Hot pressing process for non-expansive ceramic fiber sealing gasket

By optimizing the moisture content and hot pressing parameters of the ceramic fiber sealing liner in the hot pressing process of the ceramic fiber sealing liner, combined with the use of alumina and silicon oxide, the problems of complex process and insufficient sealing performance of the ceramic fiber sealing liner are solved, achieving To achieve higher quality sealing performance and meet stricter emission standards.

CN118769357APending Publication Date: 2024-10-15MOBILE SOURCE SPECIAL FIBER (HENAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410873931.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The process of ceramic fiber sealing liners in the existing technology is complex and cannot diversify the process, and the aging performance and thickness of the sealing liners are not considered, resulting in insufficient sealing performance and inability to meet increasingly stringent emission standards.

Method used

By developing a non-expanding ceramic fiber sealing liner hot pressing process on a traditional hot press, including research and testing of moisture content of ceramic fiber lining blankets, hot pressing by hot press, ceramic fiber blanket cutting process and sample preparation, the process parameters were optimized to To improve the sealing performance, aluminum oxide and silicon oxide are used as the main raw materials, combined with gravity-free stirring and electric melting processing, to form high-quality ceramic fiber wool, and the slurry is made through a beater for hot pressing molding.

Benefits of technology

It achieves high-quality molding of ceramic fiber sealing liners, improves sealing performance, meets more stringent emission standards, increases process diversity, and extends the service life of sealing liners.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118769357A_ABST
    Figure CN118769357A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of mobile machinery discharge, in particular to a non-expansive ceramic fiber sealing gasket hot-pressing process which comprises the following steps: researching and testing the moisture content of a ceramic fiber gasket blanket, hot-pressing by a hot press, cutting the ceramic fiber blanket, preparing a small sample and detecting a product. According to the hot-pressing process for the non-expansive ceramic fiber sealing gasket, new application is achieved on a traditional hot press, and product competitiveness is further improved; through the improvement of the process, the process diversification on the original production line is realized, corresponding process parameters are formed, four samples are taken from each of three ceramic gaskets with different densities, and the water absorption rate determination, hot pressing, cutting and other process treatments are carried out, so that the relationship among the water content, the final hot pressing time and the overall performance can be conveniently obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mobile machinery emission, in particular to a hot pressing process for a non-expanding ceramic fiber sealing gasket. Background Art

[0002] Sealing gaskets are an indispensable key component in automobiles. When the converter is packaged, the gasket must be filled between the shell and the carrier. The performance of the gasket directly affects the working efficiency and service life of the converter. The sealing gasket mainly plays the functions of support, shock absorption, fixation and sealing. At present, ceramic fiber is used as a high-temperature resistant material to produce this gasket both at home and abroad. Non-expanding ceramic fiber sealing gaskets are a sealing material used for high-temperature applications. They are usually made of ceramic fibers and will not expand due to temperature changes. Therefore, they can effectively prevent gas, liquid or solid particles from leaking from the sealing joint. This is essential to ensure the normal operation and safety of the system. The sealing gasket should have a certain compression performance, be able to maintain sealing after being compressed, and not lose the sealing effect due to expansion when the temperature changes. Since the implementation of the National VI standard, the overall tightening has been more than 50% compared with the National V. Without considering the influence of test conditions and test procedures, compared with the "National V" emission standard limit, the limit of carbon monoxide (CO) for gasoline vehicles has been tightened by 50%, hydrocarbons (HC) have been reduced by 50%, and nitrogen oxides (NOx) have been tightened by 42%. The use of non-expanded ceramic fiber sealing gaskets can effectively reduce gas leakage at the sealing joints, improve the sealing performance of the system, and reduce the emission of pollutants. In general, the requirements for sealing gaskets are also gradually increasing.

[0003] Chinese patent with publication number CN101772626A discloses a ceramic fiber sealing gasket based on external slurry sizing and hot pressing process, but the process is relatively complicated and cannot form process diversification; Chinese patent with publication number CN218235220U discloses a sealing gasket for an automobile catalytic converter, but does not consider the aging performance of the sealing gasket and the thickness of the gasket; Chinese patent with publication number CN216732667U discloses a process for preparing a non-metallic sealing gasket, but does not consider the thickness and aging performance of the prepared sealing gasket; Chinese patent with publication number CN104727903A discloses a ceramic fiber sealing gasket and a preparation method thereof, but the process preparation is relatively complicated and needs to be improved. Summary of the invention

[0004] The object of the present invention is to provide a hot pressing process for a non-expanding ceramic fiber sealing gasket to solve the problems raised in the above-mentioned background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: a hot pressing process for a non-expandable ceramic fiber sealing gasket, comprising the following steps: S1. Research and test on moisture content of ceramic fiber blanket The moisture content of the undried ceramic fiber embryo is relatively high. It is necessary to repeatedly test and study to determine the relationship between the moisture content and the final hot pressing time and the overall performance. The moisture content of the liner is determined by experiment. The test steps are as follows: S1.1 Sampling Samples were randomly selected from ceramic fiber blankets of different densities or batches. Four samples were taken from each of the three ceramic blankets with different densities, referring to the method used in the study on the influence of ceramic blankets on the performance of CO2 single-sided welding.

[0006] S1.2 Initial weight determination The selected samples were placed in an oven for drying. The oven temperature was set to 200°C and kept warm for 2-3 hours.

[0007] The sample was removed from the oven and placed in a desiccator to cool to room temperature.

[0008] Take out the samples from the dryer, number each sample, and use a high-precision electronic balance to weigh the initial mass of the sample and make a detailed record, which is recorded as m. 1 , and so on, four samples with different densities are processed.

[0009] S1.3 Determination of water absorption Put the weighed sample into water for water absorption test. The boiling method can be used for experimental treatment. After boiling, take out the sample and cool it to room temperature.

[0010] Weigh the sample after absorbing water and record its mass, recorded as m 2 , the same four samples need to be processed.

[0011] S1.4 Calculation of moisture content According to the mass change before and after water absorption, the moisture content of the ceramic fiber blanket is calculated. The moisture content calculation formula is: Moisture content = (m 2 -m 1 ) / m 1 ×100%).

[0012] S1.5 Recording and Analysis The experimental data, including the initial mass of the sample, the mass after water absorption, and the moisture content, were sorted out, and data tables and charts were prepared. Then, the data were analyzed to understand the variation pattern of the moisture content of the ceramic fiber blanket under different conditions, as well as the influence of the moisture content on the material properties.

[0013] S2, hot press The hot pressing parameters of the hot press machine were set, and four ceramic liner samples with calculated moisture contents were hot pressed using the hot press machine and labeled.

[0014] S3. Ceramic fiber blanket cutting process The wet ceramic fiber blanket needs to be transferred, extracted after drying, and the hot pressing performance needs to be guaranteed.

[0015] S3.1 Preparation stage: Keep cutting equipment and work area clean and tidy to avoid introducing impurities and contaminants during the transfer process.

[0016] Prepare necessary tools and auxiliary equipment, including cutting knives, transfer boards, and gloves.

[0017] S3.2 Cutting operation: Use professional cutting equipment to cut the wet ceramic fiber blanket to ensure that the cutting operation is accurate and fast to reduce the time the wet blanket is exposed to the air. Pay attention to the integrity of the wet blanket during the cutting process to avoid excessive fragments or damage.

[0018] S3.3 Wet embryo transfer: Use a smooth, dry transfer board and tray to carry the cut green blanks, which can support the weight of the green blanks and maintain their shape. Gently remove the green blanks from the cutting equipment and place them on the transfer board and tray.

[0019] S4. Small sample preparation S4.1 Material selection Alumina and silicon oxide are selected as main raw materials and are mixed according to weight percentages of 42% to 53% and 47% to 58%.

[0020] S4.2 Preparation of small samples The raw materials are added into a gravity-free mixer in a certain proportion, the stirring rate is set to 90-170 rpm, the stirring time is 10-30 minutes, and the raw materials are fully mixed. The mixed raw materials are added into an electric melting furnace for electric melting treatment to obtain mixed raw materials in a molten state, and the mixed raw materials in a molten state are dropped onto a spinning roller of a spinning machine. The spinning roller spins the molten material into fibers under high-speed rotation, and the fibers are collected into a cotton collector by an induced draft fan to obtain layered fiber cotton, which is transported to a heating furnace for heat treatment to obtain ceramic fiber cotton, and the ceramic fiber cotton after heat treatment is made into slurry by a pulping machine.

[0021] S5. Product testing After obtaining a suitable gasket sample, a bench test is performed to confirm that the performance of the product meets the process requirements. Preferably, the parameters set for the hot press in step S2 are as follows: Pressure range: The hot press machine selects 10T, 20T and 50T hot press machines for hot pressing, and controls the pressure accuracy within ±0.5T, which helps to ensure uniform pressure and high-quality molding of the liner.

[0022] Holding pressure: After hot pressing is completed, a holding time is required to maintain a certain pressure to prevent the workpiece from loosening during cooling. The holding time is set to 10s.

[0023] Preferably, in step S3.3, when the wet embryo needs to be moved to another location, forklift and cart auxiliary equipment can be used. During the movement, it is necessary to ensure that the transfer plate or pallet is stably and firmly fixed on the auxiliary equipment to prevent the wet embryo from slipping or being damaged.

[0024] Preferably, in step S4.2, when the heat-treated ceramic fiber cotton is made into slurry using a pulping machine, the slag balls in the fibers can be separated by a sedimentation method to obtain fibers with a fiber index of 70% to 95% and dry them, and then binders and additives are added to the dried fibers in proportion to form a final sample slurry.

[0025] Preferably, the accuracy of the electro-optical balance in step S1.2 is 0.0001 g.

[0026] Compared with the prior art, the present invention has the following beneficial effects: 1. The hot pressing process of the non-expanding ceramic fiber sealing gasket further improves product competitiveness by realizing new applications on traditional hot presses; and through process improvements, it achieves process diversification on the original production line and forms corresponding process parameters.

[0027] 2. The hot pressing process of the non-expanding ceramic fiber sealing gasket randomly selects samples from ceramic fiber gasket blankets of different densities or different batches, refers to the method in the study of the influence of ceramic gaskets on the performance of CO2 single-sided welding seams, takes four samples from each of the three ceramic gaskets with different densities, and conducts water absorption measurement, hot pressing and cutting and other process treatments, which can easily derive the relationship between water content and the final hot pressing time and overall performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.

[0029] Figure 1 This is a comparison chart of the optimization of hot pressing process for ceramic fiber liner molding; Figure 2 This is the process flow chart of hot pressing for ceramic fiber liner molding. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0031] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0032] See also Figure 1-2 , the present invention provides the following technical solutions: A hot pressing process for a non-expandable ceramic fiber sealing liner comprises the following steps: S1. Research and test on moisture content of ceramic fiber blanket The moisture content of the undried ceramic fiber embryo is relatively high. It is necessary to repeatedly test and study to determine the relationship between the moisture content and the final hot pressing time and the overall performance. The moisture content of the liner is determined by experiment. The test steps are as follows: S1.1 Sampling Samples were randomly selected from ceramic fiber blankets of different densities or batches. Four samples were taken from each of the three ceramic blankets with different densities, referring to the method used in the study on the influence of ceramic blankets on the performance of CO2 single-sided welding.

[0033] S1.2 Initial weight determination The selected samples were placed in an oven for drying. The oven temperature was set to 200°C and kept warm for 2-3 hours.

[0034] The sample was removed from the oven and placed in a desiccator to cool to room temperature.

[0035] Take out the samples from the dryer, number each sample, and use a high-precision electronic balance to weigh the initial mass of the sample and make a detailed record, which is recorded as m. 1 , and so on, for four samples with different densities, the accuracy of the electro-optical balance is 0.0001g.

[0036] S1.3 Determination of water absorption Put the weighed sample into water for water absorption test. The boiling method can be used for experimental treatment. After boiling, take out the sample and cool it to room temperature.

[0037] Weigh the sample after absorbing water and record its mass, recorded as m 2 , the same four samples need to be processed.

[0038] S1.4 Calculation of moisture content According to the mass change before and after water absorption, the moisture content of the ceramic fiber blanket is calculated. The moisture content calculation formula is: Moisture content = (m 2 -m 1 ) / m 1 ×100%).

[0039] S1.5 Recording and Analysis The experimental data, including the initial mass of the sample, the mass after water absorption, and the moisture content, were sorted out, and data tables and charts were prepared. Then, the data were analyzed to understand the variation pattern of the moisture content of the ceramic fiber blanket under different conditions, as well as the influence of the moisture content on the material properties.

[0040] S2, hot press The hot pressing parameters of the hot press machine were set, and four ceramic liner samples with calculated moisture contents were hot pressed using the hot press machine and labeled.

[0041] The parameters of the heat press setting are as follows: Pressure range: The hot press machine selects 10T, 20T and 50T hot press machines for hot pressing, and controls the pressure accuracy within ±0.5T, which helps to ensure uniform pressure and high-quality molding of the liner.

[0042] Holding pressure: After hot pressing is completed, a holding time is required to maintain a certain pressure to prevent the workpiece from loosening during cooling. The holding time is set to 10s.

[0043] S3. Ceramic fiber blanket cutting process The wet ceramic fiber blanket needs to be transferred, extracted after drying, and the hot pressing performance needs to be guaranteed.

[0044] S3.1 Preparation stage: Keep cutting equipment and work area clean and tidy to avoid introducing impurities and contaminants during the transfer process.

[0045] Prepare necessary tools and auxiliary equipment, including cutting knives, transfer boards, and gloves.

[0046] S3.2 Cutting operation: Use professional cutting equipment to cut the wet ceramic fiber blanket to ensure that the cutting operation is accurate and fast to reduce the time the wet blanket is exposed to the air. Pay attention to the integrity of the wet blanket during the cutting process to avoid excessive fragments or damage.

[0047] S3.3 Wet embryo transfer: Use smooth, dry transfer boards and pallets to carry the cut wet embryos. They should be able to support the weight of the wet embryos and maintain their shape. Gently remove the wet embryos from the cutting equipment and place them on the transfer boards and pallets. When the wet embryos need to be moved to another location, forklifts and carts can be used as auxiliary equipment. During the move, ensure that the transfer board or pallet is stably and firmly fixed to the auxiliary equipment to prevent the wet embryos from slipping or being damaged.

[0048] S4. Small sample preparation S4.1 Material selection Alumina and silicon oxide are selected as main raw materials and are mixed according to weight percentages of 42% to 53% and 47% to 58%.

[0049] S4.2 Preparation of small samples The raw materials are added into a gravity-free mixer in a certain proportion, the stirring rate is set to 90-170 rpm, the stirring time is 10-30 minutes, and the raw materials are fully mixed. The mixed raw materials are added into an electric melting furnace for electric melting treatment to obtain mixed raw materials in a molten state. The mixed raw materials in a molten state are dropped onto the spinning roller of a spinning machine. The spinning roller spins the molten material into fibers under high-speed rotation. The fibers are collected into a cotton collector by an induced draft fan to obtain layered fiber cotton. The fiber cotton is transported to a heating furnace for heat treatment to obtain ceramic fiber cotton. The heat-treated ceramic fiber cotton is made into slurry using a pulping machine, and then the slag balls in the fibers can be separated by a sedimentation method to obtain fibers with a fiber index of 70%-95% and dried. The dried fibers are added with binders and additives in proportion to form a final sample slurry.

[0050] S5. Product testing After obtaining suitable gasket samples, bench tests are carried out to confirm that the product performance meets the process requirements.

[0051] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A hot pressing process for a non-expandable ceramic fiber sealing gasket, characterized in that: The following steps are involved: S1. Research and test on moisture content of ceramic fiber blanket The moisture content of the undried ceramic fiber embryo is relatively high. It is necessary to repeatedly test and study to determine the relationship between the moisture content and the final hot pressing time and the overall performance. The moisture content of the liner is determined by experiment. The test steps are as follows: S1.1 Sampling Samples were randomly selected from ceramic fiber blankets of different densities or batches. Four samples were taken from each of the three ceramic blankets with different densities, referring to the method used in the study on the effect of ceramic blankets on the performance of CO2 single-sided welding. S1.2 Initial weight determination Place the selected samples in an oven for drying. Set the oven temperature to 200°C and keep it warm for 2-3 hours. Take the sample out of the oven and place it in a desiccator to cool to room temperature; Take out the samples from the dryer, number each sample, and use a high-precision electronic balance to weigh the initial mass of the sample and make a detailed record, which is recorded as m1. Repeat this process for four samples with different densities. S1.3 Determination of water absorption Put the weighed sample into water for water absorption test. The boiling method can be used for experimental treatment. After boiling, take out the sample and cool it to room temperature. Weigh the sample after absorbing water and record its mass, which is recorded as m2. The same treatment is required for the four samples; S1.4 Calculation of moisture content According to the mass change before and after water absorption, the moisture content of the ceramic fiber blanket is calculated. The moisture content calculation formula is: moisture content = (m2-m1) / m1×100%); S1.5 Recording and Analysis Organize the experimental data, including the initial mass, mass after water absorption, and moisture content of the sample, and make data tables and charts. Then analyze the data to understand the changing rules of the moisture content of the ceramic fiber blanket under different conditions, and the influence of moisture content on material properties; S2, hot press The hot pressing parameters of the hot press machine were set, and four ceramic liner samples with calculated moisture contents were hot pressed by the hot press machine, and then numbered; S3. Ceramic fiber blanket cutting process The wet ceramic fiber blanket needs to be transferred, extracted after drying, and the hot pressing performance needs to be guaranteed; S3.1 Preparation stage: Ensure cutting equipment and work area are clean and tidy to avoid the introduction of impurities and contaminants during the transfer process; Prepare necessary tools and auxiliary equipment, including cutting knives, transfer boards, and gloves; S3.2 Cutting operation: Use professional cutting equipment to cut the wet ceramic fiber blanket, ensure that the cutting operation is accurate and fast to reduce the time the wet blanket is exposed to the air, pay attention to the integrity of the wet blanket during the cutting process, and avoid excessive fragments or damage; S3.3 Wet embryo transfer: Use smooth, dry transfer boards and trays to carry the cut wet embryos, which can support the weight of the wet embryos and maintain their shape. Gently remove the wet embryos from the cutting equipment and place them on the transfer boards and trays; S4. Small sample preparation S4.1 Material selection Alumina and silicon oxide are selected as main raw materials and mixed according to weight percentages of 42% to 53% and 47% to 58%; S4.2 Preparation of small samples The raw materials are added into a zero-gravity mixer in a certain proportion, the stirring rate is set to 90-170 rpm, the stirring time is 10-30 minutes, and the raw materials are fully mixed. The mixed raw materials are added into an electric melting furnace for electric melting treatment to obtain a mixed raw material in a molten state, and the mixed raw materials in a molten state are dropped onto a spinning roller of a spinning machine. The spinning roller spins the molten material into fibers under high-speed rotation, and the fibers are collected into a cotton collector by an induced draft fan to obtain layered fiber cotton, and the fiber cotton is transported to a heating furnace for heat treatment to obtain ceramic fiber cotton, and the ceramic fiber cotton after heat treatment is made into slurry by a pulping machine; S5. Product testing After obtaining suitable gasket samples, bench tests are carried out to confirm that the product performance meets the process requirements.

2. The hot pressing process of a non-expandable ceramic fiber sealing gasket according to claim 1, characterized in that: The parameters of the hot press in step S2 are as follows: Pressure range: The hot press machine selects 10T, 20T and 50T hot press machines for hot pressing, and controls the pressure accuracy within ±0.5T, which helps to ensure uniform pressure and high-quality molding of the liner; Holding pressure: After hot pressing is completed, a holding time is required to maintain a certain pressure to prevent the workpiece from loosening during cooling. The holding time is set to 10s.

3. The hot pressing process of a non-expandable ceramic fiber sealing gasket according to claim 2, characterized in that: When the wet embryo needs to be moved to another location in step S3.3, forklift and cart auxiliary equipment can be used. During the moving process, it is necessary to ensure that the transfer plate or pallet is stably and firmly fixed on the auxiliary equipment to prevent the wet embryo from slipping or being damaged.

4. The hot pressing process of a non-expandable ceramic fiber sealing gasket according to claim 3 is characterized in that: In step S4.2, when the heat-treated ceramic fiber cotton is made into slurry using a pulping machine, the slag balls in the fibers can be separated by a sedimentation method to obtain fibers with a fiber index of 70% to 95% and dry them, and binders and additives are added to the dried fibers in proportion to form a final sample slurry.

5. The hot pressing process of a non-expandable ceramic fiber sealing gasket according to claim 4, characterized in that: The accuracy of the electro-optical balance in step S1.2 is 0.0001 g.