Preparation method of high-purity silicon dioxide aerogel and obtained silicon dioxide aerogel

The silica aerogel is prepared by using an inorganic silicon source and an acidic catalyst, and the reverse micelle extraction solution is used for drying under normal pressure, which solves the problems of high preparation cost and many impurities in the existing technology, and obtains high purity, low density and Silica airgel with excellent thermal insulation properties.

CN118771394APending Publication Date: 2024-10-15HUANGSHAN HUIZHOU JIAJIE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410974288.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing preparation methods of silica aerogels have problems such as limited production capacity of organic silicon sources, expensive raw materials, high production costs, high impurities in water glass, and complex supercritical drying process equipment and high costs, making it difficult to meet the needs of industrialization and industrialization. application requirements.

Method used

A wet gel is prepared by mixing an inorganic silicon source, deionized water and an acidic catalyst, and then a surface modifier and a non-polar solvent are added to form a reverse micelle extraction solution. High-purity silica aerogel is obtained by drying under normal pressure. Oxazolidinone derivatives serve as surface modifiers to form a spatial network structure to reduce density and increase specific surface area.

Benefits of technology

Silica aerogels that achieve low cost, low density, high specific surface area and excellent thermal insulation properties reduce production costs, simplify the process flow, and improve the purity and thermal insulation properties of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a preparation method of high-purity silicon dioxide aerogel and the obtained silicon dioxide aerogel, and belongs to the technical field of aerogel. The invention relates to a preparation method of high-purity silicon dioxide aerogel, which comprises the following steps of: preparing silicon dioxide aerogel by adopting an acid catalysis one-step gel method, modifying silicon dioxide by adopting a surface modifier, and finally performing reverse micelle extraction to avoid a tedious solvent alicyclic process, simplify the process and improve the production efficiency. The obtained silicon dioxide aerogel is high in purity, large in specific surface area, low in density and good in heat transfer performance, and can be widely applied to the fields of building heat insulation, aerospace, heat pipeline heat preservation, electronic equipment heat preservation and heat insulation and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aerogels, and in particular to a method for preparing high-purity silica aerogel and the obtained silica aerogel. Background Art

[0002] Aerogel is a type of three-dimensional nanoporous solid material. Its structure is formed by the interaction of colloidal particles or polymer molecules, and the pores are filled with gaseous dispersion medium. It has the characteristics of ultra-lightness, low density, nano-micropores, etc. It is the world's lowest density solid material and is called "solidified smoke". Kistle first prepared it through supercritical drying technology in 1931. Although it has undergone more than 90 years of research and development, various types of aerogel materials have been formed, such as oxide aerogel, organic aerogel, carbide aerogel, etc., but silica aerogel is still the one that can be industrialized and has broad application prospects. Silica aerogel has shown important application value in the fields of building insulation, heat insulation, catalysis, aerospace, etc., especially in the field of heat insulation, based on silica aerogel powder materials, composite materials such as aerogel coatings, aerogel felts, aerogel boards, and aerogel special-shaped parts that can be used in industry have been developed.

[0003] Silica aerogel is a new type of inorganic nano thermal insulation material. It is a nanoporous network structure composed of nano-scale particles. It has a low density (as low as 3kg / m 3 ), high porosity (up to 99.8%), high specific surface area (up to 1000m 2 / g) and low thermal conductivity (thermal conductivity at room temperature is as low as 0.015W / m•K), making it the material with the best thermal insulation performance to date. It is widely used in aerospace, communications, medical, building materials and other fields, including steam pipe insulation.

[0004] Although SiO2 aerogel has excellent performance, its preparation method still has certain shortcomings, especially the industrial preparation of SiO2 aerogel still has certain problems. For example, the silicon sources currently used in the preparation of SiO2 aerogel are mostly organic silicon sources such as ethyl orthosilicate, methyl orthosilicate, and polysiloxane. The price of organic silicon sources is relatively expensive, and the price fluctuates greatly. The production capacity is greatly affected by the single crystal silicon industry; and the organic silane modifiers used, such as trimethylchlorosilane and hexamethyldisilazane, are also relatively expensive, which greatly increases the production cost of SiO2 aerogel, and its large-scale production and industrial application are subject to certain restrictions. Using low-cost water glass instead of silicone as a silicon source is an important direction for the current research and industrial development of silica aerogel. However, water glass has many impurities. If the impurities are not removed, the thermal conductivity of the aerogel will be as high as 0.029-0.033W / m·K. In addition, the preparation of SiO2 aerogels currently mostly adopts supercritical drying process, however, the supercritical process equipment is complex, the cost is high, and there is a certain degree of danger. The SiO2 aerogels prepared by supercritical drying process are affected by equipment and production capacity, and it is difficult to meet the growing market demand. In addition, some existing SiO2 aerogels are prepared by conventional atmospheric pressure drying process, but when using conventional atmospheric pressure drying process to prepare SiO2 aerogels, it is necessary to cooperate with cumbersome solvent replacement steps, which has a long production cycle and high cost. Summary of the invention

[0005] In view of the above problems, the present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the present invention provides a method for preparing high-purity silica aerogel and the obtained silica aerogel, which can alleviate the problems of limited production capacity of the organosilicon source used in the current preparation, expensive raw materials such as organosilicon modifiers, high production costs, low purity of water glass, etc., and the obtained silica aerogel has high purity, large specific surface area, low density and excellent thermal insulation performance.

[0006] A method for preparing high-concentration silica aerogel comprises the following steps: S1, mixing an inorganic silicon source, deionized water and an acidic catalyst uniformly, and performing gelation to obtain a wet gel; S2, aging the wet gel obtained in S1, replacing it with anhydrous ethanol, adding a surface modifier, and keeping it at 60-70°C for 6-10h to obtain a modified gel; S3, uniformly mixing the surfactant, alcohol cosolvent and non-polar solvent to obtain a reverse micelle extraction solution; S4, mixing and soaking the modified gel obtained in S2 and the reverse micelle extraction solution obtained in S3 at a volume ratio of 1:12-25, standing and centrifuging to obtain an extraction gel; S5, drying the extracted gel obtained in S4 at normal pressure to obtain a silica aerogel; The surface modifier described in S2 is an oxazolidinone derivative.

[0007] In some embodiments of the present invention, the inorganic silicon source in S1 is at least one of sodium silicate, potassium silicate, lithium silicate, magnesium silicate, and calcium silicate.

[0008] In some embodiments of the present invention, the acidic catalyst in S1 is at least one of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, and acetic acid, wherein the mass concentration of the inorganic acid is 10-20wt%.

[0009] In some embodiments of the present invention, the mass ratio of the inorganic silicon source, deionized water and acidic catalyst in S1 is 1:5-10:0.3-1.2.

[0010] In some embodiments of the present invention, the oxazolidinone derivative is at least one of 4-isopropyl-2-oxazolidinone, 4-isopropyl-5,5-dimethyl-2-oxazolidinone, 4-phenyl-2-oxazolidinone, 4-benzyl-2-oxazolidinone, 4-benzyl-5,5-dimethyl-2-oxazolidinone, (4S)-4-[(4-aminophenyl)methyl]-2-oxazolidinone and 5,5-dimethyloxazolidine-2,4-dione; the usage mass accounts for 20-35% of the mass of the wet gel.

[0011] In some embodiments of the present invention, the surfactant in S3 is at least one of dodecyl sulfate, tetradecyl betaine, and hexadecyltrimethylammonium bromide; the alcohol cosolvent is at least one of methanol, n-propanol, isopropanol, n-butanol, isobutanol, n-pentanol, and isopentanol; and the non-polar solvent is at least one of benzene, toluene, n-pentane, n-hexane, and n-heptane.

[0012] In some embodiments of the present invention, the mass ratio of the surfactant, the alcohol cosolvent and the non-polar solvent in S3 is 1-3:5-17:80-150.

[0013] In some embodiments of the present invention, the process of normal pressure drying in S5 is: drying at 60-70° C. for 1-2 h, and drying at 100-120° C. for 1-2 h.

[0014] In the present invention, reverse micelles are used to extract silica gel, and the principle of reverse micelle extraction is that when the surfactant molecules and cosolvents are dissolved in a non-polar solvent to reach a certain critical concentration, a nano-aggregate with a hydrophilic end facing inward, a lipophilic end facing outward and a trace amount of water in the middle is formed, namely, a reverse micelle, and the cosolvent can promote the dissolution of the surfactant to form a relatively stable, larger-sized reverse micelle structure. The reverse micelle solution is an oil-in-water structure, which can take out the water in the wet gel. As the non-polar solvent enters the gel pores, the surfactants wrapped in the hydrophobic groups (-CH3) on the three-dimensional skeleton of the gel are gradually desorbed, and the lipophilic and hydrophobic groups point to the solid-liquid interface of the gel skeleton, further promoting the outward migration rate of the water phase in the gel. It can be seen that in reverse micelle extraction, the selection of surfactants and non-polar organic solvents is particularly important. In order to improve the purity of silica aerogel and not affect the cross-linking of the surface modifier with silica molecules inside the silica aerogel, the inventors selected several specific anionic surfactants (dodecyl sulfate) and cationic surfactants (tetradecyl betaine and hexadecyl trimethyl ammonium bromide) with specific alcohol cosolvents and specific non-polar solvents, and mixed them according to the preferred mass ratio to obtain a reverse micelle extraction solution. If the components of the reverse micelle extraction solution used are not the above components, it is very likely to destroy the spatial network structure formed by hydrogen bonds inside the silica aerogel.

[0015] The acid-catalyzed one-step gelation method used to prepare silica aerogels changes the electrolyte concentration or ions with specific adsorption capacity, compresses the diffusion layer thickness, changes the electromotive force, and then regulates the gelation time to simplify the process.

[0016] The surface modifier used, oxazolidinone derivative, contains a five-membered heterocyclic ring, in which the imino and carbonyl groups can form a spatial network structure around the silica aerogel through hydrogen bonds, while the substituents on the five-membered heterocyclic ring increase the internal pore structure of the silica aerogel through the steric effect, thereby reducing its density and increasing its specific surface area.

[0017] The present invention also provides a silica aerogel, which is prepared by the above-mentioned preparation method.

[0018] In some embodiments of the present invention, the specific surface area of ​​the silica aerogel is ≥700m 2 / g, thermal conductivity ≤0.013W / (m·K).

[0019] Beneficial effects: Compared with the prior art, the present invention utilizes an inorganic silicon source as a precursor, which is low in cost and widely available, and can solve the current problems of limited production capacity, impure yield, and high cost of organic silicon sources. At the same time, oxazolidinone and its derivatives are used as surface modifiers, and chemical force hydrogen bonds are used to form a spatial network structure inside the silica aerogel. Without destroying the chemical structure of the aerogel, the density of the resulting silica aerogel is reduced, its specific surface area is increased, and a lower thermal conductivity is obtained. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0021] It should be pointed out that in the process of preparing silica aerogel, the modified gel can be prepared first and then the reverse micelle extraction solution is prepared; alternatively, the reverse micelle extraction solution can be prepared first and then the modified gel is prepared; alternatively, the reverse micelle extraction solution and the modified gel can be prepared at the same time, that is, the present application does not limit the preparation order of the reverse micelle extraction solution and the modified gel.

[0022] Example 1 S1, mixing sodium silicate, deionized water and 10wt% hydrochloric acid evenly, and performing gelation to obtain a wet gel; wherein the mass ratio of sodium silicate, deionized water and 10wt% hydrochloric acid is 1:5:0.3; S2, the wet gel obtained in S1 was sealed and aged at 40°C for 40 hours, replaced with anhydrous ethanol twice, and then 4-isopropyl-2-oxazolidinone accounting for 20% of the mass of the wet gel was added, and kept at 60°C for 10 hours to obtain a modified gel; S3, mixing sodium dodecyl sulfate, methanol and benzene in a mass ratio of 1:5:80 to obtain a reverse micelle extraction solution; S4, mixing the modified gel obtained in S2 and the reverse micelle extraction solution obtained in S3 at a volume ratio of 1:12, soaking at 45°C for 3 hours, standing and centrifuging to obtain an extraction gel; S5. Dry the extracted gel obtained in S4 at normal pressure: dry at 60° C. for 2 h and at 100° C. for 1 h to obtain silica aerogel.

[0023] Example 2 S1, mixing potassium silicate, deionized water and 15wt% sulfuric acid evenly, performing gelation, and obtaining a wet gel; wherein the mass ratio of potassium silicate, deionized water and 15wt% sulfuric acid is 1:7:0.8; S2, the wet gel obtained in S1 was sealed and aged at 45°C for 40 hours, replaced twice with anhydrous ethanol, and then 28% of the mass of the wet gel was added with 4-isopropyl-5,5-dimethyl-2-oxazolidinone, and kept at 65°C for 8 hours to obtain a modified gel; S3, mixing tetradecyl beet, n-butanol and n-pentane in a mass ratio of 2:11:120 to obtain a reverse micelle extraction solution; S4, mixing the modified gel obtained in S2 and the reverse micelle extraction solution obtained in S3 in a volume ratio of 1:18, soaking at 45°C for 4 hours, standing and centrifuging to obtain an extraction gel; S5. Dry the extracted gel obtained in S4 at normal pressure: dry at 65°C for 2 h and at 110°C for 1 h to obtain silica aerogel.

[0024] Example 3 S1, mixing magnesium silicate, deionized water and 20wt% nitric acid evenly, performing gelation, and obtaining a wet gel; wherein the mass ratio of magnesium silicate, deionized water and 20wt% nitric acid is 1:10:1.2; S2, the wet gel obtained in S1 was sealed and aged at 50°C for 40 hours, replaced with anhydrous ethanol twice, and then 4-benzyl-5,5-dimethyl-2-oxazolidinone accounting for 35% of the mass of the wet gel was added, and kept at 70°C for 6 hours to obtain a modified gel; S3, mixing cetyltrimethylammonium bromide, isoamyl alcohol and n-heptane in a mass ratio of 3:17:150 to obtain a reverse micelle extraction solution; S4, mixing the modified gel obtained in S2 and the reverse micelle extraction solution obtained in S3 at a volume ratio of 1:25, soaking at 45°C for 3 hours, standing and centrifuging to obtain an extraction gel; S5. Dry the extracted gel obtained in S4 at normal pressure: dry at 70°C for 1 h and at 120°C for 2 h to obtain silica aerogel.

[0025] Example 4 The process is the same as in Example 1, except that the surfactant used is calcium stearate.

[0026] Example 5 The process is the same as in Example 1, except that the non-polar solvent used is hexamethyldisiloxane.

[0027] Example 6 The process is the same as that of Example 3, except that the mass ratio of the surfactant, alcohol cosolvent and non-polar solvent used is 4:17:150.

[0028] Example 7 The process is the same as in Example 3, except that the 4-isopropyl-2-oxazolidinone used accounts for 40% of the mass of the wet gel.

[0029] Comparative Example 1 The process is the same as in Example 1, except that 4-isopropyl-2-oxazolidinone is replaced by 2-oxazolidinone.

[0030] Comparative Example 2 The process is the same as in Example 1, except that 4-isopropyl-2-oxazolidinone is not added.

[0031] Comparative Example 3 Commercially available silica aerogel.

[0032] Performance Testing Stress test: A Shanghai Tengba texture analyzer was used to perform pressure tests of 10% stress and 20% stress on the silica aerogels obtained in Examples 1-7 and Comparative Examples 1-3; Specific surface area: measured by BET method; Thermal conductivity: measured by heat flow meter method.

[0033] The test results are detailed in Table 1:

[0034] As can be seen from the data in Table 1, the silica aerogel provided by the present invention has high mechanical properties, high specific surface area and excellent thermal insulation, and its thermal conductivity is not higher than 0.013W / (m·K). This is because the high porosity and three-dimensional network structure in the silica aerogel form a long thermal conduction path, and the heat flow can only be transferred along the pore wall when it is transferred in the solid. The long thermal conduction path allows the heat to gradually dissipate, thereby obtaining an extremely low thermal conductivity. At the same time, due to the improved mechanical strength, the silica aerogel can better resist the shrinkage and collapse caused by solvent volatilization when dried at normal pressure.

Claims

1. A method for preparing high-purity silica aerogel, characterized in that: The following steps are involved: S1, mixing an inorganic silicon source, deionized water and an acidic catalyst uniformly, and performing gelation to obtain a wet gel; S2, aging the wet gel obtained in S1, replacing it with anhydrous ethanol, adding a surface modifier, and keeping it at 60-70°C for 6-10h to obtain a modified gel; S3, uniformly mixing the surfactant, alcohol cosolvent and non-polar solvent to obtain a reverse micelle extraction solution; S4, mixing and soaking the modified gel obtained in S2 and the reverse micelle extraction solution obtained in S3 at a volume ratio of 1:12-25, standing and centrifuging to obtain an extraction gel; S5, drying the extracted gel obtained in S4 at normal pressure to obtain a silica aerogel; The surface modifier described in S2 is an oxazolidinone derivative.

2. The method for preparing high-purity silica aerogel according to claim 1, characterized in that: The inorganic silicon source in S1 is at least one of sodium silicate, potassium silicate, lithium silicate, magnesium silicate and calcium silicate.

3. The method for preparing high-purity silica aerogel according to claim 1, characterized in that: The acid catalyst in S1 is at least one of hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid and acetic acid, wherein the mass concentration of the inorganic acid is 10-20wt%.

4. The method for preparing high-purity silica aerogel according to claim 1, characterized in that: The mass ratio of the inorganic silicon source, deionized water and acidic catalyst in S1 is 1:5-10:0.3-1.

2.

5. The method for preparing high-purity silica aerogel according to claim 1, characterized in that: The oxazolidinone derivative is at least one of 4-isopropyl-2-oxazolidinone, 4-isopropyl-5,5-dimethyl-2-oxazolidinone, 4-phenyl-2-oxazolidinone, 4-benzyl-2-oxazolidinone, 4-benzyl-5,5-dimethyl-2-oxazolidinone, (4S)-4-[(4-aminophenyl)methyl]-2-oxazolidinone and 5,5-dimethyloxazolidin-2,4-dione.

6. The method for preparing high-purity silica aerogel according to claim 5, characterized in that: The mass of the oxazolidinone derivative used accounts for 20-35% of the mass of the wet gel.

7. The method for preparing high-purity silica aerogel according to claim 1, characterized in that: The surfactant in S3 is at least one of dodecyl sulfate, tetradecyl betaine, and hexadecyltrimethylammonium bromide; the alcohol cosolvent is at least one of methanol, n-propanol, isopropanol, n-butanol, isobutanol, n-pentanol, and isopentanol; the non-polar solvent is at least one of benzene, toluene, n-pentane, n-hexane, and n-heptane.

8. The method for preparing high-purity silica aerogel according to claim 7, characterized in that: The mass ratio of surfactant, alcohol cosolvent and non-polar solvent in S3 is 1-3:5-17:80-150.

9. The method for preparing high-purity silica aerogel according to claim 1, characterized in that: The process of normal pressure drying in S5 is: drying at 60-70° C. for 1-2 hours, and drying at 100-120° C. for 1-2 hours.

10. A high-purity silica aerogel, characterized in that: Prepared by the preparation method according to any one of claims 1 to 9.