Corrosion inhibitor for CO2 oil displacement produced liquid and preparation method thereof
Through a new corrosion inhibitor preparation method, the corrosion inhibitor E+1 was prepared by using the combined reaction of oleic acid, catalyst, water-carrying agent and quaternization reagent, which solved the corrosion problem in CO2 oil displacement technology and achieved Efficient corrosion inhibition effect, corrosion inhibition rate reaches 90%, significantly reducing corrosion hazards in CO2 oil flooding applications.
Patent Information
- Application Number
- CN202410692519.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-31
- Publication Date
- 2024-10-15
AI Technical Summary
In CO2 oil flooding technology, the miscibility of CO2 and formation water leads to corrosion of pipelines and mechanical equipment. The corrosion inhibition effect of existing corrosion inhibitors is poor, especially in corrosive environments with high CO2 content.
Using a new corrosion inhibitor preparation method, the corrosion inhibitor E+1 was prepared through the combined reaction of oleic acid, catalyst, water-carrying agent, diethylene triamine and quaternary ammonium reagent, and after multi-stage electric heating and ultrasonic treatment. , used in CO2 flooding produced fluids to significantly reduce corrosion hazards.
The corrosion inhibitor E+1 shows excellent corrosion inhibition effect in CO2 flooding applications, with a corrosion inhibition rate of 90%, reducing the corrosion rate to 0.01771mm/a, which is far lower than the industry standard and significantly reducing the cost of CO2 flooding. Corrosion Hazards in Oil Applications.
Smart Images

Figure BDA0004868732670000051 
Figure BDA0004868732670000052 
Figure BDA0004868732670000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of corrosion inhibitor processing, and in particular relates to a corrosion inhibitor for CO2 oil recovery production fluid and a preparation method thereof. Background Art
[0002] CO2 flooding technology refers to the general term for reservoir engineering design, CO2 injection and production technology, dynamic monitoring and adjustment, and output fluid processing technologies in oil field exploitation. It is the most promising method to improve the recovery rate of low permeability reservoirs. This technology can not only reduce the emission of industrial waste gas carbon dioxide that has a severe impact on the earth's environment, but also turn carbon dioxide into an important resource to improve oil field development effects and increase crude oil recovery. China's high-water-content oil fields in the development stage account for more than 70% of the country's total production. These high-water-content reservoirs are one of the best geological sites for CO2 storage and flooding. However, the miscibility of CO2 and formation water can cause corrosion of pipelines and mechanical equipment. CO2 dissolves in water to form carbonic acid, which has a strong corrosive effect on metals, especially in the presence of corrosive media such as H2O, HCl, organic acids, and H2S.
[0003] Current anti-corrosion measures include selecting corrosion-resistant alloy materials, applying cathodic protection, treating the surface of pipeline steel, and adding corrosion inhibitors. Among these anti-corrosion measures, adding chemical corrosion inhibitors is an economical, effective and versatile method to control corrosion scaling, which will be particularly suitable for use in oil and gas wells and gathering and transportation systems. Corrosion inhibitors usually contain heteroatoms such as N, O, S or heterocycles such as imidazole and quinoline, and have excellent corrosion inhibition effects. Imidazolinyl corrosion inhibitors are the most commercially used CO2 corrosion inhibitors. They have good thermal stability and low toxicity, and are suitable for corrosive environments with high CO2 content, but the corrosion inhibition effect is poor. Summary of the invention
[0004] The purpose of the present invention is to provide a corrosion inhibitor for CO2 oil recovery produced fluid and a preparation method thereof. The preparation method is simple and easy and can reduce costs. The prepared corrosion inhibitor E+1 is applied to the corrosion inhibition of CO2 oil recovery produced fluid, which can show an excellent corrosion inhibition effect and can greatly reduce the corrosion hazards in CO2 oil recovery applications.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:
[0006] A method for preparing a corrosion inhibitor for CO2 oil flooding produced fluid comprises the following steps:
[0007] (1) Weighing a certain amount of oleic acid and catalyst and adding them into a reaction container;
[0008] (2) Using a programmable electric heating jacket for heating, set the first program, program heating for 1-2 hours, the starting temperature is set to 90°C, and the ending temperature is set to 150°C; set the second program, program heating for 3-4 hours, the starting temperature is set to 150°C, and the ending temperature is set to 170°C; set the third program, program heating for 1-1.5 hours, the starting temperature is set to 170°C, and the ending temperature is set to 220°C; set the fourth program, program heating for 3-4 hours, the starting temperature is set to 220°C, and the ending temperature is set to 220°C;
[0009] (3) When the electric heating jacket is heated to 80-100°C, a water-carrying agent is added dropwise to the reaction vessel;
[0010] (4) When the temperature of the electric heating mantle rises to 110-130°C, diethylenetriamine is added dropwise. After the addition is completed, the water in the reaction system is separated, and then the reaction is carried out at 200-230°C for 3-4 hours;
[0011] (5) When the temperature drops to 60-70° C., a quaternary ammonium reagent is added and reacted at this temperature for 3-4 hours to obtain corrosion inhibitor E1;
[0012] (6) Weigh a certain amount of oleic acid and potassium dihydrogen phosphate and add them to corrosion inhibitor E1, and stir for 3-5 minutes under ultrasonication to obtain corrosion inhibitor E+1.
[0013] Preferably, in step (1), the catalyst is boric acid or phosphoric acid, and the amount of the catalyst used is 0.2-0.4 wt % of oleic acid.
[0014] Preferably, in step (3), the water-carrying agent is xylene or toluene, and the amount of the water-carrying agent added is 10%-20% of the total mass of oleic acid, catalyst and water-carrying agent.
[0015] Preferably, in step (4), the molar ratio between diethylenetriamine and oleic acid is (1.1-1.2):1.
[0016] Preferably, in step (5), the quaternizing agent is one of dioctyl carbonate, benzyl chloride, dimethyl sulfate, and diethyl sulfate, and the molar ratio between the quaternizing agent and oleic acid is (0.9-1):1.
[0017] Preferably, in step (6), the mass ratio of corrosion inhibitor E1, oleic acid and potassium dihydrogen phosphate is 4:0.35:0.9.
[0018] The present invention also provides a corrosion inhibitor for CO2 oil recovery produced fluid prepared by the above preparation method.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The preparation process of the present invention is simple and easy to implement, and the cost is low;
[0021] (2) The corrosion inhibitor E+1 prepared by the present invention has excellent corrosion inhibition effect. When applied to the corrosion inhibition of CO2 oil recovery produced fluid, it shows an excellent corrosion inhibition effect with a corrosion inhibition rate of 90%. After adding the corrosion inhibitor, the corrosion rate is 0.01771 mm / a, which is much lower than the industry standard of 0.076 mm / a, greatly reducing the corrosion hazard in CO2 oil recovery applications, and has broad economic and social benefits;
[0022] (3) The synthesis process of the present invention is green and low-toxic, the water-carrying agent is recycled, the quaternary ammonium agent used is low-toxic, low-harmful and odorless, and the obtained corrosion inhibitor E+1 has no special odor. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A diagram of a synthetic device for preparing a corrosion inhibitor according to the present invention;
[0024] Figure 2 This is a diagram of the experimental device for simulating actual CO2 flooding and oil transportation in the present invention;
[0025] Figure 3 This is a diagram of the electrochemical test device of the Chenhua CHI 660E electrochemical workstation of the present invention;
[0026] Figure 4 It is a graph of corrosion rate and corrosion inhibition rate in a weight loss method experiment involved in an embodiment of the present invention;
[0027] Figure 5 is a Tafel polarization curve diagram involved in an embodiment of the present invention;
[0028] Figure 6 It is the Nyquist diagram of the EIS test involved in the embodiment of the present invention;
[0029] Figure 7 It is an equivalent circuit diagram for Zsimpwin fitting involved in the embodiments of the present invention. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with specific embodiments.
[0031] Example
[0032] like Figure 1 As shown, a method for preparing a corrosion inhibitor for CO2 oil flooding produced fluid comprises the following steps:
[0033] (1) Weigh 28 g of oleic acid and 0.06 g of boric acid and add them into a 250 ml three-necked flask;
[0034] (2) Edit the programmable electric heating jacket, set the first program, program heating for 1-2 hours, set the starting temperature to 90°C, and the ending temperature to 150°C; set the second program, program heating for 3-4 hours, set the starting temperature to 150°C, and the ending temperature to 170°C; set the third program, program heating for 1-1.5 hours, set the starting temperature to 170°C, and the ending temperature to 220°C; set the fourth program, program heating for 3-4 hours, set the starting temperature to 220°C, and the ending temperature to 220°C;
[0035] (3) When the reaction temperature reaches 90°C, add 20 ml of xylene into the three-necked flask using a constant pressure dropping funnel;
[0036] (4) When the temperature reaches 120°C, add 13 ml of diethylenetriamine using a constant pressure dropping funnel. After the constant pressure dropping funnel is finished, replace it with a water separator and use the water separator to continuously separate the water in the reaction system. Then react at 220°C for 3 hours.
[0037] (5) When the temperature drops to 60° C., add 30 ml of dioctyl carbonate and react at this temperature for 3 h to obtain corrosion inhibitor E1;
[0038] (6) 4 g of the obtained corrosion inhibitor E1 was taken out, 0.35 g of oleic acid and 0.9 g of potassium dihydrogen phosphate were weighed, added to the corrosion inhibitor E1, ultrasonicated and stirred for 3 min to obtain corrosion inhibitor E+1.
[0039] like Figure 2 As shown, the corrosion inhibitor E1 and the corrosion inhibitor E+1 obtained in the above steps were added to the experimental device simulating the actual CO2 oil recovery transportation to carry out the dynamic hanging plate weight loss method experiment (the full immersion hanging plate weight loss method experiment was carried out in the 0.54Mpa CO2 gas environment and 80% water content crude oil produced liquid at 35°C; the hanging plate was type III 40*13*2mm carbon steel of HG5-1526-1983 standard, with a surface area of 12cm 2 ), and at the same time, a commonly used commercial corrosion inhibitor - quaternary ammonium salt 27 (oleic acid imidazoline sulfate methyl ester amide) (99%) (hereinafter referred to as S1) was subjected to the same weight loss method experiment to compare the corrosion inhibition performance.
[0040] Furthermore, the corrosion solution after the weight loss experiment was subjected to polarization curve test and EIS test using Chenhua CHI 660E series electrochemical workstation, standard three-electrode electrolytic cell, platinum wire electrode (Shanghai Chenhua, model CHI115) as auxiliary electrode, Ag / Agcl electrode (Shanghai Chenhua, model CHI111) as reference electrode, and carbon steel electrode (Shanghai Leton, model 3mm) as working electrode, as shown in Fig. Figure 3 shown.
[0041] Blank experiment: Do the same weight loss experiment using the above apparatus without adding any reagents.
[0042] Specific implementation:
[0043] The weight loss method calculates the corrosion rate based on the mass change of the test piece before and after the corrosion process within a certain period of time, and judges the corrosion inhibition effect of the corrosion inhibitor on the metal in the environmental medium by the speed of the corrosion. If the metal and the corrosion products are dissolved in the corrosive medium, the weight of the test piece decreases after corrosion, and the weight loss method is generally used for measurement. When the composition of the corrosion product is clear and can be firmly attached to the metal surface, the weight of the sample increases after corrosion, and the weight gain method is used for weight measurement. Because the weight method has many advantages such as simple operation, intuitive results, and high reliability of experimental results, it is currently considered to be the most basic method for evaluating the performance of corrosion inhibitors.
[0044] Electrochemical methods are used to study the mechanism of corrosion inhibition. They are based on the fact that metal corrosion is an electrochemical reaction with electrochemical properties, so the metal corrosion rate can be measured indirectly. The electrochemical methods commonly used are mainly the Tafel extrapolation method of the potentiodynamic polarization curve and the electrochemical AC impedance method.
[0045] 1. Tafel extrapolation of potentiodynamic polarization curve
[0046] In the potentiodynamic polarization curve, you can find information such as self-corrosion potential and self-corrosion current. The change of self-corrosion current can provide the measurer with clear hints about the change of corrosion rate. According to the general rule, the smaller the self-corrosion current, the smaller the corrosion rate of the metal, and the better the effect of the corrosion inhibitor. At the same time, it is also necessary to study the change of self-corrosion potential to determine the mechanism of action of the corrosion inhibitor.
[0047] 2. AC impedance method
[0048] Electrochemical impedance spectroscopy (EIS) refers to changing the AC signal into a small sine wave, and using the change of this wave to affect the electrode, and observing the corresponding response of the system after stabilization, so as to measure the impedance value of the corrosion system. Using different methods to measure impedance will get different curves, such as the Nyquist diagram. Then, the equivalent circuit is designed using Zsimpwin 3.10 software to analyze the Nyquist diagram, so as to know the corresponding equivalent circuit, and use the equivalent circuit as the basic model to infer the corrosion inhibition effect.
[0049] Weightlessness method experimental steps:
[0050] (1) Type III of HG5-1526-1983 standard 40*13*2mm, surface area 12cm 2 Use carbon steel (purchase professional corrosion coupons without degreasing or other special treatments) as the experimental coupons, soak and wash them three times in anhydrous ethanol, remove water, wipe them dry with absorbent cotton, blow them dry with cold air, weigh them, record them and keep them for later use.
[0051] (2) Weigh 20 g of crude oil and 80 g of oil recovery fluid, heat and dissolve them to prepare a corrosion solution. Four groups are prepared. The first group does not add any reagents, the second group adds 0.1 g of quaternary ammonium salt-27 (99%) (hereinafter referred to as S1), the third group adds 0.1 g of E1, and the fourth group adds 0.1 g of E+1.
[0052] (3) The corrosion solution was added to a Shanghai Yanzheng Micro-Reactor (YZPR-100(M)), the temperature was set to 35°C, the speed was set to 200RPM, the reaction time was set to 168h, 0.54Mpa CO2 was introduced, and CO2 was replenished every 24h to keep the pressure in the reactor at 0.54Mpa.
[0053] (4) Take 100 ml of 15% hydrochloric acid, add 5 g of hexamethylenetetramine, and add water to 1000 ml to prepare an acid washing solution.
[0054] (5) After the reaction is completed, remove the coupons, use heavy oil cleaning agent (professional cleaning agent purchased online: surfactant) to wash away the crude oil on the surface, use pickling solution to wash away the corrosion products, rinse the sample with clean water, soak and wash it three times in acetone and anhydrous ethanol, wipe it dry with absorbent cotton, blow it dry with cold air, weigh it, record it and keep it for later use.
[0055] The data processing method is as follows:
[0056]
[0057] In formula (1): V is the corrosion rate, mm / a;
[0058] m0——mass of the coupon before corrosion, g;
[0059] m——the mass of the coupon after corrosion, g;
[0060] s——total surface area of the coupon, cm 2 ;
[0061] t——corrosion time of coupon, h;
[0062] ρ——Test piece density, carbon steel is generally taken as 7.85g / cm 3 ;
[0063]
[0064] In formula (2): η——corrosion inhibition rate, %
[0065] V0——average corrosion rate of blank corrosion solution, mm / a;
[0066] V i ——Average corrosion rate in the corrosion solution after adding corrosion inhibitor, mm / a;
[0067] The results of the weight loss method experiment are as follows Figure 4 shown.
[0068] Depend on Figure 4 It can be seen that the corrosion inhibition effect is E+1>E1≥S1, the corrosion inhibition rate of E+1 corrosion inhibitor is as high as 90%, and the corrosion rate after adding the corrosion inhibitor is lower than the industry standard of 0.076mm / a.
[0069] Electrochemical testing:
[0070] The corrosion liquid after the weight loss experiment was subjected to polarization curve test and EIS test using Chenhua CHI660E series electrochemical workstation, standard three-electrode electrolytic cell, platinum wire electrode (Shanghai Chenhua, model CHI115) as auxiliary electrode, Ag / Agcl electrode (Shanghai Chenhua, model CHI111) as reference electrode, and carbon steel electrode (Shanghai Leton, model 3mm) as working electrode. The potential range of the dynamic potential polarization curve measurement was set to -700mV-+100mV relative to the self-corrosion potential, the potential scanning speed of the polarization curve test was 0.5mV / s, the EIS measurement was carried out under OCP, the experimental test frequency range was 1000KHz-10mHz, and the excitation signal was an AC signal with an amplitude of ±10mV. The corrosion rate V was obtained by extrapolation in the polarization curve test, and the corrosion inhibition rate was obtained by formula (2). The EIS test used Zsimpwin3.10 software to fit the electrochemical measurement system to a corresponding equivalent circuit that is simple and easy to analyze. The corrosion inhibition rate was obtained by the following formula (3):
[0071]
[0072] In formula (3): η——corrosion inhibition rate, %;
[0073] R ct ——Electrochemical impedance value in the corrosion solution after adding corrosion inhibitor, Ω·cm 2 ;
[0074] R ct0 ——Electrochemical impedance value of the system when blank sample is used, Ω·cm 2 ;
[0075] The equivalent circuit diagram is as follows Figure 7 As shown, Figure 7 middle:
[0076] RL – ohmic resistance of the solution;
[0077] W1——Permeation and diffusion impedance of crude oil molecules;
[0078] CPE – Constant Phase Element;
[0079] CPE1——Capacitance of the particle adsorption film of corrosion inhibitor / corrosion product;
[0080] Rf——Resistance of the particle adsorption film of corrosion inhibitor / corrosion product;
[0081] CPE2 - double layer capacitance;
[0082] Rct – Ohmic resistance for charge transfer.
[0083] Polarization curve test data table:
[0084]
[0085] The Tafel polarization curve obtained by the test is as follows Figure 5 shown.
[0086] From the above data, it can be seen that after adding S1, E1, E+1 corrosion inhibitors, E corr Increasing the corrosion potential moves in the positive direction. All corrosion inhibitors are cationic corrosion inhibitors, and the corrosion inhibition effect is E+1>E1>S1.
[0087] EIS test data table:
[0088]
[0089]
[0090] The Nyquist plot obtained by EIS test is shown in Figure 6 shown.
[0091] From the above data, it can be seen that after adding S1, E1, and E+1 corrosion inhibitors, R ct Compared with the blank group, the R ct , E+1>E1>S1, corrosion inhibition effect E+1>E1>S1.
[0092] In summary, the corrosion inhibitor E+1 prepared by the present invention has excellent corrosion inhibition effect. It is applied to the corrosion inhibition of CO2 oil recovery produced fluid, showing an excellent corrosion inhibition effect with a corrosion inhibition rate of 90%. The corrosion rate after adding the corrosion inhibitor is 0.01771 mm / a, which is much lower than the industry standard of 0.076 mm / a. It greatly reduces the corrosion hazard in CO2 oil recovery applications and has broad economic and social benefits.
Claims
1. A method for preparing a corrosion inhibitor for CO2 oil flooding produced fluid, characterized in that: The following steps are involved: (1) Weighing a certain amount of oleic acid and catalyst and adding them into a reaction container; (2) Using a programmable electric heating jacket for heating, set the first program, program heating for 1-2 hours, the starting temperature is set to 90°C, and the ending temperature is set to 150°C; set the second program, program heating for 3-4 hours, the starting temperature is set to 150°C, and the ending temperature is set to 170°C; set the third program, program heating for 1-1.5 hours, the starting temperature is set to 170°C, and the ending temperature is set to 220°C; set the fourth program, program heating for 3-4 hours, the starting temperature is set to 220°C, and the ending temperature is set to 220°C; (3) When the electric heating jacket is heated to 80-100°C, a water-carrying agent is added dropwise to the reaction vessel; (4) When the temperature of the electric heating mantle rises to 110-130°C, diethylenetriamine is added dropwise. After the addition is completed, the water in the reaction system is separated, and then the reaction is carried out at 200-230°C for 3-4 hours; (5) When the temperature drops to 60-70° C., a quaternary ammonium reagent is added and reacted at this temperature for 3-4 hours to obtain corrosion inhibitor E1; (6) Weigh a certain amount of oleic acid and potassium dihydrogen phosphate and add them to corrosion inhibitor E1, and stir for 3-5 minutes under ultrasonication to obtain corrosion inhibitor E+1.
2. The method for preparing a corrosion inhibitor for CO2 flooding produced fluid according to claim 1, characterized in that: In step (1), the catalyst is boric acid or phosphoric acid, and the amount of the catalyst used is 0.2-0.4wt% of oleic acid.
3. The method for preparing a corrosion inhibitor for CO2 flooding produced fluid according to claim 1 or 2, characterized in that: In step (3), the water-carrying agent is xylene or toluene, and the amount of the water-carrying agent added is 10%-20% of the total mass of oleic acid, catalyst and the water-carrying agent.
4. The method for preparing a corrosion inhibitor for CO2 flooding produced fluid according to claim 1 or 2, characterized in that: In step (4), the molar ratio of diethylenetriamine to oleic acid is (1.1-1.2):
1.
5. The method for preparing a corrosion inhibitor for CO2 flooding produced fluid according to claim 1 or 2, characterized in that: In step (5), the quaternary ammonium agent is one of dioctyl carbonate, benzyl chloride, dimethyl sulfate, and diethyl sulfate, and the molar ratio between the quaternary ammonium agent and oleic acid is (0.9-1):
1.
6. The method for preparing a corrosion inhibitor for CO2 flooding produced fluid according to claim 1 or 2, characterized in that: In step (6), the mass ratio of corrosion inhibitor E1, oleic acid and potassium dihydrogen phosphate is 4:0.35:0.
9.
7. A corrosion inhibitor for CO2 oil recovery produced fluid prepared by the preparation method according to any one of claims 1 to 6.
Citation Information
Cited By
Compound corrosion inhibitor for CO2 oil displacement produced liquid and preparation method of compound corrosion inhibitor