Method for removing inclusions in iron tailing roughing quartz particles

Through roasting water quenching, fine grinding, magnetic separation and three-stage cyclic acid leaching process, the problem of hematite and quartz conjoined during the separation and purification process of quartz resources in iron tailings was solved, and high-purity quartz sand was prepared and reduced It reduces acid consumption and operating costs, and solves the pollution and high cost problems in the existing technology.

CN118771389APending Publication Date: 2024-10-15ANSTEEL BEIJING RES INST CO LTD +1

Patent Information

Application Number
CN202410785789.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In the existing technology, during the separation and purification process of quartz resources in iron tailings, hematite and quartz are seriously connected, which makes it difficult to separate by multi-stage flotation or magnetic separation combined process, consumes a lot of acid, and has high operating costs, and chemical acid leaching is harmful to The removal effect of gas-liquid inclusions is not good, and common processes require the addition of chemical reagents, which are costly and pollute the environment.

Method used

Using roasting water quenching, fine grinding, magnetic separation, microwave roasting and three-stage cyclic acid leaching process, the mineral inclusions in the quartz particles are removed through roasting and water quenching, and a superconducting high gradient magnetic separator is used for mineral removal, combining the three stages Cyclic acid leaching removes gas-liquid inclusions to form high-purity quartz sand.

Benefits of technology

It achieves deep removal of mineral inclusions inside quartz particles, reduces chemical leaching acid consumption, reduces operating costs, improves the purity of quartz particles, reaches SiO2 content ≥ 99.9%, meets the standards for refined quartz sand, and achieves high value for iron tailings ization and resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771389A_ABST
    Figure CN118771389A_ABST
Patent Text Reader

Abstract

The invention discloses a method for removing inclusions in hematite tailing roughing quartz particles, which comprises the following steps: S1, roasting and water quenching: roasting the hematite tailing roughing quartz particles at 650-700 DEG C for 2-5 hours, and then carrying out water quenching; s2, grinding: grinding the quartz particles subjected to water quenching in the step S1 to 500-400 meshes; s3, magnetic separation: removing mineral inclusion in the quartz particles obtained in the step S2 through a superconducting high-gradient magnetic separator; s4, roasting: roasting the quartz particles obtained in the step S3 at 1000-1250 DEG C for 2-5 hours, then cooling, roasting at 750-1000 DEG C for 4-5 hours, and repeating the step 3-5 times; and S5, acid leaching: performing three-section circulating acid leaching on the quartz particles obtained in the step S4 to remove minerals and gas-liquid inclusions in the quartz particles so as to obtain the high-purity quartz sand. The grade of SiO2 in the prepared high-purity quartz is up to 99.9% or above, the standard of refined quartz sand is met, and the purposes of high-valued and resource utilization of the hematite tailings are effectively achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of recycling of solid waste resources, and in particular relates to a method for removing internal inclusions of rough quartz particles in iron tailings. Background Art

[0002] Iron tailings contain abundant valuable elements, among which SiO2 content is as high as 70% or more, and is a valuable quartz resource. How to effectively separate, purify and recycle the quartz resources in iron tailings and realize high added value of iron tailings is a major issue faced by enterprises.

[0003] In response to the above needs, researchers have successively developed multi-stage flotation, magnetic separation-flotation combination, chemical leaching, high-temperature calcination and other technologies for the preparation of high-purity quartz from iron tailings. Due to the serious intergrowth of hematite and quartz in iron tailings, and the large amount of hematite and gas-liquid inclusions wrapped inside the quartz particles, it is difficult to separate them from the quartz particles by multi-stage flotation or magnetic separation-flotation combination processes, resulting in large acid consumption and high operating costs in the back-end chemical leaching process. In addition, chemical acid leaching has little effect on the removal of gas-liquid inclusions in quartz particles. At present, the removal of gas-liquid inclusions in quartz particles is mainly achieved through the process of ammonium nitrate solution soaking-drying-water quenching, but this process requires the addition of chemical reagents, which is costly, easy to produce wastewater, and pollute the environment. Summary of the invention

[0004] The present invention provides a method for removing inclusions inside rough quartz particles in iron tailings, which overcomes the shortcomings of the prior art such as complex process, large acid consumption and high operating cost. Aiming at the serious problems of quartz ore intergrowth in hematite tailings and complex and difficult-to-treat inclusions in quartz particles, the method realizes the removal of inclusions in rough quartz particles in hematite tailings and the preparation of high-purity quartz through roasting water quenching, fine grinding, magnetic separation, microwave roasting and three-stage circulating acid leaching process.

[0005] In order to achieve the above object, the technical solution of the present invention is as follows:

[0006] The present invention provides a method for removing internal inclusions of roughing quartz particles in hematite tailings, the method comprising the following steps:

[0007] S1: Calcination and water quenching: The rough quartz particles of hematite tailings are calcined at 650-700°C for 2-5h, and then water quenched;

[0008] S2: Grinding: Grinding the quartz particles after water quenching in step S1 to 500-400 mesh;

[0009] S3: Magnetic separation: removing mineral inclusions from the quartz particles obtained in step S2 by a superconducting high gradient magnetic separator;

[0010] S4: calcining: calcining the quartz particles obtained in step S3 at 1000-1250°C for 2-5h, then cooling, and then calcining at 750-1000°C for 4-5h, and repeating this step 3-5 times;

[0011] S5: acid leaching: subjecting the quartz particles obtained in step S4 to three-stage acid leaching to remove minerals and gas-liquid inclusions in the quartz particles to obtain high-purity quartz sand;

[0012] The three-stage cycle acid leaching process is:

[0013] After the first-stage acid leaching reaction, a first-stage acid leaching liquid and a first-stage leaching residue are obtained by separation; after the second-stage acid leaching reaction, a second-stage acid leaching liquid and a second-stage leaching residue are obtained by separation; after the third-stage acid leaching reaction, a third-stage acid leaching liquid and a third-stage leaching residue are obtained by separation;

[0014] The first-stage acid leaching solution is used to adjust the pH value of hematite tailings flotation, the second-stage acid leaching solution is mixed with quartz particles for first-stage acid leaching, the third-stage acid leaching solution is mixed with the first-stage leaching residue for second-stage acid leaching, and the new acid solution is mixed with the second-stage acid leaching residue for third-stage acid leaching.

[0015] In the above technical solution, further, in step S1, the SiO2 content of the rough quartz particles of the hematite tailings is greater than 95%.

[0016] In the above technical solution, further, in step S3, the magnetic field gradient of the superconducting high gradient magnetic separator is 2.5-4.5T.

[0017] In the above technical solution, further, in step S5, the new acid solution is a mixed acid of hydrochloric acid and sulfuric acid, wherein the volume ratio of hydrochloric acid to sulfuric acid is 1:1, and the liquid-solid ratio is 4:1 to 9:1.

[0018] In the above technical solution, further, in step S5, the reaction temperature of the three-stage cycle acid leaching is 60-90° C., and the reaction time is 3-9 hours.

[0019] In the above technical solution, further, the SiO2 content in the high-purity quartz sand is ≥99.9%.

[0020] The acid leaching process of the present invention can improve the acid leaching effect by means of vibration or microwave assistance, and the vibration or microwave assistance is carried out in a manner well known in the art.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1) The present invention adopts roasting-water quenching-fine grinding-strong magnetic separation to dissociate and strongly magnetically remove the intergrowths and inclusions in the rough quartz particles of the hematite tailings, which can not only deeply remove the mineral inclusions inside the quartz particles by physical means and reduce the acid consumption of the rear-end chemical leaching, but also the fine grinding can increase the specific surface area of ​​the quartz particles and the acid leaching solution and reduce the acid leaching time.

[0023] 2) The SiO2 content in the high-purity quartz prepared by the present invention is as high as 99.9% or more, which meets the standard of refined quartz sand and effectively realizes the purpose of high value and resource utilization of hematite tailings. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a schematic diagram of the three-stage cycle acid leaching process. DETAILED DESCRIPTION

[0025] The present invention is further described below in conjunction with specific examples, but the present invention is not limited in any way. The following example is taken for the roughing of quartz particles from Anshan-type hematite tailings, and the following experimental process is described to gradually purify and finally obtain a high-purity quartz product with a SiO2 content of not less than 99.9%. The chemical composition of the raw materials in Examples 1-3 is shown in Table 1.

[0026] Table 1 Chemical composition of quartz particles (wt%)

[0027]

[0028] Example 1

[0029] S1: Calcination and water quenching: The quartz particles obtained from the rough selection of hematite tailings were calcined at 700 °C for 2 h and then water quenched;

[0030] S2: Grinding: Grinding the quartz particles after water quenching in step S1 to 500-400 meshes, so that the mineral inclusions in the quartz particles are separated from the quartz particles;

[0031] S3: Magnetic separation: The impurity minerals dissociated from the quartz particles are separated by a superconducting high gradient magnetic separator to reduce the amount of mixed acid for subsequent fine purification; the magnetic field gradient of the superconducting high gradient magnetic separator is 2.5T;

[0032] S4: calcining: the fine-grained quartz particles obtained in step S3 are calcined at 1250°C for 5 hours, cooled, and then calcined at 750°C for 5 hours; this step is repeated 5 times to remove the gas-liquid inclusions in the fine-grained quartz particles;

[0033] S5: acid leaching: finely purifying the fine-grained quartz particles obtained in step S4 through three-stage circulating acid leaching to deeply remove minerals and gas-liquid inclusions in the quartz particles;

[0034] The three-stage cycle acid leaching process is as follows: after the first stage acid leaching reaction, a first stage acid leaching solution and a first stage leaching residue are obtained; after the second stage acid leaching reaction, a second stage acid leaching solution and a second stage leaching residue are obtained; after the third stage acid leaching reaction, a third stage acid leaching solution and a third stage leaching residue are obtained;

[0035] The first-stage acid leaching solution is used to adjust the pH of hematite tailings flotation, the second-stage acid leaching solution is mixed with quartz particles for first-stage acid leaching, the third-stage acid leaching solution is mixed with the first-stage leaching residue for second-stage acid leaching, and the new acid solution is mixed with the second-stage acid leaching residue for third-stage acid leaching;

[0036] In the three-stage cycle acid leaching process, the new acid solution is a mixed acid of hydrochloric acid and sulfuric acid, wherein the volume ratio of hydrochloric acid to sulfuric acid is 1:1, the liquid-solid ratio is 4:1, the reaction temperature is 80°C, and the reaction time is 6h;

[0037] The SiO2 content in the high-purity quartz sand obtained in Example 1 is ≥99.911%.

[0038] Example 2

[0039] S1: Calcination and water quenching: The quartz particles obtained from the rough selection of hematite tailings were calcined at 650 °C for 5 h and then water quenched;

[0040] S2: Grinding: Grinding the quartz particles after water quenching in step S1 to 500-400 meshes, so that the mineral inclusions in the quartz particles are separated from the quartz particles;

[0041] S3: Magnetic separation: The impurity minerals dissociated from the quartz particles are separated by a superconducting high gradient magnetic separator to reduce the amount of mixed acid for subsequent fine purification; the magnetic field gradient of the superconducting high gradient magnetic separator is 4.5T;

[0042] S4: calcining: calcining the fine-grained quartz particles obtained in step S3 at 1000°C for 2 hours, cooling, and then calcining at 1000°C for 4 hours; this step is repeated 3 times to remove the gas-liquid inclusions in the fine-grained quartz particles;

[0043] S5: acid leaching: finely purifying the fine-grained quartz particles obtained in step S4 through three-stage circulating acid leaching to deeply remove minerals and gas-liquid inclusions in the quartz particles;

[0044] The three-stage cycle acid leaching process is as follows: after the first stage acid leaching reaction, a first stage acid leaching solution and a first stage leaching residue are obtained; after the second stage acid leaching reaction, a second stage acid leaching solution and a second stage leaching residue are obtained; after the third stage acid leaching reaction, a third stage acid leaching solution and a third stage leaching residue are obtained;

[0045] The first-stage acid leaching solution is used to adjust the pH of hematite tailings flotation, the second-stage acid leaching solution is mixed with quartz particles for first-stage acid leaching, the third-stage acid leaching solution is mixed with the first-stage leaching residue for second-stage acid leaching, and the new acid solution is mixed with the second-stage acid leaching residue for third-stage acid leaching;

[0046] In the three-stage cycle acid leaching process, the new acid solution is a mixed acid of hydrochloric acid and sulfuric acid, in which the volume ratio of hydrochloric acid to sulfuric acid is 1:1, the liquid-solid ratio is 7:1, the reaction temperature is 80°C, and the reaction time is 7h.

[0047] The SiO2 content in the high-purity quartz sand finally obtained is ≥99.929%.

[0048] Example 3

[0049] S1: Calcination and water quenching: The quartz particles obtained from the rough selection of hematite tailings were calcined at 680 °C for 3 h and then water quenched;

[0050] S2: Grinding: Grinding the quartz particles after water quenching in step S1 to 500-400 meshes, so that the mineral inclusions in the quartz particles are separated from the quartz particles;

[0051] S3: Magnetic separation: The impurity minerals dissociated from the quartz particles are separated by a superconducting high gradient magnetic separator to reduce the amount of mixed acid for subsequent fine purification; the magnetic field gradient of the superconducting high gradient magnetic separator is 3T;

[0052] S4: calcining: the fine-grained quartz particles obtained in step S3 are calcined at 1100°C for 4 hours, cooled, and then calcined at 900°C for 4.5 hours; this step is repeated 4 times to remove the gas-liquid inclusions in the fine-grained quartz particles;

[0053] S5: acid leaching: finely purifying the fine-grained quartz particles obtained in step S4 through three-stage circulating acid leaching to deeply remove minerals and gas-liquid inclusions in the quartz particles;

[0054] The three-stage cycle acid leaching process is as follows: after the first stage acid leaching reaction, a first stage acid leaching solution and a first stage leaching residue are obtained; after the second stage acid leaching reaction, a second stage acid leaching solution and a second stage leaching residue are obtained; after the third stage acid leaching reaction, a third stage acid leaching solution and a third stage leaching residue are obtained;

[0055] The first-stage acid leaching solution is used to adjust the pH of hematite tailings flotation, the second-stage acid leaching solution is mixed with quartz particles for first-stage acid leaching, the third-stage acid leaching solution is mixed with the first-stage leaching residue for second-stage acid leaching, and the new acid solution is mixed with the second-stage acid leaching residue for third-stage acid leaching;

[0056] In the three-stage circulating acid leaching process, the new acid solution is a mixed acid of hydrochloric acid and sulfuric acid, in which the volume ratio of hydrochloric acid to sulfuric acid is 1:1, the liquid-solid ratio is 7:1, the reaction temperature is 70°C, and the reaction time is 6h.

[0057] The SiO2 content in the high-purity quartz sand finally obtained is ≥99.904%.

[0058] For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments with equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should still fall within the scope of protection of the technical solution of the present invention.

Claims

1. A method for removing internal inclusions in roughing quartz particles of hematite tailings, characterized in that: The method comprises the following steps: S1: Calcination and water quenching: The rough quartz particles of hematite tailings are calcined at 650-700°C for 2-5h, and then water quenched; S2: Grinding: Grinding the quartz particles after water quenching in step S1 to 500-400 mesh; S3: Magnetic separation: removing mineral inclusions from the quartz particles obtained in step S2 by a superconducting high gradient magnetic separator; S4: calcining: calcining the quartz particles obtained in step S3 at 1000-1250°C for 2-5h, then cooling, and then calcining at 750-1000°C for 4-5h, and repeating this step 3-5 times; S5: acid leaching: subjecting the quartz particles obtained in step S4 to three-stage acid leaching to remove minerals and gas-liquid inclusions in the quartz particles to obtain high-purity quartz sand; The three-stage cycle acid leaching process is: After the first-stage acid leaching reaction, a first-stage acid leaching liquid and a first-stage leaching residue are obtained by separation; after the second-stage acid leaching reaction, a second-stage acid leaching liquid and a second-stage leaching residue are obtained by separation; after the third-stage acid leaching reaction, a third-stage acid leaching liquid and a third-stage leaching residue are obtained by separation; The first-stage acid leaching solution is used to adjust the pH value of hematite tailings flotation, the second-stage acid leaching solution is mixed with quartz particles for first-stage acid leaching, the third-stage acid leaching solution is mixed with the first-stage leaching residue for second-stage acid leaching, and the new acid solution is mixed with the second-stage acid leaching residue for third-stage acid leaching.

2. The method for removing internal inclusions of roughing quartz particles in hematite tailings according to claim 1, characterized in that: In step S1, the SiO2 content of the rough quartz particles in the hematite tailings is greater than 95%.

3. The method for removing internal inclusions of roughing quartz particles in hematite tailings according to claim 1, characterized in that: In step S3, the magnetic field gradient of the superconducting high gradient magnetic separator is 2.5-4.5T.

4. The method for removing internal inclusions of roughing quartz particles in hematite tailings according to claim 1, characterized in that: In step S5, the new acid solution is a mixed acid of hydrochloric acid and sulfuric acid, wherein the volume ratio of hydrochloric acid to sulfuric acid is 1:1, and the liquid-solid ratio is 4:1-9:

1.

5. The method for removing internal inclusions of roughing quartz particles in hematite tailings according to claim 1, characterized in that: In step S5, the reaction temperature of the three-stage cyclic acid leaching is 60-90° C., and the reaction time is 3-9 hours.

6. The method for removing internal inclusions of roughing quartz particles in hematite tailings according to claim 1, characterized in that: The SiO2 content in the high-purity quartz sand is ≥99.9%.

Citation Information

Patent Citations

  • Method for extracting vanadium from stone coal containing vanadium

    CN103421963A

  • Method for preparing high-purity quartz sand from vein quartz ore

    CN106064819A

  • Purification method of high purity quartz sand tailings

    CN110510620A

  • Method for gradient resource utilization of low-temperature Bayer process red mud

    CN115478165A

  • Method for preparing 4N8-grade high-purity quartz sand from pegmatite quartz

    CN117623320A

Cited By

  • Method for preparing quartz sand based on iron tailings

    CN122789401A