Anti-segregation agent, light cross-strength concrete and preparation method of light cross-strength concrete
By using anti-segregation agents prepared from components such as polyacrylamide, sodium carboxymethyl starch and xanthan gum in lightweight cross-reinforced concrete, an interpenetrating network structure is formed, which solves the problem of fluidity and cohesion of lightweight cross-reinforced concrete. It solves the problem of imbalance, significantly improves its fluidity and strength, and improves construction performance and anti-seepage performance.
Patent Information
- Application Number
- CN202410823041.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The fluidity and cohesion of lightweight cross-strength concrete are easily imbalanced during configuration, leading to separation and segregation, affecting its working performance and construction stability.
An anti-segregation agent prepared from polyacrylamide, sodium carboxymethyl starch and xanthan gum to form an interpenetrating network structure, improve the bonding performance between cement slurry and aggregates, and work with polycarboxylic acid to reduce water It is used in combination as an admixture to improve the fluidity and strength of concrete.
It significantly improves the fluidity, water retention, durability and strength of lightweight cross-reinforced concrete, prevents bleeding and delamination, and enhances its construction performance and impermeability.
Smart Images

Figure FDA0004909636430000011 
Figure FDA0004909636430000012 
Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of concrete, and in particular to an anti-segregation agent, a lightweight cross-reinforced concrete and a preparation method thereof. Background Art
[0002] Concrete is one of the most important civil engineering materials in contemporary times. Among them, Lightweight High-Strength Concrete (LHSC) is a special type of concrete that combines the two characteristics of light weight and high strength. It is suitable for civil construction projects such as high-rise buildings, bridges, tunnels and underground projects. The difference between lightweight high-strength concrete and ordinary concrete is that there are many voids inside. It is mainly composed of light coarse aggregate, light fine aggregate, cement, water, admixtures and other materials.
[0003] In order to ensure that lightweight cross-sectional concrete has sufficient strength, the amount of cement used in lightweight cross-sectional concrete is relatively higher than that of ordinary concrete of the same strength grade. Therefore, when preparing concrete, the fluidity and cohesion are easily out of balance. When the cohesion is low, the concrete is prone to phase separation under its own gravity or other external forces, destroying the uniformity and stability of the material composition, resulting in separation, which will lead to water seepage and segregation, and finally stratification, increasing the possibility of pump blockage. Therefore, it is necessary to design an anti-segregation agent that can meet the requirements of lightweight cross-sectional concrete to improve the working performance of concrete. Summary of the invention
[0004] In order to solve or partially solve the problems existing in the related art, the present application provides an anti-segregation agent, a lightweight cross-sectional concrete and a preparation method thereof. When the anti-segregation agent is used in the lightweight cross-sectional concrete, it can fill in part of the pores of the concrete, form an interpenetrating network structure with cement hydration products, improve the bonding performance between cement slurry and aggregate, and significantly improve the fluidity and strength of the lightweight cross-sectional concrete, so that the lightweight concrete has light weight, high strength and good working performance.
[0005] The first aspect of the present application provides an anti-segregation agent, comprising the following components in proportion by weight:
[0006]
[0007]
[0008] In some embodiments of the present application, the mass ratio of polyacrylamide, sodium carboxymethyl starch and xanthan gum is (1.25-1.5):1:1.
[0009] In some embodiments of the present application, the molecular weight of the polyacrylamide is in the range of 20,000-180,000.
[0010] In some embodiments of the present application, the steps of preparing the anti-segregation agent include:
[0011] Calcium sulphoaluminate, silica fume and sodium carboxymethyl starch are dispersed in water, stirred at a speed of 150-250 rpm, polyacrylamide and xanthan gum are added, heated to 150-200°C and stirred, then filtered, dried and crushed into anti-segregation agent powder with a particle size of less than 15 μm.
[0012] A second aspect of the present application provides a lightweight cross-reinforced concrete, comprising the following components in proportion by mass:
[0013]
[0014] The fine aggregate includes clay pottery sand and natural river sand in a mass ratio of (1-3):1;
[0015] The admixture is a composite of a polycarboxylate water reducer and the anti-segregation agent.
[0016] In some embodiments of the present application, in the admixture, the anti-segregation agent is added in an amount of 3wt%-10wt% of the polycarboxylate water-reducing agent.
[0017] In some embodiments of the present application, the limestone-fly ash composite admixture includes limestone powder, fly ash and steel fiber in a mass ratio of (40-50):(20-30):1.
[0018] In some embodiments of the present application, the clay ceramsite and clay sand are obtained by mixing clay, diatomaceous earth and xanthan gum, pressing and molding, and then drying and calcining;
[0019] The calcination temperature is 600-780°C.
[0020] In some embodiments of the present application, the particle size of the clay pellets is 5-20 mm, and the apparent density of the clay pellets is greater than 1750 kg / m 3 ;
[0021] The fineness modulus of the natural river sand and clay pottery sand is 2.5-2.8;
[0022] The cement is PO42.5 cement.
[0023] The third aspect of the present application provides a method for preparing lightweight cross-reinforced concrete, comprising the following steps:
[0024] Mix the admixture and cement evenly, and then add some water to mix into a prefabricated slurry;
[0025] The coarse aggregate and the fine aggregate are mixed, and then the limestone-fly ash composite admixture and the remaining water are added and mixed evenly, and finally the prefabricated slurry is added and stirred evenly to obtain lightweight cross-strength concrete.
[0026] The technical solution provided by this application may have the following beneficial effects:
[0027] The anti-segregation agent of the embodiment of the present application, when used in lightweight cross-linked reinforced concrete, can fill part of the pores in the concrete, form an interpenetrating network structure with cement hydration products, improve the bonding performance between cement slurry and aggregate, and significantly improve the fluidity, water retention, adhesion to the substrate, water tightness, durability and strength of the lightweight cross-linked reinforced concrete.
[0028] The lightweight cross-reinforced concrete of the embodiment of the present application is compounded with clay ceramsite and lightweight aggregate, and an anti-segregation agent is mixed with a polycarboxylic acid water-reducing agent and used as an admixture. It can maintain good fluidity in the concrete production process while reducing the water-cement ratio. At the same time, the high-strength network structure formed between the admixture, cement and limestone-fly ash composite admixture can be used to tightly connect the aggregate and cement slurry, thereby improving the strength, impermeability and crack resistance of the lightweight concrete; and a special limestone-fly ash composite admixture and clay ceramsite, clay sand, natural river sand, etc. are used as structural supporting materials for the lightweight concrete, and the grading effect is good. The materials support each other, which can further improve the strength of the lightweight concrete and can be applied to more construction projects.
[0029] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. DETAILED DESCRIPTION
[0030] To make the present invention easy to understand, the present invention will be described in detail below. However, before describing the present invention in detail, it should be understood that the present invention is not limited to the specific embodiments described. It should also be understood that the terms used herein are only for describing specific embodiments and are not intended to be limiting.
[0031] The terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The singular forms of "a", "said" and "the" used in this application and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.
[0032] Where a numerical range is provided, it is to be understood that each intermediate value between the upper and lower limits of the range and any other provisions or intermediate values in the specified range is encompassed within the present invention. The upper and lower limits of these smaller ranges may be independently included in the smaller ranges and are also encompassed within the present invention, subject to any explicitly excluded limits in the specified range. Where a specified range includes one or two limits, the scope excluding any or both of those included limits is also encompassed within the present invention. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically limited.
[0033] Unless otherwise defined, all terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. Although any methods and materials or equivalent methods and materials described herein can also be used in the practice or testing of the present invention, preferred methods and materials are now described.
[0034] In order to ensure that lightweight cross-sectional reinforced concrete has sufficient strength, the amount of cement used in lightweight cross-sectional reinforced concrete is more than that of ordinary concrete of the same strength grade. Therefore, the fluidity and cohesion are easily out of balance when configuring the concrete. When the cohesion is low, the concrete is prone to phase separation under its own gravity or other external forces, destroying the uniformity and stability of the material composition, leading to separation, which will cause water seepage and segregation, and ultimately lead to stratification, increasing the possibility of pump blockage.
[0035] In response to the above problems, the embodiments of the present application provide an anti-segregation agent, which is suitable for lightweight cross-reinforced concrete, can improve the cohesion and fluidity of lightweight cross-reinforced concrete, maintain the uniformity of concrete, help prevent the separation of aggregate and cement slurry during transportation and pouring, and facilitate concrete pumping, and has good working performance.
[0036] The anti-segregation agent of the embodiment of the present application includes the following components in proportion by weight:
[0037]
[0038] When the anti-segregation agent obtained by compounding the above materials is used in lightweight cross-reinforced concrete, it can fill part of the pores in the concrete, form an interpenetrating network structure with cement hydration products, improve the bonding performance between cement slurry and aggregate, and significantly improve the fluidity, water retention, adhesion with the substrate, water tightness, durability and strength of lightweight cross-reinforced concrete.
[0039] Among them, polyacrylamide is a high molecular polymer synthesized from acrylamide monomer through free radical polymerization reaction; sodium carboxymethyl starch is a sodium salt generated by introducing carboxymethyl groups on the hydroxyl groups of starch molecules and then sodiumizing them; xanthan gum is an extracellular acidic heteropolysaccharide produced by fermentation of Xanthomonas, and its secondary structure is a rod-shaped double helix structure formed by the side chains winding around the main chain skeleton in reverse and maintained by hydrogen bonds. Through the combination of polyacrylamide, sodium carboxymethyl starch and xanthan gum, the intermolecular interaction after compounding can form a high-strength tertiary network structure, thereby significantly improving the bonding properties of cement slurry and aggregate, and it has high water absorption, can maintain a moist environment inside the concrete, reduce shrinkage caused by water evaporation, and control the cement hydration rate, thereby improving the early strength, durability, crack resistance and construction performance of the concrete, and can improve the pore structure inside the lightweight cross-reinforced concrete and improve the concrete's impermeability.
[0040] Calcium aluminum sulfate can react with water to generate calcium sulfoaluminate hydrate, producing an expansion effect, which can be used to compensate for the shrinkage of concrete; silica fume is mainly composed of silicon dioxide, which can fill the pore structure inside the concrete. When calcium aluminum sulfate, silica fume, polyacrylamide, sodium carboxymethyl starch and xanthan gum are used in combination, they are filled in the network structure and connected to the network structure through intermolecular interactions to obtain a high-strength anti-segregation agent component. When it is used in concrete preparation, its internal structure can significantly reduce the exudation of moisture in the concrete and the settlement of coarse aggregate, thereby maintaining the uniformity of the lightweight concrete mixture, optimizing the internal structure of the lightweight concrete mixture, making it denser, and improving the strength of the lightweight concrete. It also improves the workability of the concrete, reduces the generation of pores and microcracks, and thus improves the early strength and durability of the concrete.
[0041] In some specific embodiments, the mass ratio of polyacrylamide, sodium carboxymethyl starch and xanthan gum is (1.25-1.5): 1: 1, such as 1.25: 1: 1, 1.3: 1: 1, 1.35: 1: 1, 1.4: 1: 1, 1.45: 1: 1, 1.5: 1: 1; preferably 1.3: 1: 1. By optimizing the ratio of polyacrylamide, sodium carboxymethyl starch and xanthan gum, it is helpful to improve the stability of the cross-linked network structure, thereby being able to improve the strength and impermeability of lightweight concrete while reducing the amount of cement components added, which is more conducive to its application in water conservancy construction projects.
[0042] In some specific embodiments, the molecular weight of polyacrylamide is in the range of 20,000-180,000, specifically, for example, 20,000, 50,000, 80,000, 100,000, 120,000, 150,000, 180,000, etc., preferably 120,000-150,000.
[0043] In some specific embodiments, the molecular weight range of sodium carboxymethyl starch is 1200000-3000000, specifically, for example, 1200000, 1500000, 2000000, 2500000, 3000000, etc., preferably 2000000-3000000.
[0044] By selecting polyacrylamide and sodium carboxymethyl starch with appropriate molecular weights, the viscosity can be within an appropriate range. The micro-hydrated film can be condensed on the surface of cement slurry and aggregate, and the intermolecular interaction force can form a connection with the cement slurry and aggregate, thereby improving the bonding performance between the cement slurry and the aggregate, and reducing the damage to the concrete structure caused by the stress generated when the cement slurry shrinks. The good viscosity can make the concrete have a good water retention effect, and the concrete material has good uniformity and stability, reducing the bleeding, segregation and stratification of the concrete, and improving the working performance of lightweight concrete.
[0045] In some embodiments, the calcium sulfoaluminate has a particle size of less than 9 μm.
[0046] In some embodiments, the particle size of the silica fume is less than 9 μm.
[0047] Calcium sulfoaluminate and silica fume with smaller particle sizes can be deposited on the surface of cement slurry and aggregate in the form of microparticles after forming the anti-segregation agent, thereby maintaining good viscosity and water retention, reducing the amount of cement materials while ensuring that the lightweight concrete has good strength; and because polyacrylamide, sodium carboxymethyl starch and xanthan gum are connected to the surface of silica fume and calcium sulfoaluminate, the expansion capacity of the anti-segregation agent can be controlled within a suitable range, thereby improving the durability and anti-cracking effect of the lightweight concrete, while ensuring that the concrete has suitable fluidity and the construction performance of the concrete.
[0048] In some specific embodiments, the preparation steps of the anti-segregation agent include: dispersing calcium sulfoaluminate, silica fume, and sodium carboxymethyl starch in water, stirring at a speed of 150-250 rpm, adding polyacrylamide and xanthan gum, heating to 150-200°C and stirring, then filtering, drying, and crushing to an anti-segregation agent powder with a particle size of less than 15 μm.
[0049] Specifically, under heating conditions, the mixing of the components can be accelerated to avoid incomplete reaction caused by component separation, thereby ensuring that the components in the anti-segregation agent can cooperate with each other, which is beneficial to improving its cohesiveness and fluidity during the preparation of lightweight concrete and ensuring that the lightweight concrete has good working performance.
[0050] When the anti-segregation agent of the embodiment of the present application is used in lightweight concrete, it is added in the form of an admixture, so that it reacts with cement slurry and aggregate, and is deposited on the surface of cement slurry and aggregate in the form of a micro-hydrated film to connect the cement slurry and aggregate, thereby improving the cohesion and fluidity of the concrete, so that the lightweight concrete can reduce the amount of cement while ensuring sufficient strength, and has good fluidity, which is beneficial to the pumping of the concrete.
[0051] The lightweight cross-reinforced concrete of the embodiment of the present application includes the following components in proportion by weight:
[0052]
[0053] The admixture contains a compound of a polycarboxylate water-reducing agent and the anti-segregation agent. When the polycarboxylate water-reducing agent and the anti-segregation agent are added to the lightweight traffic-strengthening concrete in a relatively small amount, the fluidity and cohesiveness of the lightweight traffic-strengthening concrete can be significantly improved, so that the aggregate and cement paste in the concrete are not easy to separate, and good uniformity and stability are ensured, thereby reducing the possibility of bleeding, segregation and stratification of the concrete, ensuring that the concrete has good working performance, and facilitating the pumping of the lightweight traffic-strengthening concrete.
[0054] In some specific embodiments, the amount of the anti-segregation agent added in the admixture is 3wt%-10wt% of the polycarboxylate water-reducing agent, such as 3wt%, 5wt%, 6wt%, 8wt%, 10wt%, etc., preferably 5wt%-8wt%. When the polycarboxylate water-reducing agent doped with a small amount of anti-segregation agent is used in lightweight cross-reinforced concrete, it can avoid the phenomenon of excessive concrete moisture caused by the sensitivity of the polycarboxylate water-reducing agent to produce, resulting in late bleeding and segregation of the concrete, and ensure that the concrete has good strength, durability and impermeability.
[0055] In some specific embodiments, in the lightweight cross-reinforced concrete, the amount of admixture added is 1wt%-3wt% of cement, such as 1wt%, 1.8wt%, 2wt%, 2.5wt%, 2.8wt%, 3wt%, etc., preferably 2wt%-2.5wt%. By optimizing the amount of admixture added in the lightweight cross-reinforced concrete, the components of the polycarboxylate water-reducing agent and the anti-segregation agent in the concrete can be fully coordinated, which can ensure that the concrete has good fluidity and good cohesion during the production process, so that the concrete has good pumping performance during the production process, is not prone to bleeding, segregation and stratification, and is not prone to excessive moisture in the concrete structure affecting the strength and durability of the concrete.
[0056] In some embodiments, the cement is PO42.5 cement.
[0057] In some specific embodiments, the limestone-fly ash composite admixture includes limestone powder, fly ash and steel fiber in a mass ratio of (40-50):(20-30):1, preferably in a mass ratio of (45-48):(20-25):1; further preferably in a mass ratio of 45:25:1. The surface of limestone powder is smooth and the water consumption is low. It can improve the shrinkage effect caused by self-drying and reduce the slump loss. At the same time, it can also react with cement to hydrate and improve the strength of concrete. Fly ash has volcanic ash characteristics. The silicate in it undergoes chemical reactions such as dissolution and polymerization under the action of alkaline substances, which can improve the shrinkage resistance and anti-seepage performance of concrete. The steel fiber is a milled steel fiber with bent ends and a length of less than 1mm. When the limestone and fly ash composite admixture is used in the production of lightweight concrete, on the one hand, the limestone and fly ash will work together with cement, water and admixtures to form a network structure with high structural strength. The steel fibers, aggregates, etc. are distributed in the network structure, which can significantly improve the strength, crack resistance and tensile strength of lightweight concrete, and improve the durability and anti-seepage performance of concrete. It is especially suitable for construction projects such as tunnels, dams, road pavements, floor slabs, bridges, etc.
[0058] The lightweight concrete of the embodiment of the present application has a water-cement ratio of 0.42-0.52. Through the combined use of the anti-segregation agent of the embodiment of the present application and the components in the lightweight concrete, the strength and impermeability of the concrete can be increased while reducing the water-cement ratio, while ensuring that the concrete production process has good fluidity, uniformity and stability, has good working performance, and is conducive to the pumping of the concrete.
[0059] In some specific embodiments, the fine aggregate includes clay sand and natural river sand in a mass ratio of (1-3):1, specifically, the mass ratio may be, for example, 1:1, 1.5, 2:1, 2.5:1, 3:1, preferably 2:1. The fineness modulus of the clay sand and natural river sand is 2.5-2.8.
[0060] In some specific embodiments, the particle size of the clay ceramsite is 5-20 mm, preferably 10-20 mm graded clay ceramsite, and the apparent density of the clay ceramsite is greater than 1750 kg / m 3 .
[0061] In some specific embodiments, clay ceramsite and clay sand are obtained by mixing clay, diatomaceous earth and xanthan gum, pressing and molding, drying and then calcining, and the calcination temperature is 600-780° C. Clay ceramsite and clay sand obtained by mixing diatomaceous earth and xanthan gum can maintain their characteristics of lightness, porosity, and air permeability, and can effectively improve their structural strength and crack resistance, which is conducive to their application in more construction projects.
[0062] In some specific embodiments, the mass ratio of clay, diatomaceous earth and xanthan gum in the clay pellet is (75-90):(10-25):(0.5-3), preferably (77-85):(15-20):1; and the calcination temperature is 600-750°C.
[0063] In some specific embodiments, the mass ratio of clay, diatomaceous earth and xanthan gum in the clay ceramsite is (80-90):(10-20):(1-3), preferably (82-87):(15-17):1.2; the calcination temperature is 700-780° C. By optimizing the ratio of clay, diatomaceous earth and xanthan gum, the content of each element in the clay ceramsite is adjusted so that the clay ceramsite meets the requirements of light weight and high strength to adapt to the conditions of construction engineering.
[0064] The lightweight cross-reinforced concrete of the embodiment of the present application is compounded with clay ceramsite and lightweight aggregate, and an anti-segregation agent is mixed with a polycarboxylic acid water-reducing agent and used as an admixture. It can maintain good fluidity in the concrete production process while reducing the water-cement ratio. At the same time, the high-strength network structure formed between the admixture, cement and limestone-fly ash composite admixture can be used to tightly connect the aggregate and cement slurry, thereby improving the strength, impermeability and crack resistance of the lightweight concrete; and a special limestone-fly ash composite admixture and clay ceramsite, clay sand, natural river sand, etc. are used as structural supporting materials for the lightweight concrete, and the grading effect is good. The materials support each other, which can further improve the strength of the lightweight concrete and can be applied to more construction projects.
[0065] The lightweight cross-reinforced concrete of the embodiment of the present application is prepared by the following preparation method:
[0066] S1. Mix the anti-segregation agent and the polycarboxylate water-reducing agent in proportion to obtain an admixture;
[0067] S2, mixing the admixture and cement evenly, and then adding part of water to mix into a prefabricated slurry;
[0068] S3, clay ceramsite and fine aggregate are mixed, and then limestone-fly ash composite admixture and the remaining water are added and mixed evenly, and finally prefabricated slurry is added and stirred evenly to obtain lightweight cross-strength concrete.
[0069] The method for preparing lightweight cross-sectional reinforced concrete in the embodiment of the present application uniformly disperses the admixture and cement materials in the prefabricated slurry prepared by uniformly mixing the admixture and cement, which is beneficial to the interaction between the components in the admixture and cement. The clay pellets and fine aggregates are pre-mixed and prepared in advance, which can also make the coarse and fine aggregates uniformly dispersed, and can reduce the probability of segregation, stratification and the like caused by the deposition of coarse aggregate or fine aggregate due to its own gravity. When the prefabricated slurry is mixed with the uniformly mixed aggregate, the slurry can be uniformly wrapped on the surface of the aggregate, thereby forming a high-strength bonding force between the coarse aggregate and the fine aggregate, and preparing a high-strength lightweight cross-sectional reinforced concrete; at the same time, due to the effect of the anti-segregation agent in the admixture, sufficient fluidity and cohesion can be maintained when the prefabricated slurry and the aggregate are mixed.
[0070] In order to make the present invention easier to understand, the present invention will be further described in detail below in conjunction with examples, which are merely illustrative and are not intended to limit the scope of application of the present invention. The raw materials or components used in the present invention can be obtained by commercial routes or conventional methods unless otherwise specified.
[0071] Preparation Example 1
[0072] The preparation steps of the anti-segregation agent include: dispersing 1.5kg of calcium sulfoaluminate, 0.5kg of silica fume, and 1.2kg of sodium carboxymethyl starch (molecular weight 2500000) in 3L of water, stirring at a speed of 200 rpm, adding 2.8kg of polyacrylamide (molecular weight 120000) and 1kg of xanthan gum, heating to 180°C and stirring, then filtering, drying, and crushing into anti-segregation agent powder with a particle size of less than 15μm.
[0073] Preparation Example 2-3
[0074] The difference from Preparation Example 1 is that the components of the anti-segregation agent are as shown in Table 1.
[0075] Table 1
[0076]
[0077] Preparation Example 4
[0078] The difference from Preparation Example 1 is that the molecular weight of polyacrylamide is 15,000, and the molecular weight of sodium carboxymethyl starch is 4,000,000.
[0079] Preparation Example 5
[0080] The difference from Preparation Example 1 is that the molecular weight of polyacrylamide is 250,000, and the molecular weight of sodium carboxymethyl starch is 1,000,000.
[0081] Preparation Example 6
[0082] The difference from Preparation Example 1 is that the anti-segregation agent does not contain sodium carboxymethyl starch.
[0083] Preparation Example 7
[0084] The difference from Preparation Example 1 is that the anti-segregation agent does not contain calcium sulfoaluminate.
[0085] Example 1
[0086] A lightweight cross-reinforced concrete is prepared by the following preparation method:
[0087] S1. Weigh the anti-segregation agent of Preparation Example 1 according to 5 wt% of the polycarboxylate water-reducing agent, and mix it evenly with the polycarboxylate water-reducing agent to obtain an admixture;
[0088] S2, mix 0.1kg admixture with 20kg cement, then add 10L water to mix into prefabricated slurry;
[0089] S3, 65kg of clay ceramsite, 40kg of clay sand, and 20kg of natural river sand were mixed, and then 16kg of limestone-fly ash composite admixture (the mass ratio of limestone ore powder, fly ash and steel fiber is 45:25:1) and 1.2L were added and mixed evenly, and finally the prefabricated slurry was added and stirred evenly to obtain lightweight cross-reinforced concrete.
[0090] Among them, the mass ratio of clay, diatomaceous earth and xanthan gum in clay pellets is 81:18:1; the calcination temperature is 750°C; the mass ratio of clay, diatomaceous earth and xanthan gum in clay sand is 83.8:15:1.2; the calcination temperature is 750°C.
[0091] Embodiment 2-5
[0092] The difference from Example 1 is that the anti-segregation agents of Preparation Examples 2-5 are selected respectively.
[0093] Embodiment 6-8
[0094] The difference from Example 3 is that the components of the lightweight concrete are as shown in Table 2.
[0095] Table 2
[0096]
[0097] Example 9
[0098] The difference from Example 3 is that the preparation process of clay ceramsite and clay sand does not contain xanthan gum.
[0099] Comparative Example 1-2
[0100] The difference from Example 1 is that the anti-segregation agents of Preparation Example 6 and Preparation Example 7 are respectively selected.
[0101] Comparative Example 3
[0102] The difference from Example 1 is that the external additive does not contain an anti-segregation agent.
[0103] Comparative Example 4
[0104] The difference from Example 1 is that the limestone-fly ash composite admixture does not contain steel fiber.
[0105] Performance Testing
[0106] The test was carried out in accordance with GB / T50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures", and the test results are shown in Table 3.
[0107] Table 3
[0108]
[0109] It can be seen from the lightweight concrete of Examples 1-9 that their water bleeding rates are all 0, while the lightweight concrete using anti-segregation agents different from those prepared in the present application, such as Comparative Example 1 and Comparative Example 2, has water bleeding rates of 1.5% and 0.8%, respectively, while the lightweight concrete without adding the anti-segregation agent has a water bleeding rate of 7.4%. It can be seen that the use of the anti-segregation agent shown in the embodiments of the present application plays an important role in preventing water bleeding, segregation and stratification of lightweight concrete, can effectively improve the working performance of concrete, and is beneficial to the pumping of concrete.
[0110] According to the lightweight concrete shown in Examples 1-5, when the molecular weight of polyacrylamide and sodium carboxymethyl starch in the anti-segregation agent is too high or too low, it will affect its viscosity, and thus affect the effect of the anti-segregation agent. When it is applied to lightweight concrete, it will affect the compressive strength of the lightweight concrete, which is not conducive to the lightweight concrete maintaining good durability.
[0111] According to the lightweight concrete shown in Example 3 and Examples 6-8, it can be seen that when the amount of admixture added and the water-cement ratio of the lightweight concrete are between 0.42 and 0.52, the synergistic effect between the components in the concrete is good, which can not only maintain good fluidity, that is, the lightweight concrete has good working performance during the production process, but also enhance the interaction between the network structure formed by the cementitious material and the admixture and the aggregate, thereby improving the strength of the lightweight concrete, so that the concrete has the characteristics of lightness and high strength at the same time.
[0112] It can be seen from the lightweight concrete shown in Example 3 and Example 9 that the use of clay ceramsite and clay sand with added xanthan gum is beneficial to improving the strength and stability of aggregates. When applied to lightweight concrete, it is beneficial to improve the strength of lightweight concrete.
[0113] It can be seen from the lightweight concrete shown in Example 1 and Comparative Example 4 that when steel fibers are added to the lightweight concrete, it is beneficial to improve the overall strength of the lightweight concrete.
[0114] The embodiments of the present application have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
Claims
1. An anti-segregation agent, characterized in that: The composition comprises the following components in proportion by weight:
2. The anti-segregation agent according to claim 1, characterized in that: The mass ratio of the polyacrylamide, sodium carboxymethyl starch and xanthan gum is (1.25-1.5):1:
1.
3. The anti-segregation agent according to claim 1, characterized in that: The molecular weight of the polyacrylamide is in the range of 20,000-180,000.
4. The anti-segregation agent according to claim 1, characterized in that The preparation steps of the anti-segregation agent include: Calcium sulphoaluminate, silica fume and sodium carboxymethyl starch are dispersed in water, stirred at a speed of 150-250 rpm, polyacrylamide and xanthan gum are added, heated to 150-200°C and stirred, then filtered, dried and crushed into anti-segregation agent powder with a particle size of less than 15 μm.
5. A lightweight reinforced concrete, characterized in that: The invention comprises the following components in proportion by weight: The fine aggregate includes clay pottery sand and natural river sand in a mass ratio of (1-3):1; The admixture is a composite of a polycarboxylate water reducer and the anti-segregation agent according to any one of claims 1 to 4.
6. The lightweight cross-reinforced concrete according to claim 5, characterized in that: In the admixture, the anti-segregation agent is added in an amount of 3wt%-10wt% of the polycarboxylate water-reducing agent.
7. The lightweight cross-reinforced concrete according to claim 5, characterized in that: The limestone-fly ash composite admixture comprises limestone mineral powder, fly ash and steel fiber in a mass ratio of (40-50):(20-30):
1.
8. The lightweight cross-reinforced concrete according to claim 5, characterized in that: The clay ceramsite and clay sand are obtained by mixing clay, diatomaceous earth and xanthan gum, pressing and molding, drying and calcining. The calcination temperature is 600-780°C.
9. The lightweight cross-reinforced concrete according to claim 8, characterized in that: The particle size of the clay ceramsite is 5-20 mm, and the apparent density of the clay ceramsite is greater than 1750 kg / m 3 ; The fineness modulus of the natural river sand and clay pottery sand is 2.5-2.8; The cement is PO42.5 cement.
10. A method for preparing lightweight cross-reinforced concrete, characterized in that: The following steps are involved: Mix the admixture and cement evenly, and then add some water to mix into a prefabricated slurry; The coarse aggregate and the fine aggregate are mixed, and then the limestone-fly ash composite admixture and the remaining water are added and mixed evenly, and finally the prefabricated slurry is added and stirred evenly to obtain lightweight cross-strength concrete.