Molecular sieve modification method and modified molecular sieve
By forming a composite of MOF material and SSZ-13 on the molecular sieve, the problem of insufficient adsorption performance of the molecular sieve at high temperatures is solved, achieving efficient adsorption and stability of carbon dioxide at high temperatures, and adapting to changes in flue gas composition.
Patent Information
- Application Number
- CN202410923992.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-11
AI Technical Summary
Existing molecular sieves have insufficient adsorption performance for carbon dioxide under high temperature conditions, and the addition of binders will dilute the effective components and block the pores, reduce the performance of the catalyst, and cannot adapt to changes in the proportion of flue gas components.
Compound I was reacted with diethyl aluminum chloride under nitrogen protection to obtain compound II, which was then self-assembled with o-carboxyphenylacetic acid to form a MOF material. It was then compounded with SSZ-13 molecular sieve and formed into granules through ultrasonic treatment and drying. Modify molecular sieves to improve their adsorption performance at high temperatures.
The modified molecular sieve can significantly increase the adsorption capacity of carbon dioxide under high temperature conditions, has stable adsorption performance, adapts to changes in flue gas composition at different temperatures, and has high selectivity and is suitable for the adsorption of CO2 in flue gas.
Smart Images

Figure CN118771402A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of molecular sieves, and in particular relates to a molecular sieve modification method and a modified molecular sieve. Background Art
[0002] With the acceleration of industrialization, global greenhouse gas emissions continue to increase, and the greenhouse effect is becoming more serious. CO2 is one of the main components of greenhouse gases, and according to statistics, it usually accounts for more than 70%. In the process of power generation or heating, the use of fossil fuels such as coal, natural gas or oil will produce a large amount of CO2. There are many ways to absorb carbon dioxide in flue gas, and using molecular sieves to absorb carbon dioxide is one of the common methods.
[0003] SSZ-13 is a powdered molecular sieve that can be used to adsorb carbon dioxide. Molecular sieves in powder form often need to add a certain amount of binders and other substances to give them a certain shape and mechanical strength before they can be used in industrial production. However, the addition of binders will not only dilute the effective components of the molecular sieve, but also block the pores of the molecular sieve and reduce the accessibility of the active sites, which will greatly reduce the performance of the catalyst in practical applications. The pore size of the molecular sieve is generally fixed, and the composition of the flue gas will change with different combustion products. Molecular sieves with fixed pore sizes will not change with changes in the proportion of flue gas components. Some components cannot be absorbed, or the target components cannot be absorbed.
[0004] The invention patent with application publication number CN116212815A discloses a modified molecular sieve capable of adsorbing carbon dioxide and a preparation method thereof. The preparation method of the modified molecular sieve capable of adsorbing carbon dioxide comprises the following steps: S1: preparing an alkaline solution;
[0005] S2: Prepare the molecular sieve raw material and dry it in an oven; S3: Add the alkaline solution and the dried molecular sieve raw material into a vacuum volumetric flask, mix them, and evacuate them; S4: Centrifuge and stir until the solution is neutral, filter and dry the product to obtain the modified molecular sieve. The pore size of the molecular sieve is fixed and will not change with the change of flue gas temperature and component ratio. Summary of the invention
[0006] The purpose of the present invention is to provide a molecular sieve modification method to increase the adsorption capacity of the molecular sieve at a higher temperature.
[0007] Another object of the present invention is to provide a modified molecular sieve.
[0008] In order to achieve the above purpose, the technical solution adopted by the present invention is:
[0009] A molecular sieve modification method comprises the following steps:
[0010] 1) Under nitrogen protection, compound I is dissolved in a solvent, diethylaluminum chloride is gradually added to react, and after the reaction is completed, compound II is purified to obtain the compound. The reaction formula is shown in formula (1);
[0011]
[0012] 2) dissolving the compound II in step 1) in ethanol and mixing it with o-carboxyphenylacetic acid to obtain a MOF material through a self-assembly reaction;
[0013] 3) adding the molecular sieve to the MOF material in step 2), drying after ultrasonic treatment to obtain a crude modified molecular sieve, purifying and activating the crude material to obtain the modified molecular sieve.
[0014] Furthermore, in step 1), the molar ratio of compound I to diethylaluminum chloride is 1:1.2-1.5, the reaction time is 2-4 hours, and the reaction temperature is 25-35°C.
[0015] Furthermore, in step 1), the solvent is dichloromethane, and 10 to 15 mL of the solvent is added for every gram of the compound I.
[0016] Furthermore, the temperature of the self-assembly reaction in step 2) is 25-35°C.
[0017] Furthermore, in step 2), the molar ratio of compound II to o-carboxyphenylacetic acid is 1:2.5 to 1:3.5; and 8 to 12 mL of ethanol is added for every gram of compound II.
[0018] Furthermore, the molecular sieve in step 3) is SSZ-13 molecular sieve.
[0019] Furthermore, in step 3), the mass ratio of the molecular sieve to compound II is 10:0.8 to 10:1.2.
[0020] Furthermore, in step 3), the ultrasonic time is 30 to 60 minutes, the drying temperature is 40 to 60° C., and the drying time is 12 to 24 hours.
[0021] Furthermore, the purification method is: using ethanol to soak and wash the modified molecular sieve crude material and drying it; the activation method is vacuum activation at 100-120° C. for 12-24 hours.
[0022] A modified molecular sieve is prepared by the molecular sieve modification method.
[0023] Beneficial effects of the present invention:
[0024] The molecular sieve modification method of the present invention uses porphyrin to synthesize compound II, and then self-assembles with o-carboxyphenylacetic acid through hydrogen bonding, and then is compounded with the molecular sieve to finally form a modified molecular sieve. The modified molecular sieve is no longer in powder form, but in granular form. The granular modified molecular sieve is easy to use and has good adsorption performance. The remaining gases in the flue gas after desulfurization and other processes are mainly water vapor, CO2 and N2. The modified molecular sieve has more polar groups and has high selectivity for adsorbing CO2.
[0025] The molecular sieve modification method of the present invention is a material obtained by self-assembly of compound II and o-carboxyphenylacetic acid, and the stretchability is different at different temperatures. The o-carboxyphenylacetic acid connects the various compounds II. As the temperature rises, the distance between molecules increases, the structure of the MOF material changes, the MOF material stretches in the molecular sieve, the contact area with carbon dioxide increases, and the carbon dioxide absorption amount is improved. Therefore, the obtained molecular sieve has a good adsorption effect on CO2 under high temperature conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is the adsorption isotherm of carbon dioxide at 40°C;
[0027] Figure 2 This is the adsorption isotherm of carbon dioxide at 90°C. DETAILED DESCRIPTION
[0028] The present invention will be further described below in conjunction with the embodiments of the present invention.
[0029] Example 1
[0030] The molecular sieve modification method of this embodiment comprises the following steps:
[0031] 1) Under nitrogen protection, 78.7 g of compound I was dissolved in 787 mL of dichloromethane, and then 14.4 g of diethylaluminum chloride was gradually added to react at a temperature of 30° C. for 2 h. After the reaction, 53.39 g of compound II was obtained by column chromatography purification and drying. The reaction formula is shown in formula (1).
[0032] 2) 42.35 g of compound II obtained in step 1) was dissolved in 424 mL of ethanol and mixed with 27 g of o-carboxyphenylacetic acid, and self-assembled at 25° C. to obtain a MOF material.
[0033] 3) Add 424 g of SSZ-13 molecular sieve to the MOF material obtained in step 2), ultrasonically treat for 30 min, and dry at 50 ° C for 12 h to obtain a modified molecular sieve crude material. The molecular sieve crude material is soaked in ethanol for 12 h and then dried for purification. The purified molecular sieve crude material is vacuum activated at 100 ° C for 24 h to obtain a modified molecular sieve.
[0034] SSZ-13 molecular sieve was purchased from Tianjin Puxitang Biopharmaceutical Technology Co., Ltd.
[0035] The volume fraction of ethanol is 95%.
[0036] The molecular sieve of this embodiment is prepared by the molecular sieve modification method of this embodiment.
[0037] Example 2
[0038] The molecular sieve modification method of this embodiment comprises the following steps:
[0039] 1) Under nitrogen protection, 78.7 g of compound I was dissolved in 944 mL of dichloromethane, and then 15.6 g of diethylaluminum chloride was gradually added to react at a temperature of 25° C. for 4 h. After the reaction, 63.82 g of compound II was obtained by column chromatography purification and drying.
[0040] 2) 42.35 g of compound II obtained in step 1) was dissolved in 339 mL of ethanol and mixed with 22.5 g of o-carboxyphenylacetic acid, and self-assembled at 25° C. to obtain a MOF material.
[0041] 3) Add 530 g of SSZ-13 molecular sieve to the MOF material obtained in step 2), ultrasonically treat for 60 min, and dry at 50 ° C for 12 h to obtain a modified molecular sieve crude material. The molecular sieve crude material is soaked in ethanol for 12 h and then dried for purification. The purified molecular sieve crude material is vacuum activated at 120 ° C for 12 h to obtain a modified molecular sieve.
[0042] SSZ-13 molecular sieve was purchased from Tianjin Puxitang Biopharmaceutical Technology Co., Ltd.
[0043] The volume fraction of ethanol is 95%.
[0044] The molecular sieve of this embodiment is prepared by the molecular sieve modification method of this embodiment.
[0045] Example 3
[0046] The molecular sieve modification method of this embodiment comprises the following steps:
[0047] 1) Under nitrogen protection, 78.7 g of compound I was dissolved in 1180 mL of dichloromethane, and then 18 g of diethylaluminum chloride was gradually added to react at a temperature of 30° C. for 3 h. After the reaction, 64.55 g of compound II was obtained by column chromatography purification and drying.
[0048] 2) 42.35 g of compound II obtained in step 1) was dissolved in 508 mL of ethanol and mixed with 31.5 g of o-carboxyphenylacetic acid, and self-assembled at 30° C. to obtain a MOF material.
[0049] 3) Add 355 g of SSZ-13 molecular sieve to the MOF material obtained in step 2), ultrasonically treat for 30 min, and dry at 40 ° C for 24 h to obtain a modified molecular sieve crude material. Soak the molecular sieve crude material in ethanol for 12 h and then dry it for purification. The purified molecular sieve crude material is vacuum activated at 100 ° C for 24 h to obtain a modified molecular sieve.
[0050] SSZ-13 molecular sieve was purchased from Tianjin Puxitang Biopharmaceutical Technology Co., Ltd.
[0051] The volume fraction of ethanol is 95%.
[0052] The molecular sieve of this embodiment is prepared by the molecular sieve modification method of this embodiment.
[0053] Example 4
[0054] The molecular sieve modification method of this embodiment comprises the following steps:
[0055] 1) Under nitrogen protection, 78.7 g of compound I was dissolved in 944 mL of dichloromethane, and then 15.6 g of diethylaluminum chloride was gradually added to react at a temperature of 35° C. for 2 h. After the reaction, 62.77 g of compound II was obtained by column chromatography purification and drying.
[0056] 2) 42.35 g of compound II obtained in step 1) was dissolved in 42.4 mL of ethanol and mixed with 27 g of o-carboxyphenylacetic acid, and self-assembled at 25° C. to obtain a MOF material.
[0057] 3) Add 424 g of SSZ-13 molecular sieve to the MOF material obtained in step 2), ultrasonically treat for 30 min, and dry at 60 ° C for 12 h to obtain a modified molecular sieve crude material. The molecular sieve crude material is soaked in ethanol for 12 h and then dried for purification. The purified molecular sieve crude material is vacuum activated at 120 ° C for 24 h to obtain a modified molecular sieve.
[0058] SSZ-13 molecular sieve was purchased from Tianjin Puxitang Biopharmaceutical Technology Co., Ltd.
[0059] The volume fraction of ethanol is 95%.
[0060] The molecular sieve of this embodiment is prepared by the molecular sieve modification method of this embodiment.
[0061] Example 5
[0062] The molecular sieve modification method of this embodiment comprises the following steps:
[0063] 1) Under nitrogen protection, 78.7 g of compound I was dissolved in 1180 mL of dichloromethane, and then 18 g of diethylaluminum chloride was gradually added to react at a temperature of 25° C. for 3 h. After the reaction, 64.36 g of compound II was obtained by column chromatography purification and drying.
[0064] 2) 42.35 g of compound II obtained in step 1) was dissolved in 339 mL of ethanol and mixed with 22.5 g of o-carboxyphenylacetic acid, and self-assembled at 35° C. to obtain a MOF material.
[0065] 3) Add 303 g of SSZ-13 molecular sieve to the MOF material obtained in step 2), ultrasonically treat for 60 min, and dry at 60 ° C for 24 h to obtain a modified molecular sieve crude material. The molecular sieve crude material is soaked in ethanol for 12 h and then dried for purification. The purified molecular sieve crude material is vacuum activated at 100 ° C for 24 h to obtain a modified molecular sieve.
[0066] SSZ-13 molecular sieve was purchased from Tianjin Puxitang Biopharmaceutical Technology Co., Ltd.
[0067] The volume fraction of ethanol is 95%.
[0068] The molecular sieve of this embodiment is prepared by the molecular sieve modification method of this embodiment.
[0069] The modified molecular sieve obtained in Example 1 is recorded as Sample 1.
[0070] The MOF material obtained in step 2) of Example 1 is recorded as Sample 2.
[0071] Commercially available SSZ-13 molecular sieve was purchased from Tianjin Puxitang Biopharmaceutical Technology Co., Ltd. and recorded as sample 3.
[0072] Test Example 1
[0073] The adsorption amount of carbon dioxide in flue gas by Sample 1-Sample 3 at 40°C and 90°C was measured, and the results are shown in Table 1.
[0074] The simulated gas was a mixture of CO2 and N2, CO2: 20 mL / min; N2: 115 mL / min.
[0075] Adsorbent Adsorption capacity at 40℃ (mg / g) Adsorption capacity at 90℃ (mg / g) Sample 1 357 323 Sample 2 306 102 Sample 3 234 157
[0076] The modified molecular sieve of Example 1 of the present application has a larger adsorption amount of carbon dioxide and better adsorption stability under the condition of higher temperature, and can adsorb carbon dioxide in flue gas at a higher temperature.
Claims
1. A molecular sieve modification method, characterized in that: The following steps are involved: 1) Under nitrogen protection, compound I is dissolved in a solvent, diethylaluminum chloride is gradually added to react, and after the reaction is completed, compound II is purified to obtain the compound. The reaction formula is shown in formula (1); 2) dissolving the compound II in step 1) in ethanol and mixing it with o-carboxyphenylacetic acid to obtain a MOF material through a self-assembly reaction; 3) adding the molecular sieve to the MOF material in step 2), drying after ultrasonic treatment to obtain a crude modified molecular sieve, purifying and activating the crude material to obtain the modified molecular sieve.
2. The molecular sieve modification method according to claim 1, characterized in that: In step 1), the molar ratio of compound I to diethylaluminum chloride is 1:1.2-1.5, the reaction time is 2-4 hours, and the reaction temperature is 25-35°C.
3. The molecular sieve modification method according to claim 1, characterized in that: In step 1), the solvent is dichloromethane, and 10 to 15 mL of the solvent is added for every gram of the compound I.
4. The molecular sieve modification method according to claim 1, characterized in that: The temperature of the self-assembly reaction in step 2) is 25-35°C.
5. The molecular sieve modification method according to claim 1, characterized in that: In step 2), the molar ratio of compound II to o-carboxyphenylacetic acid is 1:2.5 to 1:3.5; 8 to 12 mL of ethanol is added for every gram of compound II.
6. The molecular sieve modification method according to claim 1, characterized in that: The molecular sieve in step 3) is SSZ-13 molecular sieve.
7. The molecular sieve modification method according to claim 1, characterized in that: The mass ratio of the molecular sieve to compound II in step 3) is 10:0.8 to 10:1.
2.
8. The molecular sieve modification method according to claim 1, characterized in that: In step 3), the ultrasonic treatment time is 30 to 60 minutes, the drying temperature is 40 to 60° C., and the drying time is 12 to 24 hours.
9. The molecular sieve modification method according to claim 1, characterized in that: The purification method is: using ethanol to soak and wash the modified molecular sieve crude material and drying it; the activation method is vacuum activation at 100-120° C. for 12-24 hours.
10. A modified molecular sieve, characterized in that: The molecular sieve is prepared by the molecular sieve modification method of claim 1.
Citation Information
Patent Citations
Supported metalloporphyrin complex as well as preparation method and application thereof
CN114989207A
Hydrophobic modified molecular sieve capable of adsorbing carbon dioxide and preparation method thereof
CN117088383A
Synthesis of modified SSZ-16 zeolite molecular sieve and application of modified SSZ-16 zeolite molecular sieve in CO2 adsorption separation
CN117383578A
Modified activated transition metal molecular sieve and application thereof
CN117602639A
Modified particle, support, catalyst component for addition polymerization, catalyst for addition polymerization, and process for producing addition polymer