Preparation method of ultra-low carbon steel continuous casting billet, ultra-low carbon steel continuous casting billet and steel product

By adjusting the tundish steel water flow rate and the crystallizer cooling water flow rate, combined with the design of multiple pairs of foot rollers and the optimization of protective slag, the problem of steel penetration of ultra-low carbon steel slabs was solved, the steel penetration defects at the corners were reduced, and the quality of the slabs was improved. quality and production efficiency.

CN118768529AActive Publication Date: 2024-10-15HUNAN VALIN LIANYUAN IRON & STEEL CO LTD

Patent Information

Application Number
CN202410755968.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-15
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

During the continuous casting process, the molten steel flows and solidifies unevenly in the crystallizer, causing the liquid steel to penetrate into the partially solidified shell or inside the cast slab, resulting in the phenomenon of steel penetration in the ultra-low carbon steel cast slab, which is difficult to effectively solve with existing technology. This question.

Method used

By adjusting the flow rate of molten steel in the tundish, the flow rate of the crystallizer cooling water and the taper coefficient of the crystallizer, combined with the design of multiple pairs of foot rollers and the optimization of the alkalinity and melting point of the mold powder, ultra-low carbon steel continuous casting billets were prepared to reduce corner seepage. Steel defects.

Benefits of technology

Significantly reduced steel penetration defects at the corners of ultra-low carbon steel continuous casting billets, improved the apparent quality, reduced the amount of grinding, increased the ratio of hot charging and hot delivery, and improved production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768529A_ABST
    Figure CN118768529A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an ultra-low carbon steel continuous casting billet, the ultra-low carbon steel continuous casting billet and a steel product. The method comprises the steps that tundish molten steel passes through a crystallizer at the speed of 1.4 m / min to 1.6 m / min, crystallizer molten steel is obtained, and the carbon content of the tundish molten steel is smaller than or equal to 0.006%; the crystallizer molten steel is cooled, a continuous casting billet is manufactured, and crystallizer cooling comprises first cooling water in the first direction and second cooling water in the second direction; the flow velocity of the first cooling water is 5600 L / min to 5900 L / min, and the flow velocity of the second cooling water is 570 L / min to 580 L / min; when the width of the ultra-low carbon steel continuous casting billet is 900-1200 mm, the taper coefficient of the crystallizer is 1.2%; when the width of the ultra-low carbon steel continuous casting billet is 1201-1500mm, the taper coefficient of the crystallizer is 1.1%; and when the width of the ultra-low carbon steel continuous casting billet is 1501mm to 1800mm, the taper coefficient of the crystallizer is 1.0%. According to the method, the steel seepage phenomenon of the ultra-low carbon steel continuous casting billet is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of steel plate smelting, and specifically relates to a method for preparing an ultra-low carbon steel continuous casting billet, an ultra-low carbon steel continuous casting billet and a steel product. Background Art

[0002] Continuous casting is a process of directly casting liquid steel into billets. High-efficiency continuous casting has become an economical and reasonable production process in the metallurgical field at home and abroad. The key points of continuous casting include temperature control of molten steel, design and operation of crystallizer, slab casting speed control, secondary cooling, and control of protective slag in the tundish. These processes can effectively improve the quality and production efficiency of the billet.

[0003] The problem of steel infiltration in ultra-low carbon steel ingots refers to the uneven flow and solidification of molten steel in the crystallizer during the continuous casting process, which causes the liquid steel to penetrate into the partially solidified shell or the interior of the ingot, forming defects. In the related art, the solution to the problem of steel infiltration in ultra-low carbon steel ingots generally focuses on the structure and process optimization of the tundish part, but the improvement of the steel infiltration phenomenon in ultra-low carbon steel ingots is limited. Therefore, a new process is urgently needed to further improve the steel infiltration pass rate of ultra-low carbon steel ingots. There is a lack of relevant improvements to the crystallizer. Summary of the invention

[0004] In view of this, the present application provides a method for preparing ultra-low carbon steel continuous casting billets, ultra-low carbon steel continuous casting billets and steel products, aiming to provide a method that can significantly improve the steel infiltration phenomenon of ultra-low carbon steel billets, increase the available amount of ultra-low carbon steel billets, and improve the quality of ultra-low carbon steel.

[0005] In a first aspect, an embodiment of the present application provides a method for preparing an ultra-low carbon steel continuous casting billet, comprising:

[0006] Passing the molten steel in the middle package through the crystallizer at a speed of 1.4-1.6 m / min to obtain a crystallizer molten steel, wherein the carbon content of the molten steel in the middle package is ≤0.006%;

[0007] Cooling the molten steel in the crystallizer to obtain a continuous casting billet, wherein the cooling includes using first cooling water in a first direction and second cooling water in a second direction;

[0008] The flow rate of the first cooling water is 5600L / min to 5900L / min, and the flow rate of the second cooling water is 570L / min to 580L / min;

[0009] When the width of the ultra-low carbon steel continuous casting billet is 900 mm to 1200 mm (the narrowest width is 900 mm), the crystallizer taper coefficient is 1.2%;

[0010] When the width of the ultra-low carbon steel continuous casting billet is 1201 mm to 1500 mm, the crystallizer taper coefficient is 1.1%;

[0011] When the width of the ultra-low carbon steel continuous casting billet is 1501 mm to 1800 mm, the crystallizer taper coefficient is 1.0%.

[0012] According to an embodiment of one aspect of the present application, the molten steel in the middle package is passed through a crystallizer at a speed of 1.5 m / min to obtain a crystallizer molten steel, wherein the carbon content of the molten steel in the middle package is ≤0.006%;

[0013] Cooling the molten steel in the crystallizer to obtain a continuous casting billet, wherein the cooling of the crystallizer includes using first cooling water in a first direction and second cooling water in a second direction;

[0014] The flow rate of the first cooling water is 5900 L / min, and the flow rate of the second cooling water is 580 L / min;

[0015] When the width of the ultra-low carbon steel continuous casting billet is 1200 mm, the mold taper coefficient is 1.2%;

[0016] When the width of the ultra-low carbon steel continuous casting billet is 1500 mm, the crystallizer taper coefficient is 1.1%;

[0017] When the width of the ultra-low carbon steel continuous casting billet is 1800 mm, the crystallizer taper coefficient is 1.0%.

[0018] According to an embodiment of one aspect of the present application, a plurality of pairs of foot rollers are included between the crystallizer and the ultra-low carbon steel continuous casting billet, and the crystallizer includes a crystallizer support roller; the plurality of pairs of foot rollers include a first pair of foot rollers, a second pair of foot rollers, a third pair of foot rollers and a fourth pair of foot rollers in the vertical direction, and the deviation values ​​of the arcs of the first pair of foot rollers, the second pair of foot rollers, the third pair of foot rollers and the fourth pair of foot rollers from the crystallizer support rollers are +0.5mm, +1.0mm, +1.5mm, and +2.0mm, respectively.

[0019] According to an embodiment of one aspect of the present application, the method further includes: making the basicity of the protective slag located on the surface of the molten steel inside the crystallizer 0.98 to 0.9.

[0020] According to an embodiment of one aspect of the present application, the method also includes: making the melting point of the protective slag located on the surface of the molten steel inside the crystallizer 1080°C to 1020°C.

[0021] According to an embodiment of one aspect of the present application, the protective slag includes, in mass percentage, the following: SiO2: 30% to 40%, Al2O3: 2% to 5%, Fe2O3: 0.5% to 1.2%, CaO: 30% to 35%, MgO: 0.5% to 1.85%, R2O: 5% to 12%, F: 5% to 8%, FC: 1% to 3.85% and unavoidable impurities, wherein R2O represents the sum of the masses of K2O and Na2O.

[0022] According to an embodiment of one aspect of the present application, the tundish molten steel includes, in mass percentage, 0.0015% to 0.0025% C, 0.015% to 0.020% P, 0.02% to 0.05% Al, 0.25% to 0.35% Mn, 0.10% to 0.20% Si, 0.010% to 0.015% S, and the remainder is Fe and unavoidable impurities.

[0023] According to an embodiment of one aspect of the present application, the tundish molten steel includes, in mass percentage, 0.0025% to 0.0060% C, 0.015% to 0.020% P, 0.03% to 0.05% Al, 0.20% to 0.30% Mn, 0.15% to 0.25% Si, 0.012% to 0.018% S, and the remainder is Fe and unavoidable impurities.

[0024] In a second aspect, an embodiment of the present application provides an ultra-low carbon steel continuous casting billet, which is produced by the preparation method of the first aspect.

[0025] In a third aspect, an embodiment of the present application provides a steel product obtained by hot rolling and cooling the ultra-low carbon steel continuous casting billet obtained by the preparation method of the first aspect or the ultra-low carbon steel continuous casting billet of the second aspect.

[0026] This application has at least the following beneficial effects:

[0027] The method provided in the present application adopts a specific crystallizer cooling intensity, i.e., the first cooling water flow rate and the second cooling water flow rate, for the molten steel flow rate in the middle package and the drawing speed of the ultra-low carbon steel continuous casting billet during the preparation process of ultra-low carbon steel, and adopts different crystallizer taper coefficients for preparing ultra-low carbon steel casting billets of different thicknesses, which can reduce the steel infiltration defect at the corners of the ultra-low carbon steel continuous casting billet, thereby reducing the scarring problem at the edge of the hot-rolled material. The method provides a new process idea for solving the steel infiltration at the corners of ultra-low carbon steel continuous casting billets, which can improve the apparent quality of ultra-low carbon steel continuous casting billets, reduce the amount of grinding of continuous casting billets off the line, increase the proportion of hot charging and hot delivery, reduce the overall cost, and improve production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solution of the implementation regulations of this application, the following is a brief introduction to the drawings required for use in the embodiments of this application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0029] Figure 1 The figure shows the appearance of the steel infiltration at the corner of the ultra-low carbon steel ingot of the comparative example of the present application.

[0030] Figure 2A micrograph of steel infiltration at the corner of an ultra-low carbon steel ingot of a comparative example of the present application is shown.

[0031] Figure 3 A schematic diagram of the structure of the middle ladle and the crystallizer in an embodiment of the present application is shown.

[0032] Figure 4 A schematic diagram showing the relative positions of the arcs of the crystallizer and the crystallizer support rollers in an embodiment of the present application is shown.

[0033] Among them, 1. intermediate ladle, 2. crystallizer, 3. crystallizer intermediate roller. DETAILED DESCRIPTION

[0034] In order to make the application purpose, technical solution and beneficial technical effect of this application clearer, the application is further described in detail below in conjunction with the embodiments. It should be understood that the implementation regulations described in this specification are only for explaining this application, not for limiting this application.

[0035] For simplicity, the present application only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unclearly recorded range; and any lower limit can be combined with other lower limits to form an unclearly recorded range, and any upper limit can be combined with any other upper limit to form an unclearly recorded range. In addition, although not clearly recorded, each point or single value between the range endpoints is included in the range. Thus, each point or single value can be combined with any other point or single value as its own lower limit or upper limit or with other lower limits or upper limits to form an unclearly recorded range.

[0036] In the description of the present application, it should be noted that, unless otherwise specified, “above” and “below” are inclusive of the number, and the “multiple” in “one or more” means two or more than two.

[0037] The above application content of the present application is not intended to describe each disclosed embodiment or each implementation in the present application. The following description more specifically illustrates exemplary embodiments. In many places throughout the application, guidance is provided through a series of embodiments, and these implementation regulations can be used in various combinations. In each example, enumeration is only used as a representative group and should not be interpreted as exhaustive.

[0038] Preparation method of ultra-low carbon steel continuous casting billet

[0039] In a first aspect, an embodiment of the present application provides a method for preparing an ultra-low carbon steel continuous casting billet, comprising:

[0040] Passing the molten steel in the middle package through the crystallizer at a speed of 1.4-1.6 m / min to obtain a crystallizer molten steel, wherein the carbon content of the molten steel in the middle package is ≤0.006%;

[0041] Cooling the molten steel in the crystallizer to obtain a continuous casting billet, wherein the cooling includes using first cooling water in a first direction and second cooling water in a second direction;

[0042] The flow rate of the first cooling water is 5600L / min to 5900L / min, and the flow rate of the second cooling water is 570L / min to 580L / min;

[0043] When the width of the ultra-low carbon steel continuous casting billet is 900 mm to 1200 mm (the narrowest width is 900 mm), the crystallizer taper coefficient is 1.2%;

[0044] When the width of the ultra-low carbon steel continuous casting billet is 1201 mm to 1500 mm, the crystallizer taper coefficient is 1.1%;

[0045] When the width of the ultra-low carbon steel continuous casting billet is 1501 mm to 1800 mm, the crystallizer taper coefficient is 1.0%.

[0046] According to the embodiments of the present application, the carbon content of the molten steel in the middle package is ≤0.006%, indicating that this type of molten steel used to prepare ultra-low carbon steel has the characteristics of fast billet drawing speed and thin solidified billet shell. Therefore, when the molten steel in the middle package passes through the crystallizer at a speed of 1.4 to 1.6 m / min and the drawing speed of the ultra-low carbon steel continuous casting billet is 1.4 m / min to 1.6 m / min, the flow rate of the first cooling water and the flow rate of the second cooling water are within the above range, which can reduce the uneven flow and solidification of the molten steel in the crystallizer, resulting in the liquid molten steel penetrating into the partially solidified shell or the interior of the billet to form defects.

[0047] The first direction can be understood as the direction of the wide surface of the crystallizer acted by the cooling water or the direction of the length direction in the top view of the crystallizer acted by the cooling water. The second direction can be understood as the direction of the narrow surface of the crystallizer acted by the cooling water or the direction of the width direction in the top view of the crystallizer acted by the cooling water. The flow rate of the first cooling water and the flow rate of the second cooling water within the above range can further increase the shrinkage of the solidified shell of the molten steel, especially the shrinkage of the initial solidified shell in the meniscus region.

[0048] The mold taper coefficient refers to the shrinkage rate of the mold in the height direction. The thickness of the ultra-low carbon steel continuous casting billet refers to the cross-sectional width of the billet in the crystallizer, referred to as the cross-sectional width.

[0049] Furthermore, the use of a specific taper coefficient can effectively compensate for the volume shrinkage of a specific thickness of ultra-low carbon steel continuous casting billet during solidification, so that the billet of this thickness maintains good contact with the wall of the crystallizer, reduces the gap, and prevents molten steel from penetrating. Too large or too small a taper coefficient will affect the formation of the shell. Too large a taper may cause the shell to be too thick and increase internal stress, while too small a taper may cause the shell to be too thin and insufficient in strength, all of which will increase the risk of penetration.

[0050] The mold taper coefficient takes into account the situation that different molds are used to cast different billet widths. The above design is more in line with the shrinkage characteristics of the continuous casting billet at the lower mouth of the crystallizer, which is beneficial to reducing the steel infiltration phenomenon of ultra-low carbon steel continuous casting billets and improving the hot charging and delivery ratio.

[0051] Ultra-low carbon steel continuous casting billets with quality defects need to be ground offline. The billets on the production line are about 500-900 degrees Celsius. The billets need to be cooled to room temperature for grinding. The infiltrated steel is burned off with a high-temperature torch and then heated again to allow the billets to enter the continuous production line. The normal temperature of the next process of the billet is 400 to 600 degrees. Only after grinding can the billets be rolled in the subsequent production. Slabs without defects do not need to be ground offline, but are directly sent to the next process for production after production. The hot charging ratio measures the proportion of billets that do not need to be ground offline.

[0052] In some optional embodiments, the molten steel in the middle package is passed through the crystallizer at a speed of 1.5 m / min to obtain a crystallizer molten steel, wherein the carbon content of the molten steel in the middle package is ≤0.006%;

[0053] Cooling the molten steel in the crystallizer to obtain a continuous casting billet, wherein the cooling of the crystallizer includes using first cooling water in a first direction and second cooling water in a second direction;

[0054] The flow rate of the first cooling water is 5900 L / min, and the flow rate of the second cooling water is 580 L / min;

[0055] When the width of the ultra-low carbon steel continuous casting billet is 1200 mm, the mold taper coefficient is 1.2%;

[0056] When the width of the ultra-low carbon steel continuous casting billet is 1500 mm, the crystallizer taper coefficient is 1.1%;

[0057] When the width of the ultra-low carbon steel continuous casting billet is 1800 mm, the crystallizer taper coefficient is 1.0%.

[0058] In some optional embodiments, a plurality of pairs of foot rollers are included between the crystallizer and the low-carbon steel continuous casting billet, and the crystallizer includes a crystallizer support roller; the plurality of pairs of foot rollers include a first pair of foot rollers, a second pair of foot rollers, a third pair of foot rollers and a fourth pair of foot rollers in the vertical direction, and the deviation values ​​of the arcs of the first pair of foot rollers, the second pair of foot rollers, the third pair of foot rollers and the fourth pair of foot rollers from the crystallizer support rollers are respectively +0.5 mm,

[0059] +1.0mm, +1.5mm, +2.0mm.

[0060] like Figure 3As shown, a schematic diagram of the positions of the tundish steel ladle 1, the crystallizer 2 and the crystallizer support rollers 3 is shown.

[0061] Figure 4 In the figure, the left figure shows the first pair of foot rollers, the second pair of foot rollers, the third pair of foot rollers and the fourth pair of foot rollers, and the arcs of the first pair of foot rollers, the second pair of foot rollers, the third pair of foot rollers and the fourth pair of foot rollers are at original relative distances from the crystallizer support rollers. The right figure shows the first pair of foot rollers, the second pair of foot rollers, the third pair of foot rollers and the fourth pair of foot rollers, and the deviation values ​​of the arcs of the first pair of foot rollers, the second pair of foot rollers, the third pair of foot rollers and the fourth pair of foot rollers are d1: +0.5mm, d2: +1.0mm, d3: +1.5mm, d4: +2.0mm respectively.

[0062] Generally speaking, the first pair of foot rollers is located below the crystallizer, which plays an effective support and reduces bulging. The distance between the first pair of foot rollers and the lower opening of the crystallizer support roller is 240mm. In this application, the deviation value between the first pair of foot rollers and the crystallizer support roller is +0.5mm. Such a deviation value setting has the advantage of effective support and avoids the problem of bulging.

[0063] The second pair of foot rollers is located below the crystallizer and below the first pair of foot rollers, which can effectively support and reduce bulging. The distance between the second pair of foot rollers and the lower mouth of the crystallizer support roller is 480mm. In this application, the deviation value between the second pair of foot rollers and the crystallizer support roller is +1.0mm. Such a deviation value setting has the advantage of effective support and avoids the problem of bulging.

[0064] The third pair of foot rollers is located below the crystallizer and below the second pair of foot rollers, which can play a supporting role. The distance between the third pair of foot rollers and the lower opening of the crystallizer support rollers is 720mm. In this application, the deviation value between the third pair of foot rollers and the crystallizer support rollers is +1.5mm. Such a deviation value setting has an effective support advantage and avoids the problem of bulging.

[0065] The fourth pair of foot rollers is located below the crystallizer and below the third pair of foot rollers, which can effectively support and reduce bulging. The distance between the fourth pair of foot rollers and the lower mouth of the crystallizer support roller is 960mm. In this application, the deviation value between the fourth pair of foot rollers and the crystallizer support roller is +2.0mm. Such a deviation value setting has the advantage of effective support and avoids the problem of bulging.

[0066] The first pair of foot rollers, the second pair of foot rollers, the third pair of foot rollers and the fourth pair of foot rollers are respectively located in the second direction, or width direction, of the crystallizer, referred to as the narrow side. Zero deviation or negative deviation will lead to insufficient support force of the solidified billet shell on the narrow side of the crystallizer, increase the probability of steel infiltration, and thus may lead to the spread of steel infiltration in the billet, and fail to effectively control the steel infiltration phenomenon.

[0067] In some optional embodiments, the method further comprises:

[0068] The basicity of the protective slag located on the surface of the molten steel inside the crystallizer is 0.98 to 0.9.

[0069] According to the embodiment of the present application, SiO2 material can be added to reduce the CaO content, so that the basicity of the protective slag is 0.98 to 0.9.

[0070] According to the embodiments of the present application, the basicity of the protective slag is within the above range, which is beneficial to reducing the oxygen content in the molten steel and forming a good deoxidation environment, thereby helping to reduce the carbon content in the molten steel. High oxygen content easily causes carbon in the molten steel to react with oxygen to generate CO gas, increasing the activity of carbon. The basicity of the protective slag is within the above range, indicating that the chemical properties of the protective slag are relatively stable, and it can effectively isolate oxygen and moisture in the air, reduce the penetration of oxygen and moisture into the molten steel, and thus reduce the carbon content in the molten steel. The basicity of the protective slag is within the above range, indicating that the protective slag has good lubrication properties, can effectively reduce the friction between the molten steel and the wall of the crystallizer, avoid local high temperatures caused by frictional heat, and reduce the diffusion of carbon in the molten steel, thereby reducing the occurrence of steel infiltration in the ingot.

[0071] In some optional embodiments, the method further comprises:

[0072] The melting point of the protective slag located on the surface of the molten steel inside the crystallizer is 1080℃ to 1020℃.

[0073] According to an embodiment of the present application, SiO2 material can be used to reduce the CaO content, so that the basicity of the protective slag is 0.98 to 0.9.

[0074] According to the embodiment of the present application, the temperature of the molten steel inside the crystallizer is 1545°C to 1560°C. The temperature of the molten steel differs from the temperature of the protective slag by 450°C. This indicates that the melting point of the protective slag is relatively low. When the melting point of the protective slag is within the above range, it can be melted faster in the crystallizer to form a liquid covering layer. The protective slag has good lubricity and reactivity, and is convenient for absorbing oxygen and impurities in the molten steel. The good fluidity and coverage can effectively isolate the oxygen and moisture in the air, reduce the external carbon source from entering the molten steel, and thus reduce the steel infiltration phenomenon. If the melting point is higher than the above range, the protective slag is not easy to melt in the crystallizer, has poor fluidity, and poor coverage. It is easy to form uneven coverage or partially exposed areas, making it easier for oxygen and moisture in the air to penetrate into the molten steel, increasing the risk of steel infiltration.

[0075] In summary, the basicity and melting point of the mold slag are beneficial to the solidification of the solidified shell in the second direction and reduce the risk of steel infiltration. Higher basicity and melting point are not conducive to the solidification of the solidified shell on the narrow side.

[0076] In some optional embodiments, the protective slag includes, in mass percentage, the following: SiO2: 30% to 40%, Al2O3: 2% to 5%, Fe2O3: 0.5% to 1.2%, CaO: 30% to 35%, MgO: 0.5% to 1.85%, R2O: 5% to 12%, F: 5% to 8%, FC: 1% to 3.85% and unavoidable impurities, wherein R2O represents the sum of the masses of K2O and Na2O.

[0077] In some optional embodiments, the protective slag includes, by mass percentage, the following: SiO2: 33.1%, Al2O3: 3.95%, Fe2O3: 0.98%, CaO: 32.47%, MgO: 1.78%, R2O: 5%-12%, F: 5%-8%, FC: 1%-3.85% and unavoidable impurities.

[0078] In some optional embodiments, the tundish molten steel comprises, by mass percentage, 0.0015% to 0.0025% C, 0.015% to 0.020% P, 0.02% to 0.05% Al, 0.25% to 0.35% Mn, 0.10% to 0.20% Si, 0.010% to 0.015% S, and the remainder is Fe and unavoidable impurities.

[0079] In some optional embodiments, the tundish molten steel comprises, by mass percentage, 0.0025% to 0.0060% C, 0.015% to 0.020% P, 0.03% to 0.05% Al, 0.20% to 0.30% Mn, 0.15% to 0.25% Si, 0.012% to 0.018% S, and the remainder is Fe and unavoidable impurities.

[0080] In a second aspect, an embodiment of the present application provides an ultra-low carbon steel continuous casting billet, which is produced by the preparation method of the first aspect.

[0081] Ultra-low carbon steel ingots naturally have high toughness and ductility due to their ultra-low carbon content. Reducing carburization of corners makes the mechanical properties of the entire ingot more uniform, thereby improving the toughness and ductility of ultra-low carbon steel ingots. Reducing carburization of corners of ultra-low carbon steel ingots is beneficial to improving the utilization rate of ingots, reducing the amount of cutting at the edges, and improving the processing performance and economic benefits of products.

[0082] In some optional embodiments, the grinding amount of the ultra-low carbon steel continuous casting billet is ≤0.5%.

[0083] Grinding amount = grinding quality of ultra-low carbon steel continuous casting billet corner cutting / sample quality of ultra-low carbon steel continuous casting billet in the length direction

[0084] In a third aspect, an embodiment of the present application provides a steel product obtained by hot rolling and cooling the ultra-low carbon steel continuous casting billet obtained by the preparation method of the first aspect or the ultra-low carbon steel continuous casting billet of the second aspect.

[0085] By removing the infiltrated part at the edge of the ultra-low carbon steel ingot, it is beneficial to produce a steel product with no scarring at the edge. The scarring phenomenon of steel products is a kind of surface defect, usually manifested as raised or sunken carbide accumulation on the surface. These defects will significantly affect the mechanical properties, processing performance and service life of ultra-low carbon steel.

[0086] Example

[0087] The following examples describe the disclosure of the present application in more detail, and these examples are intended for illustrative purposes only, as it will be apparent to those skilled in the art that various modifications and variations may be made within the scope of the disclosure of the present application. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0088] Example 1

[0089] This embodiment provides a method for preparing an ultra-low carbon steel ingot, comprising the following steps:

[0090] The molten steel in the tundish includes, by mass percentage: 0.0015% to 0.0025% C, 0.015% to 0.020% P, 0.02% to 0.05% Al, 0.25% to 0.35% Mn, 0.10% to 0.20% Si, 0.010% to 0.015% S, and the balance is Fe and unavoidable impurities.

[0091] The molten steel in the middle package passes through the crystallizer at a speed of 1.5m / min to obtain the crystallizer molten steel, wherein the carbon content of the molten steel in the middle package is ≤0.0060%; the drawing speed of the ultra-low carbon steel continuous casting billet is 1.5m / min,

[0092] Cooling the molten steel in the crystallizer to obtain a continuous casting billet, wherein the cooling includes using first cooling water in a first direction and second cooling water in a second direction;

[0093] The water volume on the wide surface of the crystallizer is 5900L / min, and the water volume on the narrow surface is 580L / min.

[0094] The thickness of the ultra-low carbon steel ingot is 1200 mm, and the taper coefficient is set to 1.2% to ensure that the narrow surface roller supports the solidified ingot shell.

[0095] The deviation values ​​between the narrow side foot rollers of the crystallizer and the copper plate of the crystallizer are: +0.5mm for the first pair of foot rollers, +1.0mm for the second pair of foot rollers, +1.5mm for the third pair of foot rollers and +2.0mm for the fourth pair of foot rollers (+ indicates positive deviation).

[0096] The basicity of the low carbon steel protection slag on the surface of the molten steel in the crystallizer is 0.9 and the melting point is 1020℃.

[0097] Example 2

[0098] The difference between this embodiment and embodiment 1 is that the width of the low carbon steel ingot is 1500 mm and the taper coefficient is set to 1.1%.

[0099] Example 3

[0100] The difference between this embodiment and embodiment 1 is that the width of the low carbon steel ingot is 1800 mm, and the taper coefficient is set to 1.0%.

[0101] Example 4

[0102] The difference between this embodiment and Embodiment 1 is that the deviation values ​​between the narrow surface foot rollers of the crystallizer and the copper plate of the crystallizer are changed from 0mm for the first pair of foot rollers, 0mm for the second pair of foot rollers, 0mm for the third pair of foot rollers and 0mm for the fourth pair of foot rollers.

[0103] Example 5

[0104] The difference between this embodiment and embodiment 1 is that the molten steel in the tundish includes, by mass percentage, 0.0025% to 0.0060% C, 0.015% to 0.020% P, 0.03% to 0.05% Al, 0.20% to 0.30% Mn, 0.15% to 0.25% Si, 0.012% to 0.018% S, and the balance is Fe and unavoidable impurities. The ultra-low carbon steel protection slag on the surface of the molten steel in the crystallizer has a basicity of 0.98 and a melting point of 1080°C.

[0105] Comparative Example 1

[0106] The difference between this comparative example and Example 1 is that the water volume on the wide side of the crystallizer is 5344 L / min, and the water volume on the narrow side is 550 L / min. Figure 1 The micrograph of the steel infiltration at the edge of the ingot of Comparative Example 1 is shown in FIG. Figure 2 shown.

[0107] Comparative Example 2

[0108] The difference between this comparative example and Example 1 is that the molten steel in the tundish passes through the crystallizer at a speed of 1.8 m / min.

[0109] Comparative Example 3

[0110] The difference between this comparative example and Example 1 is that the width of the ultra-low carbon steel ingot is 1200 mm, and the taper coefficient is set to 0.8%.

[0111] Comparative Example 4

[0112] The difference between this comparative example and Example 2 is that the difference between this comparative example and Example 1 is that the water volume on the wide surface of the crystallizer is 5344 L / min, and the water volume on the narrow surface is 550 L / min.

[0113] Comparative Example 5

[0114] The difference between this comparative example and Example 3 is that the difference between this comparative example and Example 1 is that the water volume on the wide surface of the crystallizer is 5344 L / min, and the water volume on the narrow surface is 550 L / min.

[0115] Test Section

[0116] The edge infiltration width of the ultra-low carbon steel ingots prepared in the examples and comparative examples was tested, as well as the grinding amount and the hot charging and hot delivery ratio.

[0117] Grinding amount = (mass of the ingot before grinding - mass after decarburization by flame) / mass of the ingot before grinding

[0118] The hot charging and hot delivery ratio refers to the proportion of the number of ingots that do not need to be trimmed to the total number of ingots.

[0119] Table 1 Test results of ultra-low carbon steel ingots of Examples and Comparative Examples.

[0120]

[0121]

[0122] The above measured performance parameters are taken as average values.

[0123] The above are only specific implementations of the present application, but the protection scope of the present application is not limited thereto, and any familiarity with the present technology or replacement should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing an ultra-low carbon steel continuous casting billet, characterized in that: include: Passing the molten steel in the middle package through the crystallizer at a speed of 1.4-1.6 m / min to obtain a crystallizer molten steel, wherein the carbon content of the molten steel in the middle package is ≤0.006%; Cooling the molten steel in the crystallizer to obtain a continuous casting billet, wherein the cooling of the crystallizer includes using first cooling water in a first direction and second cooling water in a second direction; The flow rate of the first cooling water is 5600L / min to 5900L / min, and the flow rate of the second cooling water is 570L / min to 580L / min; When the width of the ultra-low carbon steel continuous casting billet is 900 mm to 1200 mm, the mold taper coefficient is 1.2%; When the width of the ultra-low carbon steel continuous casting billet is 1201 mm to 1500 mm, the crystallizer taper coefficient is 1.1%; When the width of the ultra-low carbon steel continuous casting billet is 1501 mm to 1800 mm, the crystallizer taper coefficient is 1.0%.

2. The preparation method according to claim 1, characterized in that: Passing the molten steel in the middle package through the crystallizer at a speed of 1.5 m / min to obtain a crystallizer molten steel, wherein the carbon content of the molten steel in the middle package is ≤0.006%; Cooling the molten steel in the crystallizer to obtain a continuous casting billet, wherein the cooling of the crystallizer includes using first cooling water in a first direction and second cooling water in a second direction; The flow rate of the first cooling water is 5900 L / min, and the flow rate of the second cooling water is 580 L / min; When the width of the ultra-low carbon steel continuous casting billet is 1200 mm, the crystallizer taper coefficient is 1.2%; When the width of the ultra-low carbon steel continuous casting billet is 1500 mm, the crystallizer taper coefficient is 1.1%; When the width of the ultra-low carbon steel continuous casting billet is 1800 mm, the crystallizer taper coefficient is 1.0%.

3. The preparation method according to claim 1, characterized in that: There are multiple pairs of foot rollers between the crystallizer and the ultra-low carbon steel continuous casting billet, and the crystallizer includes crystallizer support rollers; the multiple pairs of foot rollers include a first pair of foot rollers, a second pair of foot rollers, a third pair of foot rollers and a fourth pair of foot rollers in the vertical direction, and the deviation values ​​of the arcs of the first pair of foot rollers, the second pair of foot rollers, the third pair of foot rollers and the fourth pair of foot rollers from the crystallizer support rollers are +0.5mm, +1.0mm, +1.5mm, and +2.0mm respectively.

4. The preparation method according to claim 1, characterized in that: The method further comprises: making the basicity of the protective slag located on the surface of the molten steel inside the crystallizer be 0.98 to 0.

9.

5. The preparation method according to claim 1, characterized in that: The method further comprises: making the melting point of the protective slag located on the surface of the molten steel inside the crystallizer be 1080°C to 1020°C.

6. The preparation method according to claim 1, characterized in that: The protective slag includes, by mass percentage: SiO2: 30% to 40%, Al2O3: 2% to 5%, Fe2O3: 0.5% to 1.2%, CaO: 30% to 35%, MgO: 0.5% to 1.85%, R2O: 5% to 12%, F: 5% to 8%, FC: 1% to 3.85% and unavoidable impurities, wherein R2O represents the sum of the masses of K2O and Na2O.

7. The preparation method according to claim 1, characterized in that: The tundish molten steel comprises, by mass percentage, 0.0015% to 0.0025% C, 0.015% to 0.020% P, 0.02% to 0.05% Al, 0.25% to 0.35% Mn, 0.10% to 0.20% Si, 0.010% to 0.015% S, and the remainder is Fe and inevitable impurities.

8. The preparation method according to claim 1, characterized in that: The tundish molten steel comprises, by mass percentage, 0.0025% to 0.0060% C, 0.015% to 0.020% P, 0.03% to 0.05% Al, 0.20% to 0.30% Mn, 0.15% to 0.25% Si, 0.012% to 0.018% S, and the remainder is Fe and inevitable impurities.

9. An ultra-low carbon steel continuous casting billet, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 8.

10. A steel product, characterized in that The ultra-low carbon steel continuous casting billet is obtained by hot rolling and cooling the ultra-low carbon steel continuous casting billet obtained by the preparation method according to any one of claims 1 to 8 or the ultra-low carbon steel continuous casting billet according to claim 9.

Citation Information

Patent Citations

  • Preparation method of ultra-low carbon steel and ultra-low carbon steel plate

    CN101956131A

  • Method, device and equipment for controlling belly bulging amount of low-carbon steel and medium

    CN116140577A

  • Production method of low-carbon small square billet

    CN116652129A

  • Method for preventing pin hole defect in extra low carbon steel

    JP1995246448A

  • Slab continuous casting method

    JP2005177841A

Cited By

  • Preparation method of electrical steel and electrical steel

    CN119328095A

  • Method for preparing electrical steel and electrical steel

    CN119328095B