Production method of surface-defect-free low-alloy high-strength steel

By controlling the casting temperature and heating speed, combined with air cooling and slow cooling, the problem of subcutaneous defects and thermal stress cracks in the production of low-alloy high-strength steel is solved, and the production of low-alloy high-strength steel with no surface defects is achieved. , improving the surface quality and qualification rate of rolled products.

CN118768534APending Publication Date: 2024-10-15SHIGANG JINGCHENG EQUIP TECH CO LTD +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410863645.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-29
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Low-alloy high-strength steel is prone to subcutaneous defects and thermal stress cracks in cast slabs during the production process, which affects the surface quality and rolling product qualification rate.

Method used

The production process of converter/electric furnace-LF-VD/RH-continuous casting-hot feeding-rolling-slow cooling is adopted to control the casting temperature, heating speed and temperature difference, and reduce the precipitation of NbC through crystallizer stirring and secondary cooling stirring. , using air cooling and slow cooling to reduce thermal stress.

Benefits of technology

It achieves the production of low-alloy high-strength steel with no surface defects, reduces the occurrence of internal and surface cracks in the cast slab, and improves the surface quality and qualification rate of rolled products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768534A_ABST
    Figure CN118768534A_ABST
Patent Text Reader

Abstract

The invention discloses a production method of surface-defect-free low-alloy high-strength steel. The production process comprises the steps of converter / electric furnace LF-VD / RH-continuous casting, hot delivery, rolling and slow cooling. Wherein in the continuous casting process, crystallizer stirring, secondary cooling stirring and tail end stirring are adopted, the electric stirring current is 100-150 A, the electric stirring frequency is 5.0-6.0 HZ, the inlet withdrawal and straightening temperature is 1000-1100 DEG C, and the outlet withdrawal and straightening temperature is 900-1000 DEG C; and after the casting blank is pulled out and straightened, air cooling is conducted, and hot feeding steel rolling is conducted when the temperature of a cooling bed is 600-700 DEG C. The low-alloy high-strength steel provided by the invention has good surface quality, and magnetic flux leakage flaw detection is less than or equal to 0.3 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel production, and in particular relates to a method for producing surface defect-free low-alloy high-strength steel. Background Art

[0002] Low alloy high strength steel is a peritectic steel. When the molten steel solidifies, the volume shrinks, and an air gap is generated between the billet shell and the crystallizer, which affects heat conduction. Under the action of thermal stress and structural stress, subcutaneous defects of the ingot are generated, which are inherited to the surface of the rolled material during the subsequent rolling process; or the heating speed is too fast, which reduces the qualified rate of the rolled material, affects the surface quality and increases the scrap rate. In the existing technology, there is no method that can effectively solve the above technical problems of low alloy high strength steel.

[0003] In the production process of low alloy high strength steel, generally after VD is completed, a lower hanging ladle temperature is used and low superheat is controlled. Low superheat pouring can improve the internal quality of the original casting, but the temperature entering the straightening machine is too low, resulting in straightening cracks, such as Figure 1 As shown, NbC precipitates at the grain boundaries, weakening the grain boundaries.

[0004] In addition, low-alloy high-strength steel continuous casting billets are produced by the stack cooling method. When the continuous casting billets are stack cooled, stress cracks are prone to occur in the billets. When reheated, the temperature difference between the inside and outside is large, which easily generates thermal stress. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a method for producing surface defect-free low-alloy high-strength steel, and the technical solution thereof is as follows: A method for producing surface defect-free low-alloy high-strength steel, the production process of which includes: converter / electric furnace-LF-VD / RH-continuous casting-hot delivery-rolling-slow cooling.

[0006] Preferably, in the method for producing surface defect-free low-alloy high-strength steel described in the present invention, in the continuous casting process, the depth of the middle water inlet is 90-100 mm, the continuous casting speed is controlled at 0.24-0.28 m / min, the water volume of the crystallizer is 4200-4500 L / min, and the secondary cooling water volume is 0.11-0.17 L / kg.

[0007] Preferably, in the method for producing surface defect-free low-alloy high-strength steel described in the present invention, the continuous casting process adopts crystallizer stirring, secondary cooling stirring and end stirring, the electric stirring current is 100-150A, the electric stirring frequency is 5.0-6.0HZ, the entry drawing and straightening temperature is 1000-1100℃, and the exit drawing and straightening temperature is 900-1000℃.

[0008] Preferably, in the method for producing surface defect-free low-alloy high-strength steel of the present invention, in the hot delivery step, the ingot is air-cooled after being drawn and straightened to a cooling bed temperature of 600-700°C, and then hot-delivered to be rolled steel.

[0009] Preferably, in the method for producing surface defect-free low-alloy high-strength steel described in the present invention, in the rolling process, the ingot is heated in a heating furnace, the temperature of the preheating section is controlled at 800-900°C, the temperature of zone 1 is controlled at 850-950°C, the temperature of zone 3 is controlled at 900-1050°C, the temperature of zone 5 is controlled at 1000-1180°C, the temperature of zone 7 is controlled at 1170-1250°C, and the temperature of zones 9-15 is controlled at 1240-1250°C, and the total heating time is 6-7h.

[0010] Preferably, in the method for producing surface defect-free low-alloy high-strength steel of the present invention, in the rolling process, the blanking speed is controlled at 1.2-1.5 m / s, and the blanking temperature is 1050-1150°C.

[0011] Preferably, in the method for producing surface defect-free low-alloy high-strength steel of the present invention, in the rolling process, the starting rolling temperature is 930-980°C, and the round steel is slowly cooled in the pit.

[0012] Furthermore, the composition range of the low alloy high strength steel of the present invention is: C≤0.22%, Si≤0.50%, Mn: 0.95-1.65%, S≤0.010%, P≤0.015%, Cr≤0.30%, Nb: 0.020-0.030%.

[0013] Furthermore, the low alloy high strength steel of the present invention has a specification of Ф120-200mm.

[0014] The inventive principle and beneficial technical effects of the technical solution of the present invention are: (1) The present invention controls the temperature of the ingot to be 900-1000°C, and performs blast cooling after the ingot is taken out of the straightening machine. Generally, the precipitation temperature of NbC is 900-1100°C. Rapid cooling after the straightening can reduce the precipitation of NbC at the grain boundaries.

[0015] (2) The ingot casting of the present invention is not pile-cooled, but is produced by hot delivery, which reduces the temperature difference in the preheating section and reduces cracks caused by thermal stress.

[0016] (3) The present invention controls the temperature of the preheating section of the heating furnace to 800-900°C, thereby reducing the temperature difference between the ingot temperature and the furnace temperature and reducing the generation of thermal stress cracks inside the ingot.

[0017] (4) The low-alloy high-strength steel provided by the present invention has good surface quality. The surface quality meets the requirement of ≤0.3 mm after magnetic flux leakage flaw detection. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is the crack morphology of low alloy high strength steel in the existing technology.

[0019] Figure 2 This is the surface morphology of the low alloy high strength steel in Example 1 of the present invention. DETAILED DESCRIPTION

[0020] The technical solution of the present invention is further described in detail below through specific embodiments. Example 1

[0021] The chemical composition content of the low alloy high strength steel of this embodiment is shown in Table 1; its smelting production process includes: converter / electric furnace-LF-VD / RH-continuous casting-hot delivery-rolling-slow cooling; wherein the key process parameters are controlled as follows: (1) Continuous casting and hot delivery process: The depth of the tundish water inlet is 98 mm, the continuous casting speed is controlled at 0.26 m / min, the water volume of the crystallizer is 4500 L / min, and the secondary cooling water volume is 0.17 L / kg; crystallizer stirring, secondary cooling stirring and end stirring are adopted, the electric stirring current is 100 A, the electric stirring frequency is 5.5 Hz, the inlet straightening temperature is 1050 °C, the outlet straightening temperature is 940 °C, the outlet straightening temperature is air-cooled after straightening, the temperature of the cooling bed is 630 °C, and the ingot is hot-sent to steel rolling.

[0022] (2) Rolling process: The heating temperature is shown in Table 2, and the total heating time is 6.3 h. The billet opening speed after leaving the furnace is controlled at 1.3 m / s, and the billet opening temperature is 1080 °C. The rolling temperature is 940 °C, and the round steel is slowly cooled in the pit. Example 2

[0023] The chemical composition content of the low alloy high strength steel of this embodiment is shown in Table 1; its smelting production process includes: converter / electric furnace-LF-VD / RH-continuous casting-hot delivery-rolling-slow cooling; wherein the key process parameters are controlled as follows: (1) Continuous casting and hot delivery process: The depth of the tundish water inlet is 90 mm, the continuous casting speed is controlled at 0.25 m / min, the water volume of the crystallizer is 4300 L / min, the water volume of the secondary cooling is 0.14 L / kg, the crystallizer stirring, secondary cooling stirring and end stirring are adopted, the electric stirring current is 130 A, the electric stirring frequency is 5.8 Hz, the inlet straightening temperature is 1080 °C, the outlet straightening temperature is 980 °C, the outlet straightening temperature is air-cooled, the temperature of the cooling bed is 600 °C, and the ingot is hot-sent to steel rolling.

[0024] (2) Rolling process: The heating temperature is shown in Table 2, and the total heating time is 6.8 h. The billet opening speed after leaving the furnace is controlled at 1.2 m / s, and the billet opening temperature is 1150 °C. The rolling temperature is 930 °C, and the round steel is slowly cooled in the pit. Example 3

[0025] The chemical composition content of the low alloy high strength steel of this embodiment is shown in Table 1; its smelting production process includes: converter / electric furnace-LF-VD / RH-continuous casting-hot delivery-rolling-slow cooling; wherein the key process parameters are controlled as follows: (1) Continuous casting and hot delivery process: The depth of the tundish water inlet is 95 mm, the continuous casting speed is controlled at 0.24 m / min, the water volume of the crystallizer is 4200 L / min, the water volume of the secondary cooling is 0.15 L / kg, the crystallizer stirring, secondary cooling stirring and end stirring are adopted, the electric stirring current is 110 A, the electric stirring frequency is 5.0 Hz, the inlet straightening temperature is 1000 °C, the outlet straightening temperature is 900 °C, the outlet straightening temperature is air-cooled, the temperature of the cooling bed is 700 °C, and the ingot is hot-sent to steel rolling.

[0026] (2) Rolling process: The heating temperature is shown in Table 2, and the total heating time is 6 h. The billet opening speed after leaving the furnace is controlled at 1.5 m / s, and the billet opening temperature is 1070 °C. The rolling temperature is 980 °C, and the round steel is slowly cooled in the pit. Example 4

[0027] The chemical composition content of the low alloy high strength steel of this embodiment is shown in Table 1; its smelting production process includes: converter / electric furnace-LF-VD / RH-continuous casting-hot delivery-rolling-slow cooling; wherein the key process parameters are controlled as follows: (1) Continuous casting and hot delivery process: The depth of the tundish water inlet is 100 mm, the continuous casting speed is controlled at 0.28 m / min, the water volume of the crystallizer is 4400 L / min, the water volume of the secondary cooling is 0.16 L / kg, the crystallizer stirring, secondary cooling stirring and end stirring are adopted, the electric stirring current is 150 A, the electric stirring frequency is 6.0 Hz, the inlet straightening temperature is 1100 °C, the outlet straightening temperature is 1000 °C, the outlet straightening temperature is air-cooled after the straightening, the temperature of the cooling bed is 680 °C, and the ingot is hot-sent to steel rolling.

[0028] (2) Rolling process: The heating temperature is shown in Table 2, and the total heating time is 7 h. The billet opening speed after leaving the furnace is controlled at 1.4 m / s, and the billet opening temperature is 1150 °C. The continuous rolling temperature is 930 °C, and the round steel is slowly cooled in the pit. Example 5

[0029] The chemical composition content of the low alloy high strength steel of this embodiment is shown in Table 1; its smelting production process includes: converter / electric furnace-LF-VD / RH-continuous casting-hot delivery-rolling-slow cooling; wherein the key process parameters are controlled as follows: (1) Continuous casting and hot delivery process: The depth of the tundish water inlet is 95 mm, the continuous casting speed is controlled at 0.27 m / min, the water volume of the crystallizer is 4200 L / min, the water volume of the secondary cooling is 0.11 L / kg, the crystallizer stirring, secondary cooling stirring and end stirring are adopted, the electric stirring current is 130 A, the electric stirring frequency is 5.0 Hz, the inlet straightening temperature is 1040 °C, the outlet straightening temperature is 930 °C, the outlet straightening temperature is air-cooled, the temperature of the cooling bed is 620 °C, and the ingot is hot-sent to steel rolling.

[0030] (2) Rolling process: The heating temperature is shown in Table 2, and the total heating time is 6.2 h. The billet opening speed after leaving the furnace is controlled at 1.3 m / s, and the billet opening temperature is 1060 °C. The rolling temperature is 940 °C, and the round steel is slowly cooled in the pit. Example 6

[0031] The chemical composition content of the low alloy high strength steel of this embodiment is shown in Table 1; its smelting production process includes: converter / electric furnace-LF-VD / RH-continuous casting-hot delivery-rolling-slow cooling; wherein the key process parameters are controlled as follows: (1) Continuous casting and hot delivery process: The depth of the tundish water inlet is 91 mm, the continuous casting speed is controlled at 0.27 m / min, the water volume of the crystallizer is 4200 L / min, the water volume of the secondary cooling is 0.11 L / kg, the crystallizer stirring, secondary cooling stirring and end stirring are adopted, the electric stirring current is 120 A, the electric stirring frequency is 5.9 Hz, the inlet straightening temperature is 1040 °C, the outlet straightening temperature is 950 °C, the outlet straightening temperature is air-cooled, the temperature of the cooling bed is 630 °C, and the ingot is hot-sent to steel rolling.

[0032] (2) Rolling process: The heating temperature is shown in Table 2, and the total heating time is 6.8 h. The billet opening speed after leaving the furnace is controlled at 1.4 m / s, and the billet opening temperature is 1070 °C. The rolling temperature is 980 °C, and the round steel is slowly cooled in the pit. Example 7

[0033] The chemical composition content of the low alloy high strength steel of this embodiment is shown in Table 1; its smelting production process includes: converter / electric furnace-LF-VD / RH-continuous casting-hot delivery-rolling-slow cooling; wherein the key process parameters are controlled as follows: (1) Continuous casting and hot delivery process: The depth of the tundish water inlet is 99 mm, the continuous casting speed is controlled at 0.24 m / min, the water volume of the crystallizer is 4200 L / min, the water volume of the secondary cooling is 0.16 L / kg, the crystallizer stirring, secondary cooling stirring and end stirring are adopted, the electric stirring current is 120 A, the electric stirring frequency is 6.0 Hz, the inlet straightening temperature is 1090 °C, the outlet straightening temperature is 990 °C, the outlet straightening temperature is air-cooled, the temperature of the cooling bed is 650 °C, and the ingot is hot-sent to steel rolling.

[0034] (2) Rolling process: The heating temperature is shown in Table 2, and the total heating time is 6.9 h. The billet opening speed after leaving the furnace is controlled at 1.4 m / s, and the billet opening temperature is 1150 °C. The rolling temperature is 980 °C, and the round steel is slowly cooled in the pit. Example 8

[0035] The chemical composition content of the low alloy high strength steel of this embodiment is shown in Table 1; its smelting production process includes: converter / electric furnace-LF-VD / RH-continuous casting-hot delivery-rolling-slow cooling; wherein the key process parameters are controlled as follows: (1) Continuous casting and hot delivery process: The depth of the tundish water inlet is 98 mm, the continuous casting speed is controlled at 0.24 m / min, the water volume of the crystallizer is 4300 L / min, the water volume of the secondary cooling is 0.15 L / kg, the crystallizer stirring, secondary cooling stirring and end stirring are adopted, the electric stirring current is 100 A, the electric stirring frequency is 5.9 Hz, the inlet straightening temperature is 1010 °C, the outlet straightening temperature is 900 °C, the outlet straightening temperature is air-cooled, the temperature of the cooling bed is 680 °C, and the ingot is hot-sent to steel rolling.

[0036] (2) Rolling process: The heating temperature is shown in Table 2, and the total heating time is 6.7 h. The billet opening speed after leaving the furnace is controlled at 1.24 m / s, and the billet opening temperature is 1130 °C. The rolling temperature is 970 °C, and the round steel is slowly cooled in the pit.

[0037] Table 1 Chemical content of high strength steel in various examples (%)

[0038] Table 2 Heating system of high strength steel rolling process in various examples (℃)

[0039] The low-power mass and surface qualified rate of the high-strength steel in each embodiment are shown in Table 3 and Table 4 respectively.

[0040] Table 3 Low-power mass of high-strength steel in various examples

[0041] Table 4 Surface pass rate of high strength steel in various examples

[0042] It can be seen from Tables 3 and 4 that the present invention controls the temperature of the VD hanging bag, controls the temperature of the drawing and straightening machine, reduces the generation of NbC, and controls the heating rate. The low-alloy high-strength steel obtained has good surface quality and the magnetic leakage detection is ≤0.3mm.

[0043] Example 1 Surface morphology of high strength steel Figure 2 ,Depend on Figure 2 It can be seen that the surface quality of the rolled material is smooth, and no surface crack quality problem is found. The surface morphology of the high-strength steel in the other embodiments is the same as that in embodiment 1, and will not be shown one by one.

Claims

1. A method for producing surface defect-free low-alloy high-strength steel, It is characterized in that The production process of the high-strength steel includes: converter / electric furnace-LF-VD / RH-continuous casting-hot delivery-rolling-slow cooling; wherein, the continuous casting process adopts crystallizer stirring, secondary cooling stirring and end stirring, the electric stirring current is 100-150A, the electric stirring frequency is 5.0-6.0HZ, the entry drawing and straightening temperature is 1000-1100℃, and the exit drawing and straightening temperature is 900-1000℃.

2. The method for producing surface defect-free low-alloy high-strength steel according to claim 1, It is characterized in that In the continuous casting process, the depth of the water inlet of the middle ladle is 90-100 mm, the continuous casting speed is controlled at 0.24-0.28 m / min, the water volume of the crystallizer is 4200-4500 L / min, and the secondary cooling water volume is 0.11-0.17 L / kg.

3. The method for producing surface defect-free low-alloy high-strength steel according to claim 1, It is characterized in that In the hot delivery process, the ingot is air-cooled after being drawn and straightened to a cooling bed temperature of 600-700°C, and then hot-delivered to the rolled steel.

4. The method for producing surface defect-free low-alloy high-strength steel according to claim 1, It is characterized in that In the rolling process, the ingot is heated in a heating furnace, the temperature of the preheating section is controlled at 800-900°C, the temperature of zone 1 is controlled at 850-950°C, the temperature of zone 3 is controlled at 900-1050°C, the temperature of zone 5 is controlled at 1000-1180°C, the temperature of zone 7 is controlled at 1170-1250°C, and the temperature of zones 9-15 is controlled at 1240-1250°C. The total heating time is 6-7h.

5. The method for producing surface defect-free low-alloy high-strength steel according to claim 1, It is characterized in that In the rolling process, the blanking speed is controlled at 1.2-1.5 m / s and the blanking temperature is 1050-1150°C.

6. The method for producing surface defect-free low-alloy high-strength steel according to claim 1, It is characterized in that In the rolling process, the starting rolling temperature is 930-980°C, and the round steel is slowly cooled in the pit.

7. The method for producing surface defect-free low-alloy high-strength steel according to claim 1, It is characterized in that The composition range of the low alloy high strength steel is: C≤0.22%, Si≤0.50%, Mn: 0.95-1.65%, S≤0.010%, P≤0.015%, Cr≤0.30%, Nb: 0.020-0.030%.

8. The method for producing surface defect-free low-alloy high-strength steel according to claim 1, It is characterized in that The specification of the low-alloy high-strength steel is Ф120-200mm.

Citation Information

Cited By

  • Low-temperature alloy continuous casting equipment with belt feeding device and operation method of low-temperature alloy continuous casting equipment

    CN119319226A

  • Low temperature alloy continuous casting equipment with belt feeding device and operation method thereof

    CN119319226B