Indium tin zinc oxide target material with high mobility and preparation method thereof

Through a two-step oscillating pressure sintering and ball milling granulation process, the problems of low density and large grain size of IGZO targets during high-temperature sintering are solved, and a high-mobility indium tin zinc oxide target is prepared, which is suitable for new displays and Optoelectronic applications.

CN118771879AActive Publication Date: 2024-10-15ZHENGZHOU UNIV

Patent Information

Application Number
CN202411036295.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Existing IGZO targets cause abnormal grain growth and low density during the high-temperature sintering process, and cannot meet the needs of new displays for improving the field-effect mobility of thin film transistors.

Method used

A two-step oscillating pressure sintering process combined with a ball milling granulation process is used to control the relative density and grain size of the indium tin zinc oxide target by applying gradually increasing pressure and oscillating pressure in the mold to prepare high mobility indium tin oxide Zinc target.

Benefits of technology

The high mobility of the indium tin zinc oxide target material is achieved, the relative density is not less than 99.5%, the grain size is between 2 and 5 μm, and the resistivity is between 3 and 10 mΩ·cm. It is suitable for displays and other optoelectronic applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118771879A_ABST
    Figure CN118771879A_ABST
Patent Text Reader

Abstract

The embodiment of the invention discloses an indium tin zinc oxide target material with high mobility and a preparation method thereof. The method comprises the step of carrying out two-step oscillation pressure sintering treatment on spherical granules prepared from In2O3 powder, ZnO powder, SnO2 powder and metal oxide-doped powder, and specifically comprises the following steps: pre-pressing the spherical granulation powder in a mold under a first pressure; heating the pre-pressed spherical granulation powder to a first temperature; linearly increasing a first pressure applied to the mold to a second pressure before the temperature reaches the first temperature; performing first heat preservation at the first temperature and the second pressure; in the first heat preservation stage, the superposition frequency is 1-2 Hz, and the oscillation pressure is 5-10 MPa; maintaining the second pressure and cooling to a second temperature; performing second-time heat preservation at second temperature and second pressure, and applying oscillation pressure with the same size and frequency as the first-time heat preservation stage; after the second heat preservation stage is finished, heating is stopped, the external oscillation pressure is removed, and the temperature is reduced to 1000 DEG C; and cooling to room temperature along with the furnace.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sputtering target materials, and in particular relates to an indium tin zinc oxide target material with high mobility and a preparation method thereof. Background Art

[0002] Amorphous oxide semiconductor thin film transistors are widely used in active matrix displays such as liquid crystal displays or organic light-emitting diodes. In-Ga-Zn-O (IGZO) has become the first commercially successful thin film transistor due to its excellent properties such as high mobility, low leakage current and steep subthreshold swing. However, with the demand for ultra-high resolution and frame rate, the typical mobility μFE of IGZO widely used in industry is about 10 cm 2 / V·s, can no longer meet the requirements of new displays, and the field effect mobility μFE of thin film transistors needs to be further improved.

[0003] Compared with α-IGZO thin film transistors, due to In 3+ and Sn 4+ With similar 5s orbitals, In-Sn-Zn-O (ITZO) thin film transistors have the potential for high μFE, greater than 20 cm 2 ·V -1 ·s -1 Replacing part of In with Sn can reduce the manufacturing cost of thin-film transistors. On the other hand, ITZO thin-film transistors have a larger band gap, which can achieve higher transparency in the visible light range, making them very suitable for use in displays and other optoelectronic applications.

[0004] ITZO targets are usually densified by sintering in a high-temperature environment. Due to long-term heat preservation at high temperature, abnormal grain growth will inevitably occur in the grains and their density is relatively low. As the key basic material for transparent conductive oxide thin films, the relative density and grain size of the target will affect the density and chemical state of the film, thereby affecting the mobility and stability of the thin film transistor. However, the existing technology still has problems such as low relative density of the target, large grain size, high sintering temperature, and long sintering time. Summary of the invention

[0005] In view of this, on the one hand, some embodiments disclose a method for preparing an indium tin zinc oxide target with high mobility, comprising the steps of:

[0006] S1, In2O3 powder, ZnO powder, SnO2 powder and doped metal oxide powder are prepared into slurry; the doped metal oxide is an oxide of a low electronegativity metal element with different valence states;

[0007] S2, ball milling the slurry;

[0008] S3, the ball-milled slurry is mixed with a binder and spray-granulated to obtain spherical granulated powder;

[0009] S4, the spherical granulated powder is subjected to two-step oscillation pressure sintering treatment to obtain an indium tin zinc oxide target with high mobility;

[0010] Among them, the two-step oscillation pressure sintering process includes:

[0011] The spherical granulated powder is pre-pressed in a mold under a first pressure; the first pressure is 5-8Mpa;

[0012] The pre-pressed spherical granulated powder is heated to a first temperature at a heating rate of 5°C / min; before the temperature reaches the first temperature, the first pressure applied to the mold is linearly increased to a second pressure, the pressure is increased by 2 to 5 MPa at a time, and the increasing rate does not exceed 0.1 MPa / min; the first temperature is 1450 to 1500°C, and the second pressure is 30 to 40 MPa;

[0013] Performing a first heat preservation stage at a first temperature and a second pressure; superimposing an oscillating pressure with a frequency of 1 to 2 Hz and an amplitude of 5 to 10 MPa during the first heat preservation stage;

[0014] Maintaining a second pressure of 30-40 MPa, cooling the temperature to a second temperature at a cooling rate of 5°C / min; the second temperature is 1400-1450°C;

[0015] Performing a second insulation stage at a second temperature and a second pressure; wherein the second insulation stage applies an oscillating pressure of the same magnitude and frequency as the first insulation stage;

[0016] After the second heat preservation stage, the heating was stopped, the external oscillation pressure was removed, the cooling rate was set to 8°C / min, and the second pressure was maintained until the furnace temperature dropped to 1000°C; then the furnace was cooled to room temperature.

[0017] Further, in some embodiments, the preparation method of the indium tin zinc oxide target with high mobility is disclosed, and the doped metal oxide powder is Pr6O 11 One of powder, Al2O3 powder, La2O3 powder, HfO2 powder, ZrO2 powder, Nb2O5 powder, V2O5 powder, WO3 powder or MoO3 powder.

[0018] Some embodiments disclose a method for preparing an indium tin zinc oxide target with high mobility, wherein the mass ratio of In2O3 powder, ZnO powder and SnO2 powder is 20-23:20-27:50-60, the ratio of doped metal oxide to the total mass of the powder is 0.05-5:100; and the total mass content of the powder in the slurry is 50-70%.

[0019] In some embodiments of the method for preparing an indium tin zinc oxide target with high mobility, the binder is polyvinyl alcohol, and the addition amount is 0.5-1% of the weight of the powder.

[0020] In some embodiments of the method for preparing an indium tin zinc oxide target material with high mobility, the inlet air temperature of the spray granulation is 200-300° C., the exhaust air temperature is 80-100° C., and the frequency is 30-50 Hz.

[0021] In the method for preparing an indium tin zinc oxide target material with high mobility disclosed in some embodiments, the insulation time of the first insulation stage is set to 5 minutes.

[0022] In some embodiments of the method for preparing an indium tin zinc oxide target material with high mobility, the insulation time of the second insulation stage is set to 120 minutes.

[0023] Some embodiments disclose a method for preparing an indium tin zinc oxide target with high mobility, wherein the ball milling conditions include: the diameters of the zirconium oxide balls are 3, 5, and 10 mm, respectively, the number ratio is 1:1:1, the ball milling speed is 200-350 rpm, and the ball milling time is 24-48 hours.

[0024] Some embodiments disclose a method for preparing an indium tin zinc oxide target with high mobility, wherein In2O3 powder, ZnO powder, SnO2 powder, doped metal oxide powder, a dispersant and deionized water are mixed to prepare a slurry, the dispersant is ammonium polyacrylate, and the ratio of the dispersant to the total mass of the powder is 0.5 to 1:100.

[0025] On the other hand, some embodiments disclose an indium tin zinc oxide target with high mobility, which is obtained by the preparation method of the indium tin zinc oxide target with high mobility disclosed in the embodiments of the present invention. The indium tin zinc oxide target is doped with one of the low electronegativity metal elements Pr, Al, La, Hf, Zr, Nb, V, W, and Mo. The relative density of the indium tin zinc oxide target is not less than 99.5%, the grain size is between 2 and 5 μm, and the resistivity is between 3 and 10 mΩ·cm.

[0026] The method for preparing an indium tin zinc oxide target material with high mobility disclosed in an embodiment of the present invention comprises the following steps: adding doped metal oxides to In2O3 powder, ZnO powder and SnO2 powder, subjecting the doped metal oxides to a ball milling granulation process, and then subjecting the doped metal oxides to a two-step oscillation pressure sintering process to obtain an indium tin zinc oxide target material with high mobility, wherein the indium tin zinc oxide target material is doped with one of the low electronegativity metal elements Pr, Al, La, Hf, Zr, Nb, V, W and Mo; the indium tin zinc oxide target material has a relative density of not less than 99.5%, a grain size of 2 to 5 μm, and a resistivity of 3 to 10 mΩ·cm, and has good application prospects in display and other optoelectronic application fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the SEM image of the Pr-ITZO sputtering target prepared in Example 2. DETAILED DESCRIPTION

[0028] The word "embodiment" used herein as an "exemplary" does not necessarily mean that any embodiment described is superior or better than other embodiments. Performance index tests in the embodiments of the present invention are performed using conventional test methods in the art unless otherwise specified. It should be understood that the terms described in the embodiments of the present invention are only used to describe specific implementation methods and are not intended to limit the contents disclosed in the embodiments of the present invention.

[0029] Unless otherwise specified, the technical and scientific terms used herein have the same meanings as commonly understood by ordinary technicians in the technical field to which the embodiments of the present invention belong; other experimental methods and technical means not specifically specified in the embodiments of the present invention refer to experimental methods and technical means commonly used by ordinary technicians in the field.

[0030] The terms "substantially" and "approximately" used herein are used to describe small fluctuations. For example, they can refer to less than or equal to ±5%, such as less than or equal to ±2%, such as less than or equal to ±1%, such as less than or equal to ±0.5%, such as less than or equal to ±0.2%, such as less than or equal to ±0.1%, such as less than or equal to ±0.05%. The numerical data represented or presented in the range format herein are used only for convenience and brevity, and should therefore be flexibly interpreted as including not only the values ​​clearly listed as the limits of the range, but also all independent values ​​or sub-ranges contained in the range. For example, the numerical range of "1-5%" should be interpreted as including not only the clearly listed values ​​of 1% to 5%, but also the independent values ​​and sub-ranges within the range shown. Therefore, independent values ​​such as 2%, 3.5% and 4% and sub-ranges such as 1%-3%, 2%-4% and 3%-5% are included in this numerical range. This principle also applies to the range of only one numerical value. In addition, such an interpretation applies regardless of the width of the range or the characteristics described.

[0031] In this document, including in the claims, transitional words such as "comprises," "includes," "with," "having," "containing," "involving," "accommodating," etc. are understood to be open-ended, i.e., meaning "including but not limited to." Only the transitional words "consisting of" and "composed of" are closed transitional words.

[0032] In order to better illustrate the present invention, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the gist of the present invention.

[0033] Under the premise of no conflict, the technical features disclosed in the embodiments of the present invention may be arbitrarily combined, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present invention.

[0034] In some embodiments, a method for preparing an indium tin zinc oxide target having high mobility comprises the steps of:

[0035] S1, In2O3 powder, ZnO powder, SnO2 powder and doped metal oxide powder are prepared into slurry; doped metal oxide is an oxide of a low electronegative metal element with different valence states; usually, In2O3 powder, ZnO powder, SnO2 powder, doped metal oxide powder are mixed with a dispersant and water, stirred evenly, and prepared into slurry; usually, the relative proportion of each powder needs to be controlled, for example, the mass ratio of In2O3 powder, ZnO powder and SnO2 powder can be 20-23:20-27:5 0 to 60, further, the mass of the doped metal oxide powder can be determined based on the total mass of the three raw material powders, and the ratio of the mass of the doped metal oxide powder to the total mass of the powder can be controlled to be 0.05 to 5:100; generally, the mass of the dispersant needs to be controlled within a certain range, for example, the ratio of the dispersant to the total mass of the three powders can be controlled to be 0.5 to 1:100; in some embodiments, the dispersant is ammonium polyacrylate; further, the total mass of the powder in the slurry needs to be controlled, for example, the total mass content of the powder in the slurry is controlled to be 50 to 70%;

[0036] Generally, the doped metal oxide powder is an oxide of a low electronegative metal element with different valence states, for example, Pr6O 11 One of powder, Al2O3 powder, La2O3 powder, HfO2 powder, ZrO2 powder, Nb2O5 powder, V2O5 powder, WO3 powder or MoO3 powder; by doping with metal oxide powder, the grain size in the indium tin zinc oxide target material can be reduced and the distribution can be more uniform, the resistivity of the target material can be reduced, and the mobility of the target material can be improved;

[0037] S2. The slurry is ball-milled. In some embodiments, the ball-milling conditions include: the diameters of the zirconia balls are 3, 5, and 10 mm, respectively, the number ratio is 1:1:1, the ball-milling speed is 200-350 rpm, and the ball-milling time is 24-48 h;

[0038] S3, the slurry after ball milling is mixed with a binder, and spray granulation is performed to obtain spherical granulated powder; in some embodiments, the inlet air temperature of the spray granulation is 200-300°C, the exhaust air temperature is 80-100°C, and the frequency is 30-50Hz

[0039] S4, the spherical granulated powder is subjected to two-step oscillation pressure sintering treatment to obtain an indium tin zinc oxide target with high mobility;

[0040] Among them, the two-step oscillation pressure sintering process includes:

[0041] The spherical granulated powder is pre-pressed in a mold under a first pressure; the first pressure is 5-8Mpa;

[0042] The pre-pressed spherical granulated powder is heated to a first temperature at a heating rate of 5°C / min; before the temperature reaches the first temperature, the first pressure applied to the mold is linearly increased to a second pressure, the pressure is increased by 2 to 5 MPa at a time, and the increasing rate does not exceed 0.1 MPa / min; the first temperature is 1450 to 1500°C, and the second pressure is 30 to 40 MPa;

[0043] Performing a first insulation stage at a first temperature and a second pressure; superimposing an oscillating pressure with a frequency of 1 to 2 Hz and an amplitude of 5 to 10 MPa during the first insulation stage; in some embodiments, the insulation time of the first insulation stage is set to 5 minutes;

[0044] Maintaining a second pressure of 30-40 MPa, cooling the temperature to a second temperature at a cooling rate of 5°C / min; the second temperature is 1400-1450°C;

[0045] Performing a second insulation stage at a second temperature and a second pressure; wherein the second insulation stage applies an oscillating pressure of the same magnitude and frequency as that of the first insulation stage, and the insulation time of the second insulation stage is set to 120 minutes;

[0046] After the second insulation stage, the heating was stopped, the external oscillation pressure was removed, the cooling rate was set to 8°C / min, and the second pressure was maintained until the furnace temperature dropped to 1000°C; then the furnace was cooled to room temperature to obtain an indium tin zinc oxide target with high mobility.

[0047] In some embodiments, the relative density of the obtained indium tin zinc oxide target material is not less than 99.5%, the grain size is between 2 and 5 μm, and the resistivity is between 3 and 10 mΩ·cm.

[0048] The method for preparing an indium tin zinc oxide target with high mobility disclosed in an embodiment of the present invention comprises the following steps: adding doped metal oxides to In2O3 powder, ZnO powder and SnO2 powder, wherein the doped metal oxide powders can reduce the grain size in the target material and make the distribution more uniform; after a ball milling granulation process, the target material is subjected to a two-step oscillation pressure sintering process to further reduce the grain size in the target material, thereby obtaining an indium tin zinc oxide target material with high mobility; the indium tin zinc oxide target material has a relative density of not less than 99.5%, a grain size between 2 and 5 μm, and a resistivity between 3 and 10 mΩ·cm, and has good application prospects in display and other optoelectronic application fields.

[0049] The technical details are further illustrated below in conjunction with embodiments.

[0050] Example 1

[0051] The method for preparing an indium tin zinc oxide target material with high mobility disclosed in Example 1 comprises:

[0052] S1. Add 12g of ammonium polyacrylate to a zirconium oxide ball mill filled with 720g of deionized water and stir to obtain a dispersant solution. Mix 276g of In2O3 powder, 324g of ZnO powder and 600g of SnO2 powder and add them to the dispersant solution to form a slurry. In the slurry, the mass ratio of In2O3 powder, ZnO powder and SnO2 powder is 23:27:50. The solid content in the slurry is 62.5%.

[0053] S2. Ball milling the slurry: pour the slurry into a horizontal sand mill, select three different zirconia balls with diameters of 3, 5, and 10 mm, with a quantity ratio of 1:1:1, a ball milling speed of 350 rpm, and a ball milling time of 48 h;

[0054] S3, after the ball milling, 12g of polyvinyl alcohol binder was added to the slurry, and the ball milling was repeated for 30min to mix the binder evenly to obtain a mixed slurry; the obtained mixed slurry was spray dried using a spray granulator to generate a dry mixed spherical granulated powder with good fluidity, and the inlet air temperature during granulation was 250°C, the exhaust air temperature was 100°C, and the frequency was 45Hz;

[0055] S4, the spherical granulated powder is subjected to two-step oscillation pressure sintering treatment to obtain an indium tin zinc oxide target with high mobility;

[0056] Among them, the two-step oscillation pressure sintering process includes:

[0057] The spherical granulated powder is pre-pressed in a mold at a first pressure of 5 MPa;

[0058] The pre-pressed spherical granulated powder is heated to a first temperature of 1450°C at a heating rate of 5°C / min; before the temperature reaches the first temperature, the first pressure of 5 MPa applied to the mold is linearly increased to a second pressure of 30 MPa, with the pressure increasing by 2 MPa at a single increment and an increasing rate of 0.1 MPa / min;

[0059] Performing a first heat preservation stage at the first temperature and the second pressure; superimposing an oscillating pressure with a frequency of 1 Hz and an amplitude of 5 MPa during the first heat preservation stage, and maintaining the pressure for 5 minutes;

[0060] After the first heat preservation stage, the second pressure is maintained at 30 MPa, and the temperature is lowered to the second temperature of 1400°C at a cooling rate of 5°C / min;

[0061] A second insulation stage is performed at a second temperature and a second pressure, and the insulation time is 120 minutes; wherein, the second insulation stage applies an oscillating pressure of the same magnitude and frequency as the first insulation stage;

[0062] After the second insulation stage, the heating was stopped, the external oscillation pressure was removed, the cooling rate was set to 8°C / min, and the second pressure was maintained at 30 MPa until the furnace temperature dropped to 1000°C; then the furnace was cooled to room temperature.

[0063] The sintered sample was taken out, and the relative density of the final ITZO sputtering target sintered body was measured to be 99.70%, the average grain size was 2.76 μm, and the resistivity was 5.67 mΩ·cm.

[0064] Example 2

[0065] The method for preparing an indium tin zinc oxide target material with high mobility disclosed in Example 2 comprises:

[0066] S1, add 12g of ammonium polyacrylate to a zirconium oxide ball mill filled with 720g of deionized water and stir evenly to obtain a dispersant solution, add 270g of In2O3 powder, 3218g of ZnO powder, 588g of SnO2 powder, and 100g of Pr6O 11 24g of powder was mixed and added to the dispersant solution to form a slurry; in the slurry, the mass ratio of In2O3 powder, ZnO powder and SnO2 powder was 23:27:50; Pr6O 11 The mass of the powder accounts for 2% of the total mass of the powder; the solid content in the slurry is 62.5%;

[0067] S2. Ball milling the slurry: pour the slurry into a horizontal sand mill, select three different zirconia balls with diameters of 3, 5, and 10 mm, with a quantity ratio of 1:1:1, a ball milling speed of 350 rpm, and a ball milling time of 48 h;

[0068] S3, after the ball milling, 12g of polyvinyl alcohol binder was added to the slurry, and the ball milling was repeated for 30min to mix the binder evenly to obtain a mixed slurry; the obtained mixed slurry was spray dried using a spray granulator to generate a dry mixed spherical granulated powder with good fluidity, and the inlet air temperature during granulation was 250°C, the exhaust air temperature was 100°C, and the frequency was 45Hz;

[0069] S4, the spherical granulated powder is subjected to two-step oscillation pressure sintering treatment to obtain an indium tin zinc oxide target with high mobility;

[0070] Among them, the two-step oscillation pressure sintering process includes:

[0071] The spherical granulated powder is pre-pressed in a mold at a first pressure of 5 MPa;

[0072] The pre-pressed spherical granulated powder is heated to a first temperature of 1450°C at a heating rate of 5°C / min; before the temperature reaches the first temperature, the first pressure of 5 MPa applied to the mold is linearly increased to a second pressure of 30 MPa, with the pressure increasing by 2 MPa at a single increment and an increasing rate of 0.1 MPa / min;

[0073] Performing a first heat preservation stage at the first temperature and the second pressure; superimposing an oscillating pressure with a frequency of 1 Hz and an amplitude of 5 MPa during the first heat preservation stage, and maintaining the pressure for 5 minutes;

[0074] After the first heat preservation stage, the second pressure is maintained at 30 MPa, and the temperature is lowered to the second temperature of 1400°C at a cooling rate of 5°C / min;

[0075] A second insulation stage is performed at a second temperature and a second pressure, and the insulation time is 120 minutes; wherein, the second insulation stage applies an oscillating pressure of the same magnitude and frequency as the first insulation stage;

[0076] After the second insulation stage, the heating was stopped, the external oscillation pressure was removed, the cooling rate was set to 8°C / min, and the second pressure was maintained at 30 MPa until the furnace temperature dropped to 1000°C; then the furnace was cooled to room temperature.

[0077] The sintered sample was taken out, and the relative density of the final Pr-ITZO sputtering target sintered body was measured to be 99.50%, the average grain size was 2.54 μm, and the resistivity was 5.7 mΩ·cm.

[0078] Figure 1 From the SEM image of the Pr-ITZO sputtering target prepared in Example 2, it can be seen that the grain size is small and evenly distributed, there are fewer voids, and the density is high.

[0079] Example 3

[0080] The method for preparing an indium tin zinc oxide target with high mobility disclosed in Example 3 is carried out with reference to Example 2, wherein: the mass ratio of In2O3, ZnO and SnO2 is 23:27:50; Pr6O is doped 11 The mass of the powder accounts for 5% of the total mass of the powder;

[0081] The relative density of the Pr-ITZO sputtering target sintered body finally obtained was 99.45%, the average grain size was 2.45 μm, and the resistivity was 5.9 mΩ·cm.

[0082] Example 4

[0083] The method for preparing an indium tin zinc oxide target with high mobility disclosed in Example 4 is carried out with reference to the method disclosed in Example 2, wherein: the mass ratio of In2O3, ZnO and SnO2 is 23:27:50; the mass of Al2O3 accounts for 1% of the total mass of the powder.

[0084] The relative density of the Al-ITZO sputtering target sintered body finally obtained was 99.6%, the average grain size was 2.06 μm, and the resistivity was 4.90 mΩ·cm.

[0085] Example 5

[0086] The method for preparing the indium tin zinc oxide target with high mobility disclosed in Example 5 is carried out with reference to the method disclosed in Example 2, wherein: the mass ratio of In2O3, ZnO and SnO2 is 23:27:50; the mass of La2O3 accounts for 1% of the total mass of the powder.

[0087] The relative density of the La-ITZO sputtering target sintered body finally obtained was 99.60%, the average grain size was 2.43 μm, and the resistivity was 4.69 mΩ·cm.

[0088] Example 6

[0089] The method for preparing an indium tin zinc oxide target with high mobility disclosed in Example 6 is carried out with reference to the method disclosed in Example 2, wherein: the mass ratio of In2O3, ZnO and SnO2 is 23:27:50; the mass of HfO2 accounts for 1% of the total mass of the powder.

[0090] The relative density of the finally obtained Hf-ITZO sputtering target sintered body is 99.65%, the average grain size is 2.41 μm, and the resistivity is 2.40 mΩ·cm.

[0091] Example 7

[0092] The method for preparing an indium tin zinc oxide target with high mobility disclosed in Example 7 is carried out with reference to the method disclosed in Example 2, wherein: the mass ratio of In2O3, ZnO and SnO2 is 23:27:50; the mass of ZrO2 accounts for 1% of the total mass of the powder.

[0093] The relative density of the finally obtained Zr-ITZO sputtering target sintered body is 99.63%, the average grain size is 2.35 μm, and the resistivity is 3.35 mΩ·cm.

[0094] Example 8

[0095] The method for preparing an indium tin zinc oxide target with high mobility disclosed in Example 8 is carried out with reference to the method disclosed in Example 2, wherein the mass ratio of In2O3, ZnO and SnO2 is 23:27:50; and the mass of V2O5 accounts for 1% of the total mass of the powder.

[0096] The relative density of the V-ITZO sputtering target sintered body finally obtained was 99.59%, the average grain size was 2.33 μm, and the resistivity was 2.30 mΩ·cm.

[0097] Example 9

[0098] The method for preparing an indium tin zinc oxide target with high mobility disclosed in Example 9 is carried out with reference to the method disclosed in Example 2, wherein the mass ratio of In2O3, ZnO and SnO2 is 23:27:50; and the mass of Nb2O5 accounts for 1% of the total powder mass.

[0099] The relative density of the sintered Nb-ITZO sputtering target obtained was 99.61%, the average grain size was 2.30 μm, and the resistivity was 2.32 mΩ·cm.

[0100] Example 10

[0101] The method for preparing an indium tin zinc oxide target with high mobility disclosed in Example 10 is carried out with reference to the method disclosed in Example 2, wherein the mass ratio of In2O3, ZnO and SnO2 is 23:27:50; and the mass of WO3 accounts for 1% of the total mass of the powder.

[0102] The relative density of the W-ITZO sputtering target sintered body finally obtained was 99.63%, the average grain size was 2.32 μm, and the resistivity was 2.25 mΩ·cm.

[0103] Embodiment 11

[0104] The method for preparing an indium tin zinc oxide target with high mobility disclosed in Example 11 is carried out with reference to the method disclosed in Example 2, wherein: the mass ratio of In2O3, ZnO and SnO2 is 23:27:50; the mass of MoO3 accounts for 1% of the total mass of the powder.

[0105] The relative density of the Mo-ITZO sputtering target sintered body finally obtained was 99.57%, the average grain size was 2.30 μm, and the resistivity was 2.28 mΩ·cm.

[0106] From the results of Examples 1 to 11, it can be seen that after low electronegativity metal elements are doped in Examples 2 to 11, the average grain size of the target material is smaller than the average grain size in Example 1; and the resistivity of the target material in Examples 4 to 11 continues to decrease with the increase of the valence state of the doped metal element, indicating that metal element doping is indeed effective and is related to the valence state of the doped element.

[0107] The method for preparing an indium tin zinc oxide target material with high mobility disclosed in an embodiment of the present invention comprises the following steps: adding doped metal oxides to In2O3 powder, ZnO powder and SnO2 powder, subjecting the doped metal oxides to a ball milling granulation process, and then subjecting the doped metal oxides to a two-step oscillation pressure sintering process to obtain an indium tin zinc oxide target material with high mobility, wherein the indium tin zinc oxide target material is doped with one of the low electronegativity metal elements Pr, Al, La, Hf, Zr, Nb, V, W and Mo; the indium tin zinc oxide target material has a relative density of not less than 99.5%, a grain size of 2 to 5 μm, and a resistivity of 3 to 10 mΩ·cm, and has good application prospects in display and other optoelectronic application fields.

[0108] The technical solutions disclosed in the embodiments of the present invention and the technical details disclosed in the embodiments are merely illustrative of the inventive concept of the present invention and do not constitute a limitation on the technical solutions of the embodiments of the present invention. Any conventional changes, replacements or combinations of the technical details disclosed in the embodiments of the present invention have the same inventive concept as the present invention and are within the protection scope of the claims of the present invention.

Claims

1. A method for preparing an indium tin zinc oxide target material with high mobility, characterized in that: Includes steps: S1, In2O3 powder, ZnO powder, SnO2 powder and doped metal oxide powder are prepared into slurry; the doped metal oxide is an oxide of a low electronegativity metal element with different valence states; S2, ball milling the slurry; S3, the ball-milled slurry is mixed with a binder and spray-granulated to obtain spherical granulated powder; S4, the spherical granulated powder is subjected to two-step oscillation pressure sintering treatment to obtain an indium tin zinc oxide target with high mobility; Wherein, the two-step oscillating pressure sintering process comprises: The spherical granulated powder is pre-pressed in a mold under a first pressure; the first pressure is 5 to 8 MPa; The pre-pressed spherical granulated powder is heated to a first temperature at a heating rate of 5°C / min; before the temperature reaches the first temperature, the first pressure applied to the mold is linearly increased to a second pressure, the pressure is increased by 2 to 5 MPa at a time, and the increase rate does not exceed 0.1 MPa / min; the first temperature is 1450 to 1500°C, and the second pressure is 30 to 40 MPa; Performing a first heat preservation stage at a first temperature and a second pressure; superimposing an oscillating pressure with a frequency of 1 to 2 Hz and an amplitude of 5 to 10 MPa during the first heat preservation stage; Maintaining a second pressure of 30-40 MPa, cooling the temperature to a second temperature at a cooling rate of 5°C / min; the second temperature is 1400-1450°C; Performing a second insulation stage at a second temperature and a second pressure; wherein the second insulation stage applies an oscillating pressure of the same magnitude and frequency as the first insulation stage; After the second heat preservation stage, the heating was stopped, the external oscillation pressure was removed, the cooling rate was set to 8°C / min, and the second pressure was maintained until the furnace temperature dropped to 1000°C; then the furnace was cooled to room temperature.

2. The method for preparing an indium tin zinc oxide target with high mobility according to claim 1, characterized in that: The doped metal oxide powder is Pr6O 11 One of powder, Al2O3 powder, La2O3 powder, HfO2 powder, ZrO2 powder, Nb2O5 powder, V2O5 powder, WO3 powder or MoO3 powder.

3. The method for preparing an indium tin zinc oxide target with high mobility according to claim 1, characterized in that: The mass ratio of the In2O3 powder, ZnO powder and SnO2 powder is 20-23:20-27:50-60, the ratio of the doped metal oxide to the total mass of the powder is 0.05-5:100; the total mass content of the powder in the slurry is 50-70%.

4. The method for preparing an indium tin zinc oxide target with high mobility according to claim 1, characterized in that: The binder is polyvinyl alcohol, and the added amount is 0.5-1% of the weight of the powder.

5. The method for preparing an indium tin zinc oxide target with high mobility according to claim 1, characterized in that: The inlet air temperature of spray granulation is 200-300°C, the exhaust air temperature is 80-100°C, and the frequency is 30-50Hz.

6. The method for preparing an indium tin zinc oxide target with high mobility according to claim 1, characterized in that: The holding time of the first holding stage was set to 5 min.

7. The method for preparing an indium tin zinc oxide target with high mobility according to claim 1, characterized in that: The holding time of the second holding stage was set to 120 min.

8. The method for preparing an indium tin zinc oxide target with high mobility according to claim 1, characterized in that: The ball milling conditions include: the diameters of the zirconia balls are 3, 5, and 10 mm, respectively, the number ratio is 1:1:1, the ball milling speed is 200-350 rpm, and the ball milling time is 24-48 h.

9. The method for preparing an indium tin zinc oxide target with high mobility according to claim 1, characterized in that: In2O3 powder, ZnO powder, SnO2 powder, doped metal oxide powder, dispersant and deionized water are mixed to prepare slurry, wherein the dispersant is ammonium polyacrylate, and the ratio of the dispersant to the total mass of the powder is 0.5 to 1:

100.

10. An indium tin zinc oxide target with high mobility, characterized in that: Obtained by the preparation method according to any one of claims 1 to 9, the indium tin zinc oxide target is doped with one of the low electronegativity metal elements Pr, Al, La, Hf, Zr, Nb, V, W, and Mo; the relative density of the indium tin zinc oxide target is not less than 99.5%, the grain size is between 2 and 5 μm, and the resistivity is between 3 and 10 mΩ·cm.

Citation Information

Patent Citations

  • Indium tin oxide target material and sintering preparation method thereof

    CN103922703A

  • Additive-free high-mobility oxide target material and preparation method thereof

    CN115304359A

  • Praseodymium-doped indium zinc oxide sputtering target material and preparation method thereof

    CN115925410A

  • Indium zinc oxide doped rare earth metal target material and preparation method thereof

    CN116199496A

  • Indium tin zinc oxide target material and preparation method thereof

    CN116253556A

Cited By

  • Low-indium ceramic target material as well as preparation method and application thereof