High-efficiency silicon wafer polishing wax-free pad and production process thereof

By adding support pillars and reinforced struts in the base layer of the wax-free pad, and using the pore structure to increase the support strength, the problem of insufficient support of the wax-free pad is solved and the polishing efficiency is significantly improved.

CN118769144AActive Publication Date: 2024-10-15ANHUI HECHEN NEW MATERIAL CO LTD

Patent Information

Application Number
CN202410946615.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-15
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The existing wax-free pad lacks internal support during use, resulting in low support strength, easy relaxation and damage, and reduced polishing efficiency.

Method used

By adding support pillars and reinforced struts in the base layer, and inflating the support pillars through the air inlet, and using the exhaust holes to fill the base layer, the support strength of the base layer is improved, forming an efficient wax-free silicon wafer polishing pad.

Benefits of technology

Improves the support strength of the wax-free pad, avoids loosening damage, and improves polishing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118769144A_ABST
    Figure CN118769144A_ABST
Patent Text Reader

Abstract

The invention discloses a high-efficiency silicon wafer polishing wax-free pad and a production process thereof, and belongs to the technical field of wax-free pads, the high-efficiency silicon wafer polishing wax-free pad comprises a basic substrate layer and an adsorption polishing layer, and the adsorption polishing layer is arranged on the basic substrate layer. The wax-free pad solves the problems that when an existing wax-free pad is used, due to the fact that the wax-free pad lacks internal supporting, the supporting strength of the wax-free pad is low, the wax-free pad is prone to loosening and being damaged, and the polishing efficiency of the wax-free pad is reduced. The reinforcing supporting rods are evenly distributed on the circumferential face of the supporting base column, the supporting strength of the base layer can be improved through the supporting base column and the reinforcing supporting rods, air is inflated into the supporting base column through the air inlet, exhausted into the reinforcing supporting rods through the supporting base column and exhausted into the base layer through the exhaust holes in the reinforcing supporting rods, and therefore the base layer can be filled. The supporting strength of the base layer can be improved, the supporting strength of the wax-free pad is high, the wax-free pad can be prevented from being loosened and damaged, and the polishing efficiency of the wax-free pad can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wax-free pads, in particular to a high-efficiency wax-free pad for polishing silicon wafers and a production process thereof. Background Art

[0002] In the process of semiconductor material processing, silicon wafers, as the basic materials of commonly used semiconductor devices and integrated circuits, often need to be polished, and the quality of polishing technology will directly affect the quality of the silicon wafer surface and the performance of semiconductor devices; there are two main traditional polishing technologies: wax polishing and wax-free polishing. The wax technology is to bond the silicon wafer to the flat plate of the ceramic disk. During polishing, the polishing head drives the ceramic disk to rotate on the polishing cloth, and the polishing purpose is achieved under the action of mechanical pressure and polishing liquid. Practice has found that this wax polishing has the defects of wax pollution and low polishing accuracy. With the rapid development of electronic technology and the increasing degree of integration of large-scale integrated circuits, people's requirements for semiconductor devices have become more stringent, so the advantages of wax-free polishing have gradually been reflected.

[0003] The Chinese patent with the publication number CN112873074B discloses a wax-free pad for polishing, which includes a base chassis, a wafer placement hole, a snap-on pad and a wax-free adsorption pad. At least one wafer placement hole is provided on the surface of the base chassis, and a wax-free adsorption pad for adsorbing the wafer is provided in the wafer placement hole. At least one snap-on pad is provided between the wax-free adsorption pad and the inner bottom of the wafer placement hole. A composite resin is produced by reacting epoxy resin and polyurethane prepolymer, and the composite resin is used as an adhesive layer. The adhesive layer has the characteristics of both epoxy resin and polyurethane resin, has high viscosity and elasticity, and can be well bonded with the carbon fiber layer and the adsorption layer to avoid stratification of the wax-free adsorption pad. However, the above patent has the following defects:

[0004] When the existing wax-free pad is used, the wax-free pad lacks internal support, resulting in low support strength of the wax-free pad. The wax-free pad is easily loosened and damaged, thereby reducing the polishing efficiency of the wax-free pad. Summary of the invention

[0005] The purpose of the present invention is to provide a wax-free pad for high-efficiency polishing of silicon wafers and a production process thereof, which can improve the supporting strength of the wax-free pad, prevent the wax-free pad from loosening and being damaged, and improve the polishing efficiency of the wax-free pad, thereby solving the problems raised in the above-mentioned background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A high-efficiency wax-free polishing pad for silicon wafers comprises a base substrate layer and an adsorption polishing layer, wherein the adsorption polishing layer is arranged on the base substrate layer, and the thickness ratio of the base substrate layer to the adsorption polishing layer is 1:1-2.

[0008] Preferably, the base substrate layer comprises the following raw materials in parts by mass: 30-40 parts of modified epoxy resin, 10-30 parts of carbon fiber, 10-20 parts of filler and 20-30 parts of curing agent.

[0009] Preferably, the adsorption polishing layer comprises a base layer, a polishing layer and an adsorption layer, the base layer is arranged on the basic substrate layer, the base layer is provided with a polishing layer, the polishing layer is provided with a silicon wafer placement groove, and the adsorption layer is arranged in the silicon wafer placement groove.

[0010] Preferably, a support reinforcement component is arranged in the base layer, and the support reinforcement component includes a support base column and a reinforcement support rod. The support base column is arranged in the base layer, and the reinforcement support rods are evenly distributed on the circumferential surface of the support base column. The reinforcement support rods are used to enhance the support strength of the base layer.

[0011] Preferably, the support base column is connected to the reinforcing support rod, and an air inlet is provided on the support base column. The air inlet is sealed and connected to the base layer, and the air inlet passes through the polishing layer.

[0012] Preferably, the reinforcing support rod is located in the base layer, and exhaust holes are provided at the bottom and the top of the reinforcing support rod, and the exhaust holes are distributed at equal intervals.

[0013] Preferably, the polishing layer comprises the following raw materials in parts by mass: 2-10 parts of fluorine-containing polyurethane, 0-4 parts of thermoplastic polyurethane, 1-2 parts of mixed fiber material, 1-3 parts of carboxymethyl cellulose glue, 25-35 parts of abrasive adhesive, 55-70 parts of organic solvent and 0-0.3 parts of additive.

[0014] Preferably, the adsorption layer comprises the following raw materials in parts by mass: 2-20 parts of fluorine-containing polyurethane, 1-10 parts of thermoplastic polyurethane, 0-2 parts of zinc oxide, 0-3 parts of activated carbon fiber, 65-95 parts of organic solvent and 0-0.5 parts of auxiliary agent.

[0015] According to another aspect of the present invention, there is provided a production process for a high-efficiency wax-free polishing pad for silicon wafers as described above, comprising the following steps:

[0016] S1. Production of base substrate layer:

[0017] Add modified epoxy resin, carbon fiber, filler and curing agent into an extruder, stir, mix, plasticize and compact in the extruder, extrude a pre-product of a certain shape, and repeatedly extrude and extend the pre-product through a calender to form a base substrate layer with uniform thickness;

[0018] S2. Production of adsorption polishing layer:

[0019] A connected supporting column and a reinforcing support rod are processed in the base layer, an air inlet is processed on the supporting column, and an exhaust hole is processed at the bottom and top of the reinforcing support rod;

[0020] Fluorine-containing polyurethane, thermoplastic polyurethane, mixed fiber material, carboxymethyl cellulose glue, abrasive adhesive, organic solvent and additives are added into an extruder, and after being stirred, mixed, plasticized and compacted by the extruder, a pre-product of a certain shape is extruded, and the pre-product is repeatedly extruded and extended by a calender to form a polishing layer with uniform thickness;

[0021] Fluorine-containing polyurethane, thermoplastic polyurethane, zinc oxide, activated carbon fiber, organic solvent and additives are added into an extruder, stirred, mixed, plasticized and compacted by the extruder, and then a pre-product of a certain shape is extruded, and the pre-product is repeatedly extruded and extended by a calender to form an adsorption layer with uniform thickness;

[0022] Processing a silicon wafer placement groove on the polishing layer, processing an adsorption layer in the silicon wafer placement groove, and processing the polishing layer on the surface of the base layer to form an adsorption polishing layer;

[0023] S3, production of wax-free pads:

[0024] The produced absorbent polishing layer is placed on a base backing layer and, after lamination, forms a wax-free pad.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The present invention adds support columns and reinforcing rods in the base layer, and the reinforcing rods are evenly distributed on the circumferential surface of the support columns. The support strength of the base layer can be improved through the support columns and the reinforcing rods. Air is inflated into the support columns through the air inlet, discharged into the reinforcing rods through the support columns, and then discharged into the base layer through the exhaust holes on the reinforcing rods. The base layer can be filled, the support strength of the base layer can be improved, the support strength of the wax-free pad can be high, the wax-free pad can be prevented from being loosened and damaged, and the polishing efficiency of the wax-free pad can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a forward schematic diagram of a wax-free pad for high-efficiency polishing of silicon wafers according to the second embodiment of the present invention;

[0028] Figure 2 It is a forward schematic diagram of the adsorption polishing layer of the second embodiment of the present invention;

[0029] Figure 3 It is a forward exploded view of the adsorption polishing layer of the second embodiment of the present invention;

[0030] Figure 4 It is a forward schematic diagram of a wax-free pad for high-efficiency polishing of silicon wafers according to the first embodiment of the present invention;

[0031] Figure 5 It is a forward exploded view of the connection between the base layer and the polishing layer of the first embodiment of the present invention;

[0032] Figure 6 It is a partial exploded view of the adsorption polishing layer of the first embodiment of the present invention;

[0033] Figure 7 It is a forward exploded view of the adsorption polishing layer of the first embodiment of the present invention;

[0034] Figure 8 It is a front schematic diagram of the support reinforcement assembly of the first embodiment of the present invention.

[0035] In the figure: 1, base substrate layer; 2, adsorption polishing layer; 21, base layer; 22, polishing layer; 221, silicon wafer placement groove; 23, adsorption layer; 24, support reinforcement component; 241, support base column; 2411, air inlet; 242, reinforcement support rod; 2421, exhaust hole. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] In order to solve the problem that the existing wax-free pads lack internal support during use, resulting in low support strength of the wax-free pads, which makes the wax-free pads easy to loosen and damage, thereby reducing the polishing efficiency of the wax-free pads, please refer to Figure 1-Figure 8 , this embodiment provides the following technical solutions:

[0038] Embodiment 1

[0039] A high-efficiency wax-free polishing pad for silicon wafers comprises a base substrate layer 1 and an adsorption polishing layer 2. The base substrate layer 1 is provided with the adsorption polishing layer 2, and the thickness ratio of the base substrate layer 1 to the adsorption polishing layer 2 is 1:2.

[0040] In this embodiment, the base substrate layer 1 includes the following raw materials in parts by mass: 30 parts of modified epoxy resin, 10 parts of carbon fiber, 10 parts of filler and 20 parts of curing agent.

[0041] In this embodiment, the adsorption polishing layer 2 includes a base layer 21, a polishing layer 22 and an adsorption layer 23. The base layer 21 is arranged on the basic substrate layer 1, and the polishing layer 22 is arranged on the base layer 21. A silicon wafer placement groove 221 is opened on the polishing layer 22, and the adsorption layer 23 is arranged in the silicon wafer placement groove 221.

[0042] In this embodiment, a support reinforcement component 24 is arranged in the base layer 21, and the support reinforcement component 24 includes a support base column 241 and a reinforcement support rod 242. The support base column 241 is arranged in the base layer 21, and the reinforcement support rods 242 are evenly distributed on the circumferential surface of the support base column 241. The reinforcement support rods 242 are used to enhance the support strength of the base layer 21.

[0043] It should be noted that by adding support base columns 241 and reinforcing support rods 242 in the base layer 21, and making the reinforcing support rods 242 evenly distributed on the circumferential surface of the support base columns 241, the support strength of the base layer 21 can be improved by the support base columns 241 and the reinforcing support rods 242, so that the support strength of the wax-free pad is high, the wax-free pad can be prevented from loosening and being damaged, and the polishing efficiency of the wax-free pad can be improved.

[0044] In this embodiment, the support base column 241 is connected to the reinforcing support rod 242 , and an air inlet 2411 is provided on the support base column 241 . The air inlet 2411 is sealed and connected to the base layer 21 , and the air inlet 2411 passes through the polishing layer 22 .

[0045] In this embodiment, the reinforcing support rod 242 is located in the base layer 21 , and the bottom and top of the reinforcing support rod 242 are both provided with exhaust holes 2421 , and the exhaust holes 2421 are distributed at equal intervals.

[0046] It should be noted that air is inflated into the support base column 241 through the air inlet 2411, discharged into the reinforcing support rod 242 through the support base column 241, and discharged into the base layer 21 through the exhaust hole 2421 on the reinforcing support rod 242, so that the base layer 21 can be filled, the supporting strength of the base layer 21 can be improved, the supporting strength of the wax-free pad can be high, the wax-free pad can be prevented from being loosened and damaged, and the polishing efficiency of the wax-free pad can be improved.

[0047] In this embodiment, the polishing layer 22 includes the following raw materials in parts by mass: 10 parts of fluorine-containing polyurethane, 4 parts of thermoplastic polyurethane, 2 parts of mixed fiber material, 3 parts of carboxymethyl cellulose glue, 35 parts of abrasive adhesive, 70 parts of organic solvent and 0.3 parts of additive.

[0048] In this embodiment, the adsorption layer 23 includes the following raw materials in parts by mass: 20 parts of fluorine-containing polyurethane, 10 parts of thermoplastic polyurethane, 2 parts of zinc oxide, 3 parts of activated carbon fiber, 95 parts of organic solvent and 0.5 parts of auxiliary agent.

[0049] In order to better demonstrate the production process of a high-efficiency wax-free polishing pad for silicon wafers, this embodiment provides a production process of a high-efficiency wax-free polishing pad for silicon wafers according to the above-mentioned method, comprising the following steps:

[0050] S1. Production of base substrate layer 1:

[0051] Add modified epoxy resin, carbon fiber, filler and curing agent into an extruder, stir, mix, plasticize and compact in the extruder, extrude a pre-product of a certain shape, and repeatedly extrude and extend the pre-product through a calender to form a base substrate layer 1 with uniform thickness;

[0052] S2, production of adsorption polishing layer 2:

[0053] A supporting column 241 and a reinforcing support rod 242 are formed in the base layer 21, an air inlet 2411 is formed on the supporting column 241, and an exhaust hole 2421 is formed on the bottom and top of the reinforcing support rod 242;

[0054] Fluorine-containing polyurethane, thermoplastic polyurethane, mixed fiber material, carboxymethyl cellulose glue, abrasive adhesive, organic solvent and additives are added into an extruder, stirred, mixed, plasticized and compacted by the extruder, and a pre-product of a certain shape is extruded, and the pre-product is repeatedly extruded and stretched by a calender to form a polishing layer 22 with uniform thickness;

[0055] Fluorine-containing polyurethane, thermoplastic polyurethane, zinc oxide, activated carbon fiber, organic solvent and additives are added into an extruder, stirred, mixed, plasticized and compacted by the extruder, and then a pre-product of a certain shape is extruded, and the pre-product is repeatedly extruded and stretched by a calender to form an adsorption layer 23 with uniform thickness;

[0056] A silicon wafer placement groove 221 is processed on the polishing layer 22, and an adsorption layer 23 is processed in the silicon wafer placement groove 221, and the polishing layer 22 is processed on the surface of the base layer 21 to form an adsorption polishing layer 2;

[0057] S3, production of wax-free pads:

[0058] The produced adsorption polishing layer 2 is placed on the base substrate layer 1 and, after lamination, a wax-free pad is formed.

[0059] Embodiment 2

[0060] A high-efficiency wax-free polishing pad for silicon wafers comprises a base substrate layer 1 and an adsorption polishing layer 2. The base substrate layer 1 is provided with the adsorption polishing layer 2, and the thickness ratio of the base substrate layer 1 to the adsorption polishing layer 2 is 1:2.

[0061] In this embodiment, the base substrate layer 1 includes the following raw materials in parts by mass: 30 parts of modified epoxy resin, 10 parts of carbon fiber, 10 parts of filler and 20 parts of curing agent.

[0062] In this embodiment, the adsorption polishing layer 2 includes a base layer 21, a polishing layer 22 and an adsorption layer 23. The base layer 21 is arranged on the basic substrate layer 1, and the polishing layer 22 is arranged on the base layer 21. A silicon wafer placement groove 221 is opened on the polishing layer 22, and the adsorption layer 23 is arranged in the silicon wafer placement groove 221.

[0063] In this embodiment, a support reinforcement component 24 is arranged in the base layer 21, and the support reinforcement component 24 includes a support base column 241 and a reinforcement support rod 242. The support base column 241 is arranged in the base layer 21, and the reinforcement support rods 242 are evenly distributed on the circumferential surface of the support base column 241. The reinforcement support rods 242 are used to enhance the support strength of the base layer 21.

[0064] It should be noted that by adding support base columns 241 and reinforcing support rods 242 in the base layer 21, and making the reinforcing support rods 242 evenly distributed on the circumferential surface of the support base columns 241, the support strength of the base layer 21 can be improved by the support base columns 241 and the reinforcing support rods 242, so that the support strength of the wax-free pad is high, the wax-free pad can be prevented from loosening and being damaged, and the polishing efficiency of the wax-free pad can be improved.

[0065] In this embodiment, the polishing layer 22 includes the following raw materials in parts by mass: 10 parts of fluorine-containing polyurethane, 4 parts of thermoplastic polyurethane, 2 parts of mixed fiber material, 3 parts of carboxymethyl cellulose glue, 35 parts of abrasive adhesive, 70 parts of organic solvent and 0.3 parts of additive.

[0066] In this embodiment, the adsorption layer 23 includes the following raw materials in parts by mass: 20 parts of fluorine-containing polyurethane, 10 parts of thermoplastic polyurethane, 2 parts of zinc oxide, 3 parts of activated carbon fiber, 95 parts of organic solvent and 0.5 parts of auxiliary agent.

[0067] Compared with the first embodiment, the structures of the air inlet 2411 and the exhaust hole 2421 are eliminated in the second embodiment. The wax-free pad is produced by the same production process as the first embodiment, and the production steps of the air inlet 2411 and the exhaust hole 2421 are eliminated accordingly.

[0068] Comparative Example

[0069] A high-efficiency wax-free polishing pad for silicon wafers comprises a base substrate layer 1 and an adsorption polishing layer 2. The base substrate layer 1 is provided with the adsorption polishing layer 2, and the thickness ratio of the base substrate layer 1 to the adsorption polishing layer 2 is 1:2.

[0070] In this embodiment, the base substrate layer 1 includes the following raw materials in parts by mass: 30 parts of modified epoxy resin, 10 parts of carbon fiber, 10 parts of filler and 20 parts of curing agent.

[0071] In this embodiment, the adsorption polishing layer 2 includes a base layer 21, a polishing layer 22 and an adsorption layer 23. The base layer 21 is arranged on the basic substrate layer 1, and the polishing layer 22 is arranged on the base layer 21. A silicon wafer placement groove 221 is opened on the polishing layer 22, and the adsorption layer 23 is arranged in the silicon wafer placement groove 221.

[0072] In this embodiment, the polishing layer 22 includes the following raw materials in parts by mass: 10 parts of fluorine-containing polyurethane, 4 parts of thermoplastic polyurethane, 2 parts of mixed fiber material, 3 parts of carboxymethyl cellulose glue, 35 parts of abrasive adhesive, 70 parts of organic solvent and 0.3 parts of additive.

[0073] In this embodiment, the adsorption layer 23 includes the following raw materials in parts by mass: 20 parts of fluorine-containing polyurethane, 10 parts of thermoplastic polyurethane, 2 parts of zinc oxide, 3 parts of activated carbon fiber, 95 parts of organic solvent and 0.5 parts of auxiliary agent.

[0074] Compared with the second embodiment, the structure of the support and reinforcement component 24 is eliminated in the comparative example, and the wax-free pad is produced by the same production process as the second embodiment, and the production steps of the support and reinforcement component 24 are eliminated accordingly.

[0075] The wax-free pads produced in Examples 1-2 and Comparative Examples were subjected to performance tests, and the performance test results of the wax-free pads are shown in Table 1:

[0076] Table 1: Wax-free pad performance test results

[0077]

[0078]

[0079] Therefore, it can be seen from the above table that the wax-free pads produced in Examples 1-2 all have good supporting strength and anti-loosening performance.

[0080] Among them, compared with Example 1, the supporting strength and anti-relaxation performance of Example 2 are reduced. Since the air inlet 2411 and the exhaust hole 2421 are not added in Example 2, the supporting strength and anti-relaxation performance of the wax-free pad are reduced, which indicates that the air inlet 2411 and the exhaust hole 2421 can improve the supporting strength and anti-relaxation performance of the wax-free pad.

[0081] Among them, compared with Example 2, the support strength and anti-relaxation performance of the comparative example are reduced. Since the support reinforcement component is not added in the comparative example, the support strength and anti-relaxation performance of the wax-free pad are reduced, which shows that the support reinforcement component can improve the support strength and anti-relaxation performance of the wax-free pad.

[0082] Therefore, by adding support columns 241 and reinforcing rods 242 in the base layer 21, and making the reinforcing rods 242 evenly distributed on the circumferential surface of the support columns 241, the support strength of the base layer 21 can be improved through the support columns 241 and the reinforcing rods 242, and air is inflated into the support columns 241 through the air inlet 2411, discharged into the reinforcing rods 242 through the support columns 241, and then discharged into the base layer 21 through the exhaust holes 2421 on the reinforcing rods 242, so that the base layer 21 can be filled, the support strength of the base layer 21 can be improved, the support strength of the wax-free pad can be high, the wax-free pad can be prevented from being loosened and damaged, and the polishing efficiency of the wax-free pad can be improved.

[0083] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0084] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high-efficiency wax-free polishing pad for silicon wafers, comprising a base substrate layer (1) and an adsorption polishing layer (2), characterized in that: An adsorption polishing layer (2) is arranged on the base substrate layer (1), and the thickness ratio between the base substrate layer (1) and the adsorption polishing layer (2) is 1:1-2.

2. A wax-free pad for high-efficiency polishing of silicon wafers according to claim 1, characterized in that: The basic substrate layer (1) comprises the following raw materials in parts by mass: 30-40 parts of modified epoxy resin, 10-30 parts of carbon fiber, 10-20 parts of filler and 20-30 parts of curing agent.

3. A wax-free pad for high-efficiency polishing of silicon wafers according to claim 2, characterized in that: The adsorption polishing layer (2) comprises a base layer (21), a polishing layer (22) and an adsorption layer (23); the base layer (21) is arranged on a base substrate layer (1); the polishing layer (22) is arranged on the base layer (21); a silicon wafer placement groove (221) is provided on the polishing layer (22); and the adsorption layer (23) is arranged in the silicon wafer placement groove (221).

4. A wax-free pad for high-efficiency polishing of silicon wafers according to claim 3, characterized in that: A support reinforcement component (24) is arranged in the base layer (21), and the support reinforcement component (24) comprises a support base column (241) and a reinforcement support rod (242). The support base column (241) is arranged in the base layer (21), and the reinforcement support rods (242) are evenly distributed on the circumferential surface of the support base column (241). The reinforcement support rods (242) are used to enhance the support strength of the base layer (21).

5. A wax-free pad for high-efficiency polishing of silicon wafers according to claim 4, characterized in that: The support base column (241) is connected to the reinforcing support rod (242), and an air inlet (2411) is provided on the support base column (241). The air inlet (2411) is sealed and connected to the base layer (21), and the air inlet (2411) passes through the polishing layer (22).

6. A wax-free pad for high-efficiency polishing of silicon wafers according to claim 5, characterized in that: The reinforcing support rod (242) is located in the base layer (21), and the bottom and top of the reinforcing support rod (242) are both provided with exhaust holes (2421), and the exhaust holes (2421) are distributed at equal intervals.

7. A wax-free pad for high-efficiency polishing of silicon wafers according to claim 6, characterized in that: The polishing layer (22) comprises the following raw materials in parts by mass: 2-10 parts of fluorine-containing polyurethane, 0-4 parts of thermoplastic polyurethane, 1-2 parts of mixed fiber material, 1-3 parts of carboxymethyl cellulose glue, 25-35 parts of abrasive adhesive, 55-70 parts of organic solvent and 0-0.3 parts of auxiliary agent.

8. A wax-free pad for high-efficiency polishing of silicon wafers according to claim 7, characterized in that: The adsorption layer (23) comprises the following raw materials in parts by mass: 2-20 parts of fluorine-containing polyurethane, 1-10 parts of thermoplastic polyurethane, 0-2 parts of zinc oxide, 0-3 parts of activated carbon fiber, 65-95 parts of organic solvent and 0-0.5 parts of auxiliary agent.

9. A production process for a high-efficiency wax-free polishing pad for silicon wafers according to claim 8, characterized in that: The steps include: S1. Production of base substrate layer (1): Adding modified epoxy resin, carbon fiber, filler and curing agent into an extruder, stirring, mixing, plasticizing and compacting in the extruder, extruding a pre-product of a certain shape, and repeatedly extruding and stretching the pre-product through a calender to form a base substrate layer (1) with uniform thickness; S2. Production of adsorption polishing layer (2): A supporting base column (241) and a reinforcing support rod (242) are formed in the base layer (21) so as to be connected to each other, an air inlet (2411) is formed on the supporting base column (241), and an exhaust hole (2421) is formed at the bottom and top of the reinforcing support rod (242); Fluorine-containing polyurethane, thermoplastic polyurethane, mixed fiber material, carboxymethyl cellulose glue, abrasive adhesive, organic solvent and additives are added into an extruder, stirred, mixed, plasticized and compacted by the extruder, and then a pre-product of a certain shape is extruded, and the pre-product is repeatedly extruded and stretched by a calender to form a polishing layer (22) with uniform thickness; Fluorine-containing polyurethane, thermoplastic polyurethane, zinc oxide, activated carbon fiber, organic solvent and additives are added into an extruder, stirred, mixed, plasticized and compacted by the extruder, and then a pre-product of a certain shape is extruded, and the pre-product is repeatedly extruded and stretched by a calender to form an adsorption layer (23) with uniform thickness; A silicon wafer placement groove (221) is machined on the polishing layer (22), and an adsorption layer (23) is machined in the silicon wafer placement groove (221), and the polishing layer (22) is machined on the surface of the base layer (21) to form an adsorption polishing layer (2); S3, production of wax-free pads: The produced adsorption polishing layer (2) is placed on the base substrate layer (1) and, after lamination, a wax-free pad is formed.

Citation Information

Patent Citations

  • Corner-chipping-preventing wax-free pad for wafer polishing and production process of corner-chipping-preventing wax-free pad

    CN115008342A

  • Planar discontinuous shear thickening SiC grinding and polishing integrated polishing device

    CN117020929A

  • Wax-free pad for single-side polishing of semiconductor silicon crystal material and production process of wax-free pad

    CN117067123A

  • Chemical mechanical polishing pad with track supporting structure and application of chemical mechanical polishing pad

    CN117564931A

  • Anti-scratch wax-free pad for polishing

    CN219747606U

Cited By

  • Mechanical polishing pad with CMP (chemical mechanical polishing) composite groove and preparation method of mechanical polishing pad

    CN120480799A

  • A CMP composite groove mechanical polishing pad and its preparation method

    CN120480799B