of the height of the assembled bottom mold, the outer mold and the top mold.
[0007] Preferably, the outer diameter of the bottom end of the pouring riser is the same as the internal cavity width of the top mold, and gradually widens from the bottom end to above the top surface of the top mold. The inner diameter of the pouring riser above the top mold is 60-110mm.
[0008] Preferably, the internal shape of the bottom mold, outer mold, core mold and top mold after assembly is the same as the designed casting shape.
[0009] Preferably, the pouring and rising nozzle is assembled to the top mold, and the assembly surface between the two is stepped;
[0010] Alternatively, the pouring head and the top mold are integrally formed.
[0011] Preferably, the assembly surfaces among the structures in the bottom mold, the outer mold, the core mold and the top mold are stepped.
[0012] The technical solution of the present invention also provides a piston casting process using the sand core structure for piston casting in the above technical solution, comprising the following steps:
[0013] Design shrinkage coefficient and castings according to piston product model;
[0014] Design the bottom mold, outer mold, core mold, top mold and pouring riser of the sand core structure according to the casting;
[0015] According to the three-dimensional data model of the bottom mold, outer mold, core mold, top mold and pouring riser, an inkjet printer is used to print, and quartz sand or ceramsite sand is combined by spraying a binder, and stacked layer by layer to form a sand core structure;
[0016] The printed bottom mold, outer mold, core mold, top mold and pouring riser are sanded and assembled from bottom to top, wherein the bottom mold is placed first, then the core mold is installed into the bottom mold, and then the outer mold, top mold and pouring riser are assembled;
[0017] The assembled sand core structure for piston casting is buried in the sand box, and then the smelted metal liquid is poured into the sand core structure through the pouring riser until the pouring riser is filled with metal liquid, thus completing the piston casting;
[0018] The cooled sand core structure is disassembled to obtain a piston casting.
[0019] Preferably, when the smelted metal liquid is poured into the sand core structure through the pouring riser, the pouring speed of the metal liquid is controlled at 60-120 kg / min, and the casting time is controlled within 1 min;
[0020] The metal liquid includes but is not limited to ductile iron liquid, gray iron liquid, and aluminum alloy liquid.
[0021] Preferably, the shrinkage coefficient is 0.9-1.1.
[0022] Preferably, when assembling the sand core structure for piston casting, the core mold is first positioned by the bottom mold and then pressed and fixed by the outer mold; the assembly gap between the core mold, the outer mold and the bottom mold is ≤0.5mm.
[0023] The sand core structure for piston casting and the piston casting process proposed by the present invention have the following beneficial technical effects:
[0024] (1) The unique pouring and riser design in the sand core structure for piston casting proposed in the present invention serves as both a runner and a riser, and there is no need to design a separate runner. The structural design is simple and reliable. At the same time, the pouring and riser is the highest point in position and the highest point in temperature, and the sequential solidification and gravity effects can be used to achieve self-shrinkage compensation of the casting, thereby simplifying the piston casting process while ensuring the quality of the casting.
[0025] (2) The sand core structure for piston casting proposed in the present invention is designed to face the piston top upward, which is conducive to ensuring the sequential solidification of the casting. The wall thickness of the bottom mold and the outer mold is consistent, which can ensure the cooling speed. The top mold is located at the geometric center of the sand core structure, which can ensure the gravity self-compensation function. The interior of the core mold is a hollow conformal design, which can play a breathable role, thereby further ensuring the quality of the casting.
[0026] (3) The sand core structure for piston casting proposed in the present invention can realize conformal design, realize sequential solidification of the casting from bottom to top, make the cooling rate of the casting uniform, ensure the quality of the casting, and solve the problems of bloated structure and complex assembly of traditional sand core casting piston molds.
[0027] (4) The present invention proposes a sand core structure parting design for piston casting, in which the assembly surface between each structure is stepped. On the one hand, it can prevent the metal liquid from flowing out, on the other hand, it simplifies the assembly process of the sand core structure, and on the other hand, it is conducive to achieving self-shrinkage compensation for the casting, further ensuring the quality of the casting.
[0028] (5) The piston casting process proposed in the present invention has a simplified process, saves multiple steps such as placing cold iron, spraying paint, and baking, greatly improves production efficiency, saves manufacturing costs, and has a wide range of applications and can be applied to industrial production.
[0029] (6) The piston casting process proposed in the present invention utilizes a unique sand core structure for piston casting. After the metal liquid is poured from the pouring head, the pouring head has the highest temperature and the highest position. Through sequential solidification and gravity, the self-shrinkage function of the casting is realized, thereby ensuring the casting quality.
[0030] (7) The piston casting process proposed in the present invention ensures the dimensional qualification rate of the castings by designing the shrinkage coefficient.
[0031] Additional aspects and advantages of the present invention will be given in part in the following description, and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0033] Figure 1 A schematic structural diagram of a sand core structure for piston casting according to an embodiment of the present invention is shown;
[0034] Figure 2 A schematic structural diagram of a sand core structure for piston casting according to another embodiment of the present invention is shown;
[0035] Figure 3 A schematic structural diagram of a sand core structure for piston casting according to another embodiment of the present invention is shown.
[0036] in, Figures 1 to 3 The corresponding relationship between the reference numerals and the components is as follows:
[0037] 102 bottom mold, 104 outer mold, 106 core mold, 108 top mold, 110 pouring and riser, 112 stepped assembly surface. DETAILED DESCRIPTION
[0038] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.
[0039] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0040] Combine the following Figures 1 to 3 A sand core structure for piston casting and a piston casting process according to an embodiment of the present invention are specifically described.
[0041] like Figures 1 to 3As shown, a sand core structure for piston casting according to an embodiment of the present invention includes: a bottom mold, an outer mold, a core mold, a top mold, a pouring nozzle, etc. The overall sand core structure is designed to correspond to the piston top upward, which can ensure the sequential solidification of the casting. The wall thickness of the bottom mold and the outer mold is consistent, which can ensure the cooling speed. The top mold is located at the geometric center of the sand core structure, which can ensure the gravity self-compensation function. The core mold is hollow and conformable, which can play a breathable role. The core mold is assembled to the inside of the bottom mold, the outer mold is assembled above the bottom mold, and the top mold is assembled above the outer mold. The pouring nozzle is arranged above the top mold, and the pouring nozzle coincides with the central axis of the top mold, and is connected to the internal cavity of the top mold. Thereby, the pouring nozzle can be used as a runner and a nozzle, without the need for a separate runner, so that the entire sand core structure for piston casting is simple in design and easy to assemble. First, pour the metal liquid into the pouring riser as a pouring cup. After the pouring is completed, it is used as a riser. At this time, the temperature is the highest and the position is also the highest. Therefore, the self-shrinkage function of the casting can be realized by utilizing the effects of sequential solidification and gravity to ensure the quality of the casting.
[0042] Furthermore, if Figure 1 As shown, the height of the pouring and riser is 1 / 5-1 / 3 of the height of the assembled bottom mold, outer mold and top mold.
[0043] Furthermore, if Figure 1 As shown, the outer diameter of the bottom end of the pouring riser is the same as the internal cavity width of the top mold, and gradually widens from the bottom end to above the top surface of the top mold. The inner diameter of the pouring riser above the top mold is 60-110mm.
[0044] Thereby, the integrated function of the pouring riser as a runner and a riser is further ensured.
[0045] Furthermore, the internal shape of the bottom mold, outer mold, core mold and top mold after assembly is the same as the designed casting shape. Through this upper and lower parting and shape-conforming design, the cooling speed of the casting is further guaranteed to be uniform, and high-quality piston castings can be produced in a simplified structure without the need for a chiller.
[0046] Further, the pouring riser is assembled to the top mold, and the assembly surface between the two is stepped;
[0047] Alternatively, the pouring riser and the top mold are integrally formed.
[0048] The assembly surfaces among the structures of the bottom mold, the outer mold, the core mold and the top mold are stepped.
[0049] Therefore, on the one hand, the outflow of metal liquid can be prevented; on the other hand, the assembly process of the sand core structure is simplified; on the other hand, it is conducive to realizing self-shrinkage compensation of the casting and further ensuring the quality of the casting.
[0050] Example 1
[0051] A piston casting process, using Figure 1 The sand core structure for piston casting and the ductile iron QT700-2 metal liquid are shown. Specifically, the following steps are included:
[0052] S102, design the shrinkage coefficient and casting according to the piston product model, and the shrinkage coefficient is 1.1;
[0053] S104, design the bottom mold, outer mold, core mold, top mold and pouring riser of the sand core structure according to the casting, such as Figure 1 As shown, the height of the bottom mold is 95mm, the height of the outer mold is 110mm, the height of the core mold is 220mm, the height of the top mold is 90mm, the height of the pouring head is 70mm, the inner diameter is 70mm, and the outer diameter is 120mm (the pouring head is located at the upper part of the top mold);
[0054] S106, according to the three-dimensional data model of the bottom mold, the outer mold, the core mold, the top mold and the pouring riser, an inkjet printer is used to print, and quartz sand or ceramsite sand is combined by spraying a binder, and stacked layer by layer to form a sand core structure;
[0055] S108, sand-clean the printed bottom mold, outer mold, core mold, top mold and pouring riser, and assemble them from bottom to top after sand-cleaning, wherein the bottom mold is placed first, and then the core mold is installed in the bottom mold, the core mold is first positioned by the bottom mold, and then the outer mold is assembled, the core mold is fixed by the outer mold, and then the top mold and pouring riser are assembled, and the assembly gap between the core mold and the outer mold and the bottom mold is ≤0.5mm.
[0056] S110, burying the assembled sand core structure for piston casting into a sand box, and then pouring the smelted ductile iron QT700-2 metal liquid into the sand core structure through the pouring riser until the pouring riser is filled with the metal liquid, thereby completing the piston casting, wherein the pouring speed of the metal liquid is controlled at 120 kg / min, and the piston casting time is controlled within 25 seconds;
[0057] S112, disassembling the cooled sand core structure to obtain a piston casting.
[0058] The ductile iron piston casting prepared in Example 1 was compared with the ductile iron piston casting prepared by the conventional process. The comparison results are shown in Table 1 below.
[0059] Table 1
[0060] Tensile strength / MPa Hardness HBW Elongation / % Traditional crafts 716 269 2.8 This embodiment 739 285 3.6
[0061] As can be seen from Table 1, the piston casting process proposed in the present invention utilizes a unique sand core structure for piston casting, which not only simplifies the process, saves multiple steps such as placing cold iron, spraying paint, and baking, greatly improves production efficiency, but also casts castings with better performance.
[0062] Example 2
[0063] A piston casting process, using Figure 2 The sand core structure for piston casting and the gray cast iron HT250 metal liquid are shown. Specifically, the following steps are included:
[0064] S202, design the shrinkage coefficient and casting according to the piston product model, and the shrinkage coefficient is 1.05;
[0065] S204, design the bottom mold, outer mold, core mold, top mold and pouring riser of the sand core structure according to the casting, such as Figure 1 As shown, the height of the bottom mold is 95mm, the height of the outer mold is 105mm, the height of the core mold is 210mm, the height of the top mold is 100mm, the height of the pouring and rising gate is 75mm, the inner diameter is 80mm, and the outer diameter is 130mm (the pouring and rising gate is located at the upper part of the top mold);
[0066] S206, according to the three-dimensional data model of the bottom mold, the outer mold, the core mold, the top mold and the pouring riser, an inkjet printer is used to print, and quartz sand or ceramsite sand is combined by spraying a binder, and stacked layer by layer to form a sand core structure;
[0067] S208, sand-clean the printed bottom mold, outer mold, core mold, top mold and pouring riser, and assemble them from bottom to top after sand-cleaning, wherein the bottom mold is placed first, and then the core mold is installed in the bottom mold, the core mold is first positioned by the bottom mold, and then the outer mold is assembled, the core mold is fixed by the outer mold, and then the top mold and pouring riser are assembled, and the assembly gap between the core mold and the outer mold and the bottom mold is ≤0.5mm.
[0068] S210, burying the assembled sand core structure for piston casting into a sand box, and then pouring the smelted gray cast iron HT250 metal liquid into the sand core structure through the pouring riser until the pouring riser is filled with the metal liquid, thereby completing the piston casting, wherein the pouring speed of the metal liquid is controlled at 100 kg / min, and the piston casting time is controlled within 20 seconds;
[0069] S212, disassembling the cooled sand core structure to obtain a piston casting.
[0070] The gray cast iron piston casting prepared in Example 2 was compared with the gray cast iron piston casting prepared by the traditional process. The comparison results are shown in Table 2 below.
[0071] Table 2
[0072] Tensile strength / MPa Hardness HBW Elongation / % Traditional crafts 257 200 0.5 This embodiment 279 210 0.7
[0073] As can be seen from Table 2, the piston casting process proposed in the present invention utilizes a unique sand core structure for piston casting, which not only simplifies the process and saves multiple steps such as placing cold iron, spraying paint, and baking, greatly improving production efficiency, but also the cast castings have better performance.
[0074] Example 3
[0075] A piston casting process, using Figure 3 The sand core structure for piston casting and aluminum alloy ZL109 metal liquid shown in the figure specifically include the following steps:
[0076] S302, design the shrinkage coefficient and casting according to the piston product model, and the shrinkage coefficient is 1;
[0077] S304, design the bottom mold, outer mold, core mold, top mold and pouring riser of the sand core structure according to the casting, such as Figure 1 As shown, the height of the bottom mold is 95mm, the height of the outer mold is 100mm, the height of the core mold is 200, the height of the top mold is 110mm, the height of the pouring and rising gate is 90mm, the inner diameter is 100mm, and the outer diameter is 140mm (the pouring and rising gate is located at the upper part of the top mold);
[0078] S306, according to the three-dimensional data model of the bottom mold, the outer mold, the core mold, the top mold and the pouring riser, an inkjet printer is used to print, and quartz sand or ceramsite sand is combined by spraying a binder, and stacked layer by layer to form a sand core structure;
[0079] S308, sand-clean the printed bottom mold, outer mold, core mold, top mold and pouring riser, and assemble them from bottom to top after sand-cleaning, wherein the bottom mold is placed first, and then the core mold is installed in the bottom mold, the core mold is first positioned by the bottom mold, and then the outer mold is assembled, the core mold is fixed by the outer mold, and then the top mold and pouring riser are assembled, and the assembly gap between the core mold, the outer mold and the bottom mold is ≤0.5mm.
[0080] S310, burying the assembled sand core structure for piston casting into a sand box, and then pouring the smelted aluminum alloy ZL109 metal liquid into the sand core structure through the pouring riser until the pouring riser is filled with the metal liquid, thereby completing the piston casting, wherein the pouring speed of the metal liquid is controlled at 60 kg / min, and the piston casting time is controlled within 40 seconds;
[0081] S312, disassembling the cooled sand core structure to obtain a piston casting.
[0082] The aluminum alloy piston casting prepared in Example 3 was compared with the aluminum alloy piston casting prepared by the traditional process. The comparison results are shown in Table 3 below.
[0083] Table 3
[0084] Tensile strength / MPa Hardness HBW Elongation / % Traditional crafts 216 111 0.6 This embodiment 235 115 0.9
[0085] As can be seen from Table 3, the piston casting process proposed in the present invention utilizes a unique sand core structure for piston casting, which not only simplifies the process, saves multiple steps such as placing cold iron, spraying paint, and baking, greatly improves production efficiency, but also casts castings with better performance.
[0086] In the present invention, the terms "first", "second", and "third" are used for descriptive purposes only and should not be understood as indicating or implying relative importance; the term "plurality" refers to two or more, unless otherwise clearly defined. The terms "installed", "connected", "connected", "fixed", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; "connected" can be a direct connection or an indirect connection through an intermediate medium. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0087] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by terms such as “upper”, “lower”, “left”, “right”, “front” and “back” are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or unit referred to must have a specific direction, be constructed and operated in a specific orientation, and therefore, cannot be understood as a limitation on the present invention.
[0088] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0089] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A sand core structure for piston casting, characterized in that: include: The bottom mold, outer mold, core mold and top mold are arranged in coordination, and the sand core structure as a whole is designed to correspond to the piston top facing upward. The wall thickness of the bottom mold and the outer mold is consistent, and the top mold is located at the geometric center of the sand core structure. The interior of the core mold is a hollow conformal design, wherein the core mold is assembled to the inside of the bottom mold, the outer mold is assembled above the bottom mold, and the top mold is assembled to the top of the outer mold; a pouring riser is arranged above the top mold, and the pouring riser coincides with the central axis of the top mold, and the pouring riser is communicated with the internal cavity of the top mold.
2. The sand core structure for piston casting according to claim 1, characterized in that: The height of the pouring riser is 1 / 5-1 / 3 of the height of the assembled bottom mold, the outer mold and the top mold.
3. The sand core structure for piston casting according to claim 2, characterized in that: The outer diameter of the bottom end of the pouring riser is the same as the internal cavity width of the top mold, and gradually widens from the bottom end to above the top surface of the top mold. The inner diameter of the pouring riser above the top mold is 60-110mm.
4. The sand core structure for piston casting according to any one of claims 1 to 3, characterized in that: The inner shape of the bottom mold, outer mold, core mold and top mold after assembly is the same as the designed casting shape.
5. The sand core structure for piston casting according to claim 4, characterized in that: The pouring riser is assembled on the top mold, and the assembly surface between the two is stepped; Alternatively, the pouring head and the top mold are integrally formed.
6. The sand core structure for piston casting according to claim 5, characterized in that: The assembly surfaces among the structures in the bottom mold, the outer mold, the core mold and the top mold are stepped.
7. A piston casting process using the sand core structure for piston casting according to any one of claims 1 to 6, characterized in that: The following steps are involved: Design shrinkage coefficient and castings according to piston product model; Design the bottom mold, outer mold, core mold, top mold and pouring riser of the sand core structure according to the casting; According to the three-dimensional data model of the bottom mold, outer mold, core mold, top mold and pouring riser, an inkjet printer is used to print, and quartz sand or ceramsite sand is combined by spraying a binder, and stacked layer by layer to form a sand core structure; The printed bottom mold, outer mold, core mold, top mold and pouring riser are sanded and assembled from bottom to top, wherein the bottom mold is placed first, then the core mold is installed into the bottom mold, and then the outer mold, top mold and pouring riser are assembled; The assembled sand core structure for piston casting is buried in the sand box, and then the smelted metal liquid is poured into the sand core structure through the pouring riser until the pouring riser is filled with metal liquid, thus completing the piston casting; The cooled sand core structure is disassembled to obtain a piston casting.
8. The piston casting process of the sand core structure for piston casting according to claim 7, characterized in that: When the smelted metal liquid is poured into the sand core structure through the pouring riser, the pouring speed of the metal liquid is controlled at 60-120kg / min, and the casting time is controlled within 1min; The metal liquid includes but is not limited to ductile iron liquid, gray iron liquid, and aluminum alloy liquid.
9. The piston casting process of the sand core structure for piston casting according to claim 8, characterized in that: The shrinkage coefficient is 0.9-1.
1.
10. The piston casting process of the sand core structure for piston casting according to claim 9, characterized in that: When assembling the sand core structure for piston casting, the core mold is first positioned by the bottom mold and then pressed and fixed by the outer mold; the assembly clearance between the core mold, the outer mold and the bottom mold is ≤0.5mm.