Additive repair thermal deformation method for overcoming thread damage of aircraft thin-wall annular assembly
By using special tooling and optimized powder in the laser additive repair of aircraft thin-walled annular components, the problems of weld penetration and thermal deformation are solved, the repair quality and efficiency are improved, the mechanical properties after repair are ensured, and the service life of the aircraft is extended. .
Patent Information
- Application Number
- CN202410812614.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-22
- Publication Date
- 2024-10-15
AI Technical Summary
Thread damage of aircraft thin-walled annular components can easily lead to weld penetration and thermal deformation during the laser additive repair process, and the material 1Cr17Ni2 stainless steel is prone to pores, resulting in unqualified performance after repair. It is difficult to effectively solve these problems with existing technology.
Special tooling and optimized powder preparation methods are used, including adding Y element to 1Cr17Ni2 stainless steel to prepare laser additive repair powder with a particle size of 53μm-150μm. Combined with heat dissipation and anti-deformation tooling and laser repair technology, material-level performance verification and Magnetic particle inspection to ensure repair quality.
It improves the quality of laser additive repair of thread damage in thin-walled annular components of aircraft, avoids welding penetration and thermal deformation, ensures that the mechanical properties after repair meet the requirements, and extends the service life of the aircraft.
Smart Images

Figure CN118768575A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of additive repair, and in particular to an additive repair thermal deformation method for overcoming thread damage of a thin-walled annular component of an aircraft. Background Art
[0002] During the aircraft overhaul process, thread damage problems of thin-walled circular ring components with load-bearing components often occur. The repair work can only be carried out under the original heat treatment state and without any auxiliary heat treatment premise, and it is ensured that the performance of the repaired area should meet the mechanical performance requirements. In order to ensure the quality of its repair, its repair method can only be completed by laser cladding repair. The repair process is: mechanical processing to remove the entire thread-laser additive-laser processing of the thread. However, the wall of the thin-walled component is easy to weld through, and the thermal effect during the laser cladding repair process will cause the component to deform; at the same time, the component material is 1Cr17Ni2 stainless steel, which is easy to produce pores during the laser additive repair process, resulting in defects in the mechanical processing of the thread after additive, and ultimately resulting in unqualified performance of the repaired product, so that the entire thread must be removed and repaired again by additive. Based on this, it is urgent to design a laser repair process to overcome the defect formation and thermal deformation during the laser additive repair of the annular component, and improve the quality and efficiency of additive repair of thread damage of the aircraft thin-walled annular component. Summary of the invention
[0003] In order to solve the above problems, the present invention proposes a method for additively repairing thermal deformation of damaged threads of aircraft thin-walled annular components.
[0004] A method for overcoming thermal deformation of aircraft thin-walled annular component thread damage by additive repair, the specific steps of which are as follows:
[0005] S1. Use special tooling: control the assembly gap between the special tooling and the thin-walled annular component to 0.04mm;
[0006] S2. Preparation of powder for laser additive repair:
[0007] S21, the repair powder is prepared by adding Y element to 1Cr17Ni2 stainless steel, the mass fraction of 1Cr17Ni2 in the repair powder is 99.5%-99.9%, and the mass fraction of Y is 0.1%-0.5%;
[0008] S22, preparation of repair powder;
[0009] S3. Conduct material-level performance verification:
[0010] S31. The tensile test bar is made of the same 1Cr17Ni2 material as the thin-walled annular component. A groove-shaped notch is prefabricated on the test bar, and the groove on the sample is filled by laser cladding;
[0011] S32, after making the rod-shaped tensile specimen, perform X-ray flaw detection to detect the internal defects of the cladding area;
[0012] S33, the weld is located at the center of the specimen, and the tensile test is carried out on a WDW-100 testing machine to detect the mechanical properties of the laser cladding test piece;
[0013] S4. Detection process:
[0014] S41, turning off all threads on the thin-walled annular component;
[0015] S42, installing the heat dissipation and anti-deformation tooling on the thin-walled annular component, and installing the thin-walled annular component as a whole on the positioner;
[0016] S43. Use a wire brush or mechanical grinding tool to clean the end surface of the repaired area to remove the oxide layer, ensure that the metal luster is exposed, the surface is clean and cleaned with acetone;
[0017] S44, laser additive repair of thin-walled annular components;
[0018] S45, machining threads on the thin-walled annular component repaired by laser additive manufacturing;
[0019] S5. Carry out magnetic particle inspection on the machined thin-walled circular components, and they can be put into use if there are no cracks.
[0020] The special tooling in step S1 includes an internal hollow barrel body, a cover surface arranged at the end surface of the internal hollow barrel body, and a water inlet and a water outlet arranged at the cover surface. The internal hollow barrel body and the cover surface are sealed by welding.
[0021] The special tooling in step S1 is made of red copper; the assembly clearance of the product is 0.05 mm.
[0022] The preparation steps of step S21 are as follows:
[0023] S211, adding Y element to 1Cr17Ni2 stainless steel to prepare alloy ingot;
[0024] S212, performing degreasing and rust removal pretreatment on the alloy ingot;
[0025] S213, atomizing the pretreated alloy ingot to make powder, and sieving and post-processing the powder to obtain powder for laser additive repair with a particle size of 53 μm-150 μm;
[0026] The maximum load of the testing machine in step S33 is 100KN, and the loading rate is 1mm / S.
[0027] In the step S42, a water inlet pipe and a water outlet pipe are respectively installed on the water inlet 3 and the water outlet 4 of the heat dissipation deformation tooling, wherein the water inlet pipe and the water outlet pipe are respectively connected to the circulating water chiller.
[0028] The beneficial effects of the present invention are:
[0029] The present invention applies laser additive repair heat dissipation and anti-deformation tooling design technology, powder design and preparation technology, and laser repair process to laser additive repair of thread damage of aircraft thin-walled annular components, solving the problem that the application of conventional powders and conventional process repairs is difficult to meet the use requirements of thin-walled annular components, thereby improving the quality of laser additive repair of aircraft thin-walled annular components. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0031] Figure 1 It is a schematic diagram of the three-dimensional structure of the special tooling of the present invention;
[0032] Figure 2 It is a side view structural schematic diagram of the special tooling of the present invention;
[0033] Figure 3 It is a schematic diagram of the main structure of the special tooling of the present invention;
[0034] Figure 4 For the present invention Figure 3 AA cross-sectional structural diagram;
[0035] Figure 5 It is a schematic diagram of the assembly structure of the present invention;
[0036] Figure numerals: 1. internal hollow barrel body; 2. cover; 3. water inlet; 4. water outlet. DETAILED DESCRIPTION
[0037] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below.
[0038] like Figures 1 to 5 As shown, a method for overcoming thermal deformation of aircraft thin-walled annular component thread damage by additive repair, the specific steps are as follows:
[0039] S1. Use special tooling: control the assembly gap between the special tooling and the thin-walled annular component to 0.04mm;
[0040] S2. Preparation of powder for laser additive repair:
[0041] S21, the repair powder is prepared by adding Y element to 1Cr17Ni2 stainless steel, the mass fraction of 1Cr17Ni2 in the repair powder is 99.5%-99.9%, and the mass fraction of Y is 0.1%-0.5%;
[0042] S22, preparation of repair powder;
[0043] S3. Conduct material-level performance verification:
[0044] S31. The tensile test bar is made of the same 1Cr17Ni2 material as the thin-walled annular component. A groove-shaped notch is prefabricated on the test bar, and the groove on the sample is filled by laser cladding;
[0045] S32, after making the rod-shaped tensile specimen, perform X-ray flaw detection to detect the internal defects of the cladding area;
[0046] S33, the weld is located at the center of the specimen, and the tensile test is carried out on a WDW-100 testing machine to detect the mechanical properties of the laser cladding test piece;
[0047] S4. Detection process:
[0048] S41, turning off all threads on the thin-walled annular component;
[0049] S42, installing the heat dissipation and anti-deformation tooling on the thin-walled annular component, and installing the thin-walled annular component as a whole on the positioner;
[0050] S43. Use a wire brush or mechanical grinding tool to clean the end surface of the repaired area to remove the oxide layer, ensure that the metal luster is exposed, the surface is clean and cleaned with acetone;
[0051] S44, laser additive repair of thin-walled annular components;
[0052] S45, machining threads on the thin-walled annular component repaired by laser additive manufacturing;
[0053] S5. Carry out magnetic particle inspection on the machined thin-walled circular components, and they can be put into use if there are no cracks.
[0054] The special tooling in step S1 includes an internal hollow barrel body 1, a cover surface 2 arranged at the end surface of the internal hollow barrel body 1, and a water inlet 3 and a water outlet 4 arranged at the cover surface 2. The internal hollow barrel body 1 and the cover surface 2 are sealed by welding, and a flowing water cooling system is configured inside the device.
[0055] The step S3 of laser additive manufacturing of the optimally designed alloy powder and the optimal repair process on the 1Cr17Ni2 substrate can obtain a tensile strength effect that meets the requirements, ensure the safety of the aircraft, extend the service life of the aircraft, and have high economic benefits.
[0056] According to the thread damage morphology of thin-walled annular components and the characteristics of thin walls, and the heat accumulation effect caused by continuous laser action during laser additive repair, which leads to thermal deformation, the deformation amount after laser additive repair of the annular part accessories is introduced to determine the repair quality. In order to ensure the effect of the annular anti-deformation tooling, the thermal conductivity and rigidity requirements of the material used to make the anti-deformation tooling need to be considered. Based on this, the special tooling of step S1 is made of red copper; the assembly clearance of the product is 0.05mm.
[0057] According to the above alloy powder composition design criteria and preparation methods, 5 composition cases were designed and prepared, namely:
[0058] Scheme 1: Component composition: 1Cr17Ni2 powder with a mass fraction of 99.5%, and Y with a mass fraction of 0.5%;
[0059] Scheme 2 composition: 1Cr17Ni2 powder with a mass fraction of 99.6%, and Y with a mass fraction of 0.4%;
[0060] Scheme 3 composition: 1Cr17Ni2 powder with a mass fraction of 99.7%, and Y with a mass fraction of 0.3%;
[0061] Scheme 4 composition: 1Cr17Ni2 powder with a mass fraction of 99.8%, and Y with a mass fraction of 0.2%;
[0062] Scheme 5: Components: 1Cr17Ni2 powder with a mass fraction of 99.9% and Y with a mass fraction of 0.1%;
[0063] The 1Cr17Ni2 stainless steel substrate was repaired using the optimal laser repair parameters, and the repair bonding performance was tested:
[0064]
[0065] The performance optimization test shows that the powder repair performance of Scheme 3 is the best. Therefore, the product repair adopts the powder repair of Scheme 3, and then the repair preparation is carried out.
[0066] The preparation steps of step S21 are as follows:
[0067] S211, adding Y element to 1Cr17Ni2 stainless steel to prepare alloy ingot;
[0068] S212, performing degreasing and rust removal pretreatment on the alloy ingot;
[0069] S213, atomizing the pretreated alloy ingot to make powder, and sieving and post-processing the powder to obtain powder for laser additive repair with a particle size of 53 μm-150 μm;
[0070] The maximum load of the testing machine in step S33 is 100KN, and the loading rate is 1mm / S.
[0071] In the step S42, a water inlet pipe and a water outlet pipe are respectively installed on the water inlet 3 and the water outlet 4 of the heat dissipation deformation tooling, wherein the water inlet pipe and the water outlet pipe are respectively connected to the circulating water chiller.
[0072] The present invention applies laser additive repair heat dissipation and anti-deformation tooling design technology, powder design and preparation technology, and laser repair process to laser additive repair of thread damage of aircraft thin-walled annular components, solving the problem that the application of conventional powders and conventional process repairs is difficult to meet the use requirements of thin-walled annular components, thereby improving the quality of laser additive repair of aircraft thin-walled annular components.
[0073] The repair parameters of step S44 are as follows:
[0074] Laser cladding equipment: complete set of laser cladding equipment, i.e. 4KW IPG laser and Kuka robot;
[0075] Carrier gas: 99.999% high purity argon;
[0076] Restorative powder: powder prepared by optimizing the design of ingredients;
[0077] Powder specifications: 53~150μm;
[0078] Laser power: 700~950W;
[0079] Scanning speed: 8-10 mm / s;
[0080] Powder feeder reading: low%;
[0081] Powder carrier gas: 380~400L / h;
[0082] Overlap rate: 50-60%;
[0083] Spot diameter 1.5~2.5mm;
[0084] Chiller flow rate: 1~3L / min.
[0085] In the step S44, after each layer is repaired, an infrared thermometer is used to monitor the temperature between the repaired layers, and when the temperature between the layers is lower than 60° C., the next layer is melt-clad.
[0086] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for overcoming thermal deformation of thread damage in aircraft thin-walled annular components by additive repair. Features: The specific steps are as follows: S1. Use special tooling: control the assembly gap between the special tooling and the thin-walled annular component to 0.04mm; S2. Preparation of powder for laser additive repair: S21, the repair powder is prepared by adding Y element to 1Cr17Ni2 stainless steel, the mass fraction of 1Cr17Ni2 in the repair powder is 99.5%-99.9%, and the mass fraction of Y is 0.1%-0.5%; S22, preparation of repair powder; S3. Conduct material-level performance verification: S31. The tensile test bar is made of the same 1Cr17Ni2 material as the thin-walled annular component. A groove-shaped notch is prefabricated on the test bar, and the groove on the sample is filled by laser cladding; S32, after making the rod-shaped tensile specimen, perform X-ray flaw detection to detect the internal defects of the cladding area; S33, the weld is located at the center of the specimen, and the tensile test is carried out on a WDW-100 testing machine to detect the mechanical properties of the laser cladding test piece; S4. Detection process: S41, turning off all threads on the thin-walled annular component; S42, installing the heat dissipation and anti-deformation tooling on the thin-walled annular component, and installing the thin-walled annular component as a whole on the positioner; S43. Use a wire brush or mechanical grinding tool to clean the end surface of the repaired area to remove the oxide layer, ensure that the metal luster is exposed, the surface is clean and cleaned with acetone; S44, laser additive repair of thin-walled annular components; S45, machining threads on the thin-walled annular component repaired by laser additive manufacturing; S5. Carry out magnetic particle inspection on the machined thin-walled circular components, and they can be put into use if there are no cracks.
2. According to claim 1, a method for overcoming thermal deformation of aircraft thin-walled annular component thread damage by additive repair, Features: The special tooling in step S1 comprises an internal hollow barrel body (1), a cover surface (2) arranged at the end surface of the internal hollow barrel body (1), and a water inlet (3) and a water outlet (4) arranged at the cover surface (2); the internal hollow barrel body (1) and the cover surface (2) are sealed by welding.
3. According to claim 1, a method for overcoming thermal deformation of aircraft thin-walled annular component thread damage by additive repair, Features: The special tooling in step S1 is made of red copper; the assembly clearance of the product is 0.05 mm.
4. According to claim 1, a method for overcoming thermal deformation of aircraft thin-walled annular component thread damage by additive repair, Features: The preparation steps of step S21 are as follows: S211, adding Y element to 1Cr17Ni2 stainless steel to prepare alloy ingot; S212, performing degreasing and rust removal pretreatment on the alloy ingot; S213, atomizing the pretreated alloy ingot to make powder, and sieving and post-processing the powder to obtain powder for laser additive repair with a particle size of 53 μm-150 μm.
5. A method for overcoming thermal deformation of thread damage of aircraft thin-walled annular components by additive repair according to claim 4, Features: The maximum load of the testing machine in step S33 is 100KN, and the loading rate is 1mm / S.
6. A method for overcoming thermal deformation of aircraft thin-walled annular component thread damage by additive repair according to claim 2, Features: In the step S42, a water inlet pipe and a water outlet pipe are respectively installed on the water inlet (3) and the water outlet (4) of the heat dissipation deformation tooling, wherein the water inlet pipe and the water outlet pipe are respectively connected to a circulating water chiller.
7. According to claim 1, a method for overcoming thermal deformation of aircraft thin-walled annular component thread damage by additive repair, Features: The repair parameters of step S44 are as follows: Laser cladding equipment: complete set of laser cladding equipment; Carrier gas: 99.999% high purity argon; Restorative powder: powder prepared by optimizing the design of ingredients; Powder specifications: 53~150μm; Laser power: 700~950W; Scanning speed: 8-10 mm / s; Powder feeder reading: low%; Powder carrier gas: 380~400L / h; Overlap rate: 50-60%; Spot diameter 1.5~2.5mm; Chiller flow rate: 1~3L / min.
8. According to claim 1, a method for overcoming thermal deformation of aircraft thin-walled annular component thread damage by additive repair, Features: In the step S44, after each layer is repaired, an infrared thermometer is used to monitor the temperature between the repaired layers, and when the temperature between the layers is lower than 60° C., the next layer is melt-clad.