Method for preparing sodium bentonite through particle size control
By carrying out particle size control pretreatment and sodium treatment of raw bentonite ore, the problems of incomplete sodium treatment and excess sodium treatment were solved, the efficient production of sodium bentonite was achieved, and the quality and production stability of the product were improved.
Patent Information
- Application Number
- CN202410924328.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing production process of sodium bentonite, there are problems such as uneven particle size, incomplete sodiumization, excessive dosage of sodiumizing agent and long storage time, resulting in low production efficiency and substandard products.
By pre-treating the raw bentonite ore, controlling the particle size to <2mm, mixing water and soda agent, extruding, aging reaction and drying and grinding, sodium bentonite with uniform particle size can be obtained.
It realizes the perfection of the sodium reaction, improves the product qualification rate and production stability, reduces the cost, and is suitable for a variety of industrial uses.
Smart Images

Figure CN118771401A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of sodium bentonite processing, and in particular to a method for preparing sodium bentonite by controlling particle size. Background Art
[0002] Sodium bentonite is widely used in many fields due to its unique physical and chemical properties. For example, sodium bentonite is added to coatings to improve the viscosity and rheological properties of the coating; it is used as a foundry sand binder to prepare sand molds, and its good plasticity helps prevent sand inclusion, scarring, block loss and sand mold collapse in castings, while improving the quality and precision of castings; as a major component of drilling mud, it can expand rapidly in water, provide a good suspension and gel state, thereby helping to control the cooling of the drill bit, remove debris and protect the well wall.
[0003] Most of the bentonite in nature is calcium-based bentonite, which has inferior process and technical performance to sodium-based bentonite. Therefore, artificial sodiumization is often used in industry to transform calcium-based bentonite into sodium-based bentonite. At present, most factories use wet and semi-dry sodiumization methods, accompanied by extrusion sodiumization and storage aging processes. Due to the extensive production process, the particle size of the raw materials is often not controlled, resulting in incomplete sodiumization of large particles of bentonite, excessive sodiumization agent, and long storage aging time, which may reduce the efficiency of the sodiumization production line or cause the product to fail to meet the standards. Summary of the invention
[0004] The object of the present invention is to solve at least one of the above-mentioned deficiencies in the prior art. For example, one of the objects of the present invention is to achieve controllable particle size and perfect sodiumization reaction and excellent sodiumization effect.
[0005] In order to achieve the above object, the present invention provides a method for preparing sodium bentonite by controlling particle size.
[0006] The method may include: pre-treating bentonite ore to obtain target bentonite particles with a particle size of less than 2 mm; mixing the target bentonite particles, water and a sodium-forming agent and then extruding them to obtain first sodium-formed bentonite granules; subjecting the first sodium-formed bentonite granules to an aging reaction to obtain second sodium-formed bentonite granules; and drying and grinding the second sodium-formed bentonite granules to obtain the sodium-formed bentonite.
[0007] Optionally, the pretreatment may include: coarse crushing, first inspection screening, fine crushing and second inspection screening stages; wherein, the coarse crushing is to crush the raw ore to obtain bentonite particles with a particle size of <15mm; the first inspection screening can screen out bentonite particles with particle sizes ≥8mm and <8mm respectively; the object of fine crushing is the bentonite particles with a particle size of <8mm; the second inspection screening can screen out bentonite particles with particle sizes of >≥2mm and <2mm respectively.
[0008] Optionally, the pretreatment may further include: for the bentonite particles with a particle size of ≥8 mm, returning them to the coarse crushing section for coarse crushing and then performing the first inspection and screening.
[0009] Optionally, the pretreatment may further include: for the bentonite particles with a particle size of ≥2 mm, returning them to the fine crushing section for fine crushing and then performing the second inspection and screening.
[0010] Optionally, the bentonite ore may include at least one of calcium-based bentonite, calcium-magnesium-based bentonite and calcium-magnesium-sodium-based bentonite; and the particle size of the bentonite ore is less than 200 mm.
[0011] Alternatively, the amount of water used may be 20% to 40% of the mass of the target bentonite particles.
[0012] Alternatively, the amount of the sodium-forming agent may be 1.5% to 4% of the mass of the target bentonite particles.
[0013] Alternatively, the sodiumizing agent may include one or more of sodium carbonate, sodium bicarbonate, sodium silicate, sodium phosphate and sodium hydroxide.
[0014] Alternatively, the moisture content of the second sodium bentonite granules after drying may be 8% to 14%.
[0015] Optionally, the drying may include at least one of air-drying and oven-drying.
[0016] Optionally, the grinding process is to grind the dried second sodium bentonite granules into fine powder using a grinding device, wherein the grinding device includes a Raymond mill, a jet mill, or a cyclone mill.
[0017] Optionally, the particle size of the sodium bentonite can be 180-325 mesh, the blue absorption can be 30-40g / 100g, the free expansion times can be 20-30ml / 2g, the swelling value can be 80-95ml / 3g, the wet compressive strength can be 90-130kPa, the hot wet tensile strength can be 2.5-4.5kPa, and the viscosity can be 25-35 (600r / min) / (mPa.s).
[0018] Compared with the prior art, the beneficial effects of the present invention include at least one of the following:
[0019] 1) The method for preparing sodium bentonite of the present invention has simple process, convenient operation, low cost, and easy equipment selection and matching, that is, the production line is easy to realize.
[0020] 2) The method for preparing sodium bentonite of the present invention can avoid the problems of incomplete sodiumization, excessive use of sodiumizing agent, or long storage and aging time by controlling the particle size.
[0021] 3) The method for preparing sodium bentonite of the present invention has uniform particle size, sufficient sodium reaction, high qualified rate of obtained products, stable production, avoidance of unqualified products, and low amount of discarded finished products.
[0022] 4) The various indices of sodium bentonite prepared by the present invention have been improved to a certain extent, and can meet the quality indicators of bentonite for casting, metallurgical pellets and drilling mud, and are suitable for a variety of industrial uses. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The above and other objects and / or features of the present invention will become more apparent through the following description in conjunction with the accompanying drawings, in which:
[0024] Figure 1 A schematic diagram of a process flow for preparing sodium bentonite by controlling particle size according to the present invention is shown. DETAILED DESCRIPTION
[0025] Hereinafter, a method for preparing sodium bentonite by controlling particle size according to the present invention will be described in detail in conjunction with exemplary embodiments.
[0026] It should be noted that “first”, “second”, “third”, “fourth”, “fifth”, etc. are only for the convenience of description and distinction, and cannot be understood as indicating or implying relative importance. For the “+” and “-” before the particle size parameter of the present invention, their meanings respectively represent the oversize and undersize, that is, the oversize particles that cannot pass through the target sieve and the undersize particles that can pass through the target sieve.
[0027] Exemplary Embodiment 1
[0028] This exemplary embodiment provides a method for preparing sodium bentonite by particle size control. The method has controllable particle size of raw material feed, simple process, controllable particle size, and low cost. Uniformly sodium-containing sodium bentonite can be obtained, which is critical to promoting the stable and standard production of products in the sodium bentonite production industry. Figure 1 A schematic diagram of a process flow for preparing sodium bentonite by controlling particle size according to the present invention is shown.
[0029] like Figure 1 As shown, the method may include the following steps:
[0030] S01: Coarsely crushing the bentonite ore to obtain first bentonite particles.
[0031] In this embodiment, the bentonite ore may include one or more of calcium-based bentonite, calcium-magnesium-based bentonite, and calcium-magnesium-sodium-based bentonite; the color may include off-white, brick red, gray, gray-black, khaki, blue-gray, etc.; the texture includes hard, soft and transitional types; the main phase may be montmorillonite, containing a small amount of quartz, tridymite, cristobalite, illite, and calcite; the particle size is less than 200 mm, such as 190 mm, 185 mm, 170 mm, 160 mm, etc.
[0032] In this embodiment, the coarse crushing can be carried out by one or more of a toothed roller crusher, a double roller crusher, a jaw crusher, a gyratory crusher, and a cone crusher. The purpose of selecting the above crushers is that the above crushers have a large crushing ratio and a processing capacity, and are suitable for crushing a large number of ores with lower hardness to a lower particle size. The discharge port size can be set to be less than 15mm, such as 14.5mm, 14mm, 12.5mm, 11mm, etc. The purpose of selecting the above discharge port size is to ensure that the particle size of the coarse crushed product is mostly -8mm.
[0033] In this embodiment, according to the actual operating conditions, one or more of manual feeding, mine car feeding, disc feeder feeding, and bottom feeding can be selected in the coarse crushing process, so that the feeding speed can be flexibly controlled according to production needs.
[0034] S02: The first bentonite particles are inspected and sieved using an 8 mm sieve to obtain second bentonite particles with a particle size of +8 mm and third bentonite particles with a particle size of -8 mm, i.e., second bentonite particles that cannot pass through the 8 mm sieve (particle size ≥ 8 mm) and third bentonite particles that can pass through the 8 mm sieve (particle size < 8 mm).
[0035] In this embodiment, the inspection screening can be carried out by using a vibrating screen for particle size control, including a linear vibrating screen, a combined vibrating screen, etc. The above-mentioned vibrating screen can obtain higher screening efficiency than conventional screening, and can collect different particle sizes through multiple layers of screens. At the same time, when vibrating and screening, it can disperse the agglomerated samples to avoid the difficulty of screening due to adhesion between bentonite particles. The purpose of selecting an 8mm sieve is to use an 8mm particle size as the screening particle size entering the fine crushing section, which can make the fine crushing part easier to achieve and avoid clogging.
[0036] As an option of the present invention, the vibrating screen can be configured with two groups of different screens, corresponding to two feed ports A and B and three discharge ports A', B' and C', the sizes of the two groups of screens are 8mm and 2mm respectively, and the coarsely crushed material enters the vibrating screen from port A; the material on the screen ≥8mm at the A' discharge port is returned to step S01) for coarse crushing, the material under the screen <8mm at the B' discharge port and the material on the screen ≥2mm enter the fine crushing section of step S03); the material under the screen <2mm at the C' discharge port enters the sodium processing workshop.
[0037] The present invention selects to send bentonite materials with a diameter of less than 2 mm into the subsequent sodiumization process because bentonite particles with a particle size of less than 2 mm are more uniformly and thoroughly sodiumized during the sodiumization process of adding water and alkali.
[0038] S03: The second bentonite particles with a size of ≥8 mm are returned to the coarse crushing section for further crushing, and the third bentonite particles are finely crushed and screened to obtain fourth bentonite particles with a particle size of ≥2 mm (i.e., particles on the 2 mm sieve) and fifth bentonite particles with a particle size of <2 mm (i.e., particles under the 2 mm sieve). The particles can be returned to the coarse crushing section via a conveyor belt and an electromagnetic feeder.
[0039] In this embodiment, the fine crushing stage is carried out by rollers, which may include one or more of a double roller mill, a hydraulic roller mill and a high-pressure roller mill, and the roller spacing is set to 2-3 mm. The fine crushed product can be transported to the B port of the vibrating screen by a conveyor belt for inspection and screening. The purpose of using rollers is to obtain a larger crushing ratio, which is used to reduce the energy consumption of fine crushing, and at the same time, the force between particles under the fluidization theory of the material bed can be used to better control the particle size of the product.
[0040] In this embodiment, the vibrating screen used for inspection and screening is the same vibrating screen used for inspection and screening in coarse crushing. The vibrating screen plays the role of inspection and screening of coarse crushed materials and inspection and screening of fine crushed materials at the same time.
[0041] In this embodiment, for the conveyor belt and electromagnetic feeder, the starting point of the conveyor belt is connected to the material discharge port of the vibrating screen, and the end point of the conveyor belt is connected to the inlet B' of the electromagnetic feeder. The feeding and conveying area of the electromagnetic feeder is longer than 0.5m, and the tail is connected to the inlet of the fine crushing equipment.
[0042] In this embodiment, the fine crushing section can be set up with multiple stages of fine crushing process according to the mixing ratio of the bentonite ore, such as two to three stages in a double-roll mill, a hydraulic double-roll mill and a high-pressure roller mill. The purpose of setting up multiple stages of fine crushing process is to avoid that some materials have high hardness or strong viscosity, and single-stage crushing cannot make them reach the target particle size. Multi-stage crushing can better control the particle size.
[0043] S04: Return the fourth bentonite particles ≥ 2 mm to the fine crushing section for further fine crushing and inspection screening. A conveyor belt and an electromagnetic feeder can be used to return to the fine crushing section.
[0044] In this embodiment, the fourth bentonite particles are inspected and screened again to ensure that the bentonite particles entering the water and alkali sodium adding chemical stage are all <2 mm (ie, they can all pass through a 2 mm sieve).
[0045] S05: During the process of transporting the fifth bentonite particles to the sodium treatment workshop, water and a sodium treatment agent are added and then the particles are put into a screw extruder to obtain first sodium treatment bentonite particles through extrusion. The particles can be transported by a belt conveyor.
[0046] In this embodiment, the water used can be industrial water, and the amount of water added is 20% to 40% of the mass of the bentonite (i.e., the fifth bentonite particles), such as 21%, 23%, 25%, 26%, 39%, etc. The reason for selecting the above amount of water added is to allow the sodium agent to be evenly mixed with the bentonite without excessive humidity causing bonding.
[0047] In the present embodiment, the sodiumizing agent used can be one or more of sodium carbonate, sodium bicarbonate, sodium silicate, sodium phosphate, and sodium hydroxide. The amount of the sodiumizing agent can be 1.5% to 4% of the mass of the bentonite (i.e., the fifth bentonite particle), such as 1.5%, 1.6%, 1.8%, 2%, 2.5%, 4%, etc. The purpose of selecting the amount of the sodiumizing agent is to ensure that the sodiumization reaction is carried out thoroughly without excess sodiumizing agent.
[0048] In this embodiment, the extrusion is to homogenize and disperse the bentonite containing industrial water and the sodium-forming agent through a screw extruder to obtain the first sodium-formed bentonite granules.
[0049] S06: The first sodium bentonite granules are transported to a storage yard for aging to obtain second sodium bentonite granules.
[0050] In this embodiment, the aging reaction may include directly stacking the first sodium bentonite pellets in a storage yard or stacking them covered with waterproof materials. The aging reaction time may be 2 weeks to 13 weeks, such as 4 weeks, 5 weeks, 7 weeks, 10 weeks, 13 weeks, etc., to obtain the second sodium bentonite pellets.
[0051] The purpose of the aging reaction is to save manpower and material resources and allow the sodium reaction to continue under natural conditions. The purpose of selecting the above aging time is to ensure that the sodium reaction is thorough without wasting excessive time.
[0052] S07: The obtained second sodium bentonite granules are aired, dried and ground to obtain the sodium bentonite.
[0053] In this embodiment, drying may include: the drying yard reduces the moisture content of the second sodium bentonite particles to 15% to 22%, such as 15%, 18.5%, 19%, 20%, 20.5%, 22%, etc. through sun drying and air drying. The purpose of reducing the moisture content of the sample to the above range through drying is to reduce the subsequent drying time in the drying kiln and save coal consumption.
[0054] In this embodiment, drying may include: using an industrial kiln (such as a rotary kiln, a fluidized bed drying kiln) to reduce the moisture content of the second sodium bentonite particles after drying to 8% to 14%, such as 8%, 8.6%, 9%, 10%, 11%, 14%, etc. Drying the sample to the above moisture content range through a rotary kiln can prevent the finished product from agglomerating as much as possible during the grinding process, affecting the grinding stage, and at the same time facilitate storage and transportation after grinding.
[0055] In this embodiment, the grinding may include: grinding the dried second sodium bentonite granules through a grinding device, and obtaining the sodium bentonite after grinding.
[0056] The grinding equipment includes Raymond mill, air flow mill and cyclone mill. The purpose of selecting these grinding equipment in the present invention is that these mills can achieve better grinding and dispersing effects, are suitable for grinding bentonite particles with high viscosity and low particle hardness, and can avoid the problem of easy adhesion of conventional mills.
[0057] In this embodiment, the sodium bentonite prepared by the present invention has the following properties:
[0058] The particle size can be 180-325 mesh, such as 180 mesh, 200 mesh, 210 mesh, 220 mesh, 300 mesh, etc.
[0059] The blue absorption amount can be 30-40g / 100g, such as 32g / 100g, 33.5g / 100g, 34g / 100g, 34.5g / 100g, 36g / 100g, etc.
[0060] The free expansion times can be 20-30ml / 2g, such as 20ml / 2g, 22.5ml / 2g, 24ml / 2g, 24.5ml / 2g, 28ml / 2g, etc.
[0061] The swelling value can be 80-95 ml / 3g, such as 80 ml / 3g, 82 ml / 3g, 83 ml / 3g, 83.5 ml / 3g, 94 ml / 3g, etc.
[0062] The wet compressive strength can be 90-130 kPa, such as 90 kPa, 95 kPa, 98 kPa, 100 kPa, 110 kPa, etc.
[0063] The hot wet tensile strength can be 2.5 to 4.5 kPa, such as 2.5 kPa, 2.8 kPa, 3 kPa, 3.5 kPa, 4.2 kPa, etc.;
[0064] The viscosity can be 25 to 35 (600r / min) / (mPa.s), such as 25 (600r / min) / (mPa.s), 28 (600r / min) / (mPa.s), 30 (600r / min) / (mPa.s), 30.5 (600r / min) / (mPa.s), 35 (600r / min) / (mPa.s), etc. Among them, (600r / min) / (mPa.s) refers to the viscosity value measured at 600r / min, in mPa.s.
[0065] The parameter range of the above properties can meet the quality indicators of bentonite for casting, metallurgical pelletizing and drilling mud (see Table 1-3), and is suitable for a variety of industrial uses.
[0066] Table 1 Quality indexes of bentonite for casting
[0067]
[0068] Table 2 Quality indexes of bentonite for metallurgical pelletization
[0069]
[0070] Table 3 Quality indexes of bentonite for drilling mud
[0071]
[0072] In order to better understand the above exemplary embodiments of the present invention, they are further described below with reference to specific examples.
[0073] Comparative Example
[0074] The bentonite ore is coarsely crushed to obtain the first bentonite particles; after the first stage inspection and screening, the second bentonite particles ≥8 mm and the third bentonite particles <8 mm are obtained, and the bentonite particles with a particle size of ≥10.0 mm and <20.0 mm (numbered DB-1) and the bentonite particles with a particle size of ≥8.0 mm and <10.0 mm (numbered DB-2) are taken from the second bentonite particles.
[0075] The third bentonite particles are finely crushed and screened to obtain fourth bentonite particles ≥2 mm and fifth bentonite particles <2 mm, and bentonite particles with a particle size of ≥2.0 and <5.0 mm among the fourth bentonite particles are selected (numbered DB-3).
[0076] Example
[0077] The fifth bentonite particles obtained in the comparative example were sieved to take bentonite particles with a particle size of 0.6 to 1.6 mm (numbered SL-1), bentonite particles with a particle size of ≥0.22 and <0.6 mm (numbered SL-2), bentonite particles with a particle size of <0.22 mm (i.e., capable of passing through a 0.22 mm sieve) (numbered SL-3), and bentonite particles with a particle size of <0.074 mm (i.e., capable of passing through a 0.074 mm sieve) (numbered SL-4).
[0078] Test example:
[0079] The bentonite particles obtained in the above comparative examples and examples were transported to the sodium workshop by a conveyor belt, added with water and a sodium agent, and then entered into a screw extruder to obtain the first sodium bentonite granules after extrusion. The sodium bentonite granules were transported to the storage yard and aged for 8 weeks to obtain the second sodium bentonite granules. The second sodium bentonite granules were then aired, dried and ground to obtain sodium bentonite (numbered as above).
[0080] The obtained sodium bentonite samples were tested for blue absorption, free expansion times, swelling value, wet compressive strength and hot wet tensile strength. The test results are shown in Table 4 below.
[0081] Table 4 Various index data of sodium bentonite
[0082]
[0083] Table 4 shows the various indicators of the above sodium bentonite. From the data in the table, it can be seen that the blue absorption of comparative examples DB-1, DB-2 and DB-3 is about 33g / 100g, the free expansion times are about 20ml / 2g, the swelling value is about 70ml / 3g, the wet compressive strength is about 98kPa, the hot wet tensile strength is about 2.9kPa, and the viscosity is about 22 (600r / min) / (mPa.s). The blue absorption of example samples SL-1, SL-2, SL-3 and SL-4 is about 35g / 100g, the free expansion times are about 25ml / 2g, the swelling value is about 92ml / 3g, the wet compressive strength is about 120kPa, the hot wet tensile strength is about 4.2kPa, and the viscosity is about 28 (600r / min) / (mPa.s). All indicators have been greatly improved, which can meet the quality indicators of bentonite for casting, metallurgical pelletizing and drilling mud, and are suitable for a variety of industrial uses.
[0084] Experimental data show that the performance of the sodium bentonite sample obtained by controlling the bentonite particle size at -2mm for sodiumization experiment is better than that of the sodium bentonite sample obtained by controlling the bentonite particle size at +2mm for sodiumization experiment, indicating that the method of preparing sodium bentonite by particle size control in this patent is feasible.
[0085] Although the present invention has been described above in conjunction with the exemplary embodiments and the accompanying drawings, it should be apparent to those skilled in the art that various modifications may be made to the above-described embodiments without departing from the spirit and scope of the claims.
Claims
1. A method for preparing sodium bentonite by particle size control, characterized in that: The method comprises: Pre-treating the bentonite ore to obtain target bentonite particles with a particle size of less than 2 mm; Extruding the target bentonite particles, water and a sodium-forming agent to obtain first sodium-formed bentonite granules; subjecting the first sodium bentonite granules to an aging reaction to obtain second sodium bentonite granules; The sodium bentonite is obtained by drying and grinding the second sodium bentonite granules.
2. The method for preparing sodium bentonite by particle size control according to claim 1, characterized in that: The pretreatment includes four stages: coarse crushing, first inspection and screening, fine crushing and second inspection and screening, wherein: Coarse crushing is to crush the raw ore to obtain bentonite particles with a particle size of less than 15 mm; The first inspection screening can screen out bentonite particles with particle sizes ≥8mm and <8mm respectively; The finely crushed objects are bentonite particles with a particle size of <8 mm; The second inspection screening can screen out bentonite particles with particle sizes ≥2mm and <2mm respectively.
3. The method for preparing sodium bentonite by particle size control according to claim 2, characterized in that: The pretreatment further comprises: for the bentonite particles with a particle size of ≥8 mm, returning to the coarse crushing section for coarse crushing and then performing the first inspection screening, until the first inspection screening can only screen out bentonite particles with a particle size of <8 mm.
4. The method for preparing sodium bentonite by particle size control according to claim 2, characterized in that: The pretreatment further comprises: for the bentonite particles with a particle size of ≥2 mm, returning them to the fine crushing section for fine crushing and then performing the second inspection and screening.
5. The method for preparing sodium bentonite by particle size control according to claim 1, characterized in that: The bentonite ore includes at least one of calcium-based bentonite, calcium-magnesium-based bentonite and calcium-magnesium-sodium-based bentonite; the particle size of the bentonite ore is less than 200 mm.
6. The method for preparing sodium bentonite by particle size control according to claim 1, characterized in that: The amount of water used is 20% to 40% of the mass of the target bentonite particles; The dosage of the sodiumizing agent is 1.5% to 4% of the mass of the target bentonite particles.
7. The method for preparing sodium bentonite by particle size control according to claim 1, characterized in that: The sodiumizing agent includes one or more of sodium carbonate, sodium bicarbonate, sodium silicate, sodium phosphate and sodium hydroxide.
8. The method for preparing sodium bentonite by particle size control according to claim 1, characterized in that: The moisture content of the second sodium bentonite granules after drying is 8% to 14%.
9. The method for preparing sodium bentonite by particle size control according to claim 1, characterized in that: The grinding process comprises grinding the dried second sodium bentonite granules through a grinding device, wherein the grinding device comprises a Raymond mill, a jet mill, and a cyclone pulverizer, and the sodium bentonite is obtained after grinding.
10. The method for preparing sodium bentonite by particle size control according to claim 1, characterized in that: The sodium bentonite has a particle size of 180-325 meshes, a blue absorption of 30-40 g / 100 g, a free expansion multiple of 20-30 ml / 2 g, a swelling value of 80-95 ml / 3 g, a wet compressive strength of 90-130 kPa, a hot wet tensile strength of 2.5-4.5 kPa, and a viscosity of 25-35 (600 r / min) / (mPa.s).
Citation Information
Patent Citations
Preparation method of bentonite for drilling mud and device thereof
CN105366686A
Preparation method for modified sodium base bentonite
CN107585772A
Dry-type preparation method of modified bentonite
CN113683094A