Polyester resin for high-hardness and high-temperature-resistant powder coating as well as preparation method and application of polyester resin

By using triglycidyl trimesolate curing system and high-temperature extraction reaction in powder coatings, a high-hardness, high-temperature-resistant polyester resin is prepared, which solves the problems of insufficient curing agent performance and difficulty in utilizing furfural residue in the existing technology. , realizing the economic significance of high-performance coating and environmental protection.

CN118772384APending Publication Date: 2024-10-15ANHUI YONGLI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410984117.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

In existing outdoor weather-resistant powder coatings, the HAA curing agent has pinhole defects in the coating film curing, the TGIC curing agent is limited due to its sensitization, and the polyester resin has insufficient compatibility, making it difficult to achieve high hardness and high-temperature yellowing resistance, and Furfural residue is difficult to comprehensively utilize on a large scale, leading to environmental pollution.

Method used

Triglycidyl trimesolate curing system is used to prepare high-quality polymers through the polymerization of p-cresol, phenol, furfural residue, formaldehyde, dimethyl adipate, 1,3-dihydroxybutane, ethylmalonic acid and other raw materials. Hard, high-temperature-resistant polyester resin, and through high-temperature extraction and hydroxymethylation reaction, combined with transesterification graft chain extension reaction, form a high-functionality polyester resin, combined with triglycidyl trimesolate curing agent, to achieve high Performance coating.

Benefits of technology

The polyester resin has achieved high hardness and high-temperature yellowing resistance, which reduces the cost, improves the comprehensive utilization rate of furfural slag, enhances the functionality of the polyester resin, the fluidity and curing performance of the coating film, and meets the needs of decorative powder coatings. installation requirements and reduce environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004956908120000011
    Figure FDA0004956908120000011
  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides polyester resin for a high-hardness and high-temperature-resistant powder coating as well as a preparation method and application of the polyester resin, and belongs to the technical field of powder coatings. The catalyst is prepared from p-cresol, phenol, furfural residues, formaldehyde, dimethyl adipate, 1, 3-dihydroxybutane, ethyl malonic acid, 1, 1-cyclohexyl diacetic acid and other raw materials through polymerization. Phenol, p-cresol and phenolic lignin are adopted to prepare a polyhydroxymethylated mixed product to participate in a polymerization reaction together, a final product chain segment contains a high-content hindered phenol antioxidant group, the high-temperature yellowing resistance is good, high-functionality lignin in furfural residues is extracted at high temperature to participate in the polymerization reaction, and the high-temperature yellowing resistance is good. According to the present invention, the furfural residue is comprehensively utilized, the functionality of the polymer is high, the coating film obtained after low temperature curing with the triglycidyl trimesic acid curing agent has characteristics of high hardness and excellent high temperature yellowing resistance, and the conventional performances such as impact and gloss meet the application requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder coatings, and specifically relates to a polyester resin for high-hardness and high-temperature-resistant powder coatings, and a preparation method and application thereof. Background Art

[0002] Powder coating is a solid powdered synthetic resin coating composed of solid resin, pigment, filler and additives. Unlike ordinary solvent-based coatings and water-based coatings, its dispersion medium is not solvent and water, but air. It has the characteristics of no solvent pollution and 100% film formation, and has developed rapidly in recent years.

[0003] Outdoor weather-resistant powder coatings are mainly powder coatings with HAA curing agents and TGIC curing agents. The cost-effective HAA system powder coatings have the advantages of low usage of curing agent HAA (hydroxyalkylamide) and no allergenicity. This type of powder coating has developed rapidly in indoor powder coatings, but HAA curing agent is a hydroxyl compound, and there are defects such as coating film curing pinholes, which leads to certain restrictions on its market application. Although TGIC curing agent has good application performance, it is restricted by the EU and other regions due to problems such as allergenicity. The newly emerged curing agent triglycidyl trimesic acid (Aplus101) in the industry has the effect of replacing TGIC and can be used in the EU, but because it is a curing agent product with a benzene ring structure as the main body, it has deficiencies in high-temperature yellowing performance. The polyester resin used in other curing agent systems has poor curing performance in this system due to insufficient compatibility. At the same time, the hardness of the coating film is required to be high in decorative powder coating. How to achieve the above performance and reduce costs is the direction of continuous research in the industry.

[0004] Furfural residue is generally a biomass waste produced by hydrolyzing corn cobs, corn stalks, rice husks, cottonseed husks, etc. to produce furfural (furan formaldehyde). It contains a large amount of lignin and hemicellulose. Due to its certain salt content and weak acidity, it will pollute the environment if it is directly discarded. It is currently difficult to utilize it on a large scale. Summary of the invention

[0005] In view of the above problems, the present invention develops a high-hardness, high-temperature-resistant yellowing polyester resin that matches the curing system of triglycidyl trimesic acid (Aplus101), which is obtained by polymerization using p-cresol, phenol, furfural residue, formaldehyde, dimethyl adipate, 1,3-dihydroxybutane, ethylmalonic acid, 1,1-cyclohexanediacetic acid, etc. as raw materials.

[0006] One of the purposes of the present invention is to provide a polyester resin for high-hardness, high-temperature-resistant powder coating.

[0007] The second object of the present invention is to provide a method for preparing the polyester resin for high-hardness, high-temperature resistant powder coating.

[0008] The third object of the present invention is to provide an application of the polyester resin for high-hardness, high-temperature resistant powder coating.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] In a first aspect, the present invention provides a polyester resin for high hardness and high temperature resistant powder coating, wherein the polyester resin for high hardness and high temperature resistant powder coating is prepared by polymerizing raw materials including the following mass fractions:

[0011]

[0012] The raw materials for preparing the polyester resin for high-hardness and high-temperature resistant powder coating also include catalyst 1, catalyst 2, antioxidant and activated carbon; catalyst 1 is concentrated hydrochloric acid with a mass fraction of 36-38%, and the amount used is 0.8-1.5% of the mass of p-cresol; catalyst 2 is tetrabutyl titanate, and the amount used is 0.3-0.5% of the mass of dimethyl adipate.

[0013] Preferably, the antioxidant is antioxidant 168, i.e. tris[2.4-di-tert-butylphenyl]phosphite, and the amount used is 5-8% of the mass of phenol;

[0014] Preferably, the amount of activated carbon used is 1-1.5% of the mass of the furfural residue.

[0015] Furfural residue is the waste residue produced when furfural is prepared from corn cobs in industry, with a size of 80-120 mesh and a volatile content of 2-5%, which can be purchased from Hongye Biotechnology Co., Ltd.

[0016] The mass content of the formaldehyde aqueous solution is 37-40%.

[0017] Typical but non-limiting weight parts of p-cresol are, for example, 24, 25, 26, 27, 28 parts;

[0018] Typical but non-limiting weight fractions of phenol are, for example, 7, 8, 9, or 10 parts;

[0019] Typical but non-limiting weight parts of N,N-dimethylformamide are, for example, 8, 9, 10, 11, 12, 13 parts;

[0020] Typical but non-limiting mass fractions of furfural residue are, for example, 25, 26, 27, 28, 29, 30 parts;

[0021] Typical but non-limiting weight fractions of the aqueous formaldehyde solution are, for example, 80, 82, 84, 85, 86, 88, 90, 92, 94, 95 parts;

[0022] Typical but non-limiting weight fractions of dimethyl adipate are, for example, 55, 56, 57, 58, 59, 60, 61, 62 parts;

[0023] Typical but non-limiting weight fractions of 1,3-dihydroxybutane are, for example, 9, 10, 11, 12, 13 parts;

[0024] Typical but non-limiting weight fractions of ethylmalonic acid are, for example, 15, 16, 17, 18, 19 parts;

[0025] Typical but non-limiting mass fractions of 1,1-cyclohexanediacetic acid are, for example, 5, 6, or 7 parts.

[0026] In a second aspect, the present invention provides a method for preparing the above-mentioned polyester resin for high-hardness, high-temperature resistant powder coating, comprising the following steps:

[0027] A, the furfural slag of formula ratio is first added into the washing kettle, add water of 1.2-1.5 times of furfural slag quality, start stirring and heat up to carry out stirring washing, to remove residual water-soluble salt in the furfural slag, the pH value of regulator solution is to 6.8-7.5, then through centrifugation, oven dry obtain the furfural slag after processing, standby;

[0028] B. Add the treated furfural residue into a reactor, add the formulated amount of p-cresol, phenol and N,N-dimethylformamide, stir well, and heat to perform dissolution and extraction reaction;

[0029] C. When there is no significant change in the insoluble matter in the reaction system, add the formulated amount of activated carbon for high-temperature decolorization treatment, cool down, and then perform filter pressing to remove the insoluble matter to obtain a usable filtrate;

[0030] D. Then the filtrate is pumped back into the reactor, the formulated amount of formaldehyde solution and catalyst 1 are added, and the temperature is raised to carry out hydroxymethylation reaction;

[0031] E. Sampling and detecting free p-cresol and phenol by liquid chromatography. When the conversion rates of free p-cresol and phenol are both greater than 98%, gradually raising the temperature, and gradually removing excess formaldehyde aqueous solution, catalyst 1 and N,N-dimethylformamide during the heating process;

[0032] F. Sampling and testing, when the content of volatile matter is less than 1%, adding the formulated amount of dimethyl adipate and catalyst 2, and then heating to carry out transesterification grafting chain extension reaction;

[0033] G. Sampling and detecting the content of free dimethyl adipate in the polymer by gas chromatography. When the conversion rate of dimethyl adipate reaches 97% or more, adding the formulated amount of 1,3-dihydroxybutane and ethylmalonic acid, and then continuing to raise the temperature to carry out chain extension polymerization reaction. When the acid value of the polymer reaches 25-32 mgKOH / g, adding the formulated amount of antioxidant, and starting the vacuum system for vacuum polycondensation;

[0034] H. Take samples to detect the acid value of the polymer. When the acid value of the polymer reaches 12-18 mgKOH / g, release the vacuum system of the reactor, add the formulated amount of 1,1-cyclohexanediacetic acid to carry out carboxyl end-capping reaction, and when the acid value of the polymer reaches 40-48 mgKOH / g, stop the reaction, then discharge the material at high temperature, and use a steel belt with a cooling system to cool the polyester resin, crush and granulate it to obtain the polyester resin.

[0035] In some embodiments, in step A, the temperature is raised to 50-60° C. and the washing is stirred for 0.5-1 h.

[0036] In some embodiments, in step B, the temperature is raised to 140-145° C. and the extraction reaction is carried out for 2-4 hours.

[0037] In some embodiments, in step C, the high temperature decolorization treatment temperature is 140-145°C for 5-8 min; and the temperature is lowered to 40-50°C.

[0038] In some embodiments, in step D, the temperature is raised to 85-90°C.

[0039] In some embodiments, in step E, the temperature is raised to 170-175°C.

[0040] In some embodiments, in step F, the temperature is gradually increased to 190-195° C. at a heating rate of 10-12° C. / h.

[0041] In some embodiments, in step G, the temperature is further increased to 225-230° C. at a heating rate of 6-8° C. / h; the vacuum degree is -0.096 MPa to -0.098 MPa.

[0042] In a specific embodiment, the preparation method of the polyester resin for high hardness and high temperature resistant powder coating comprises the following steps:

[0043] A, the furfural slag of formula ratio is added in the washing kettle earlier, add water of 1.2-1.5 times of furfural slag quality, start stirring and be warming up to 50-60 ℃ and carry out stirring washing 0.5-1h, to remove residual water-soluble salt in the furfural slag, add 10% sodium carbonate solution to regulate the pH value of solution to 6.8-7.5, then through centrifugation, oven dry obtain the furfural slag (volatile matter 2% within) after processing, standby;

[0044] B. Add the treated furfural residue into the reactor, add the formulated amount of p-cresol, phenol and N,N-dimethylformamide, stir well, heat to 140-145°C, and carry out heat preservation, dissolution and extraction reaction for 2-4 hours;

[0045] C. When there is no obvious change in the insoluble matter in the reaction system, it means that all kinds of organic matter such as lignin that can be extracted from the furfural residue have been basically extracted and dissolved. Add the formulated amount of activated carbon at 140-145℃ for high-temperature decolorization for 5-8min, cool to 40-50℃, and then filter press to remove the insoluble matter to obtain a usable filtrate;

[0046] D. The filtrate is then pumped back into the reactor, and the formulated amount of formaldehyde aqueous solution and catalyst 1 are added, and the temperature is raised to 85-90° C., and then the temperature is kept to carry out the hydroxymethylation reaction;

[0047] E. Sampling and detecting free p-cresol and phenol by liquid chromatography. When the conversion rates of free p-cresol and phenol are both greater than 98%, indicating that the hydroxymethylation reaction is basically completed, the temperature is gradually raised to 170-175° C., and the excess formaldehyde aqueous solution, catalyst 1 and N,N-dimethylformamide are gradually removed during the heating process;

[0048] F. Sampling and testing. When the content of volatile matter is less than 1%, add the formulated amount of dimethyl adipate and catalyst 2, then gradually increase the temperature to 190-195° C. at a heating rate of 10-12° C. / h, and keep warm to carry out transesterification grafting chain extension reaction;

[0049] G. Take a sample and use gas chromatography to detect the content of free dimethyl adipate in the polymer. When the conversion rate of dimethyl adipate reaches more than 97%, it means that the transesterification grafting chain extension reaction is basically completed; at this time, add the formula amount of 1,3-dihydroxybutane and ethylmalonic acid, and then continue to heat up to 225-230°C at a heating rate of 6-8°C / h to carry out chain extension polymerization reaction. When the acid value of the polymer reaches 25-32mgKOH / g, add the formula amount of antioxidant 168, start the vacuum system for vacuum polycondensation, and control the vacuum degree at -0.096Mpa to -0.098Mpa;

[0050] H. Take samples to detect the acid value of the polymer. When the acid value of the polymer reaches 12-18 mgKOH / g, release the vacuum system of the reactor, add the formulated amount of 1,1-cyclohexanediacetic acid to carry out carboxyl end-capping reaction, and when the acid value of the polymer reaches 40-48 mgKOH / g, stop the reaction, then discharge the material at high temperature, and use a steel belt with a cooling system to cool the polyester resin, crush and granulate it to obtain the polyester resin.

[0051] The polyester resin for high-hardness and high-temperature-resistant powder coating obtained by the invention is light yellow transparent resin particles, with an acid value of 40-48 mgKOH / g and a softening point of 105-114°C.

[0052] In a third aspect, the present invention provides a use of the above-mentioned polyester resin for high-hardness, high-temperature-resistant powder coating in triglycidyl trimesic acid-cured powder coating.

[0053] Beneficial effects:

[0054] The product of the invention firstly adopts phenol, p-cresol and N,N-dimethylformamide as a mixed high-temperature extraction solvent to extract, dissolve and decolorize functional components such as lignin in furfural residue at high temperature, and then carries out hydroxymethylation reaction with formaldehyde to obtain polyhydroxy compounds, and finally obtains polyester resin through polymerization reaction with other dibasic acids and diols. The invention adopts phenol and p-cresol, which not only greatly improve the extraction efficiency of phenolic lignin in furfural residue, but also react with formaldehyde, wherein phenol is used as a trifunctional compound, p-cresol is used as a difunctional compound, and phenolic lignin is used as a high-functional substance to prepare a polyhydroxymethylated mixed product, which participates in the polymerization reaction of polyester resin together. The final product chain segment contains a relatively high content of hindered phenolic antioxidant groups, and has good high-temperature yellowing resistance. Meanwhile, the high-functionality phenolic lignin compounds in the furfural residue are extracted at high temperature to participate in the polymerization reaction, which not only realizes the comprehensive utilization of furfural residue and reduces the cost, but also improves the functionality of polyester resin. In the process of preparing polyester, an appropriate amount of active end groups are retained to increase the fluidity and end group activity of the coating film during curing. After low-temperature curing (160°C / 15min) with a trimesic acid triglycidyl ester curing agent (Aplus101), the coating film has not only high hardness, but also excellent high-temperature yellowing resistance, and conventional properties such as impact and gloss also meet application requirements.

[0055] The main characteristic hindered phenol structure in the polyester resin segment is shown as follows:

[0056]

[0057] This method not only reduces costs but also realizes high-value-added comprehensive utilization of furfural residue in the field of powder coatings by comprehensively utilizing the effective ingredients in furfural residue. At the same time, it also develops a high-performance polyester resin product that matches the triglycidyl trimesic acid curing agent (Aplus101).

[0058] The present invention has been described in detail above, but the above embodiments are only illustrative in nature and are not intended to limit the present invention. In addition, this article is not limited by any theory described in the above prior art or invention content or the following examples. DETAILED DESCRIPTION

[0059] The present invention is further described below in conjunction with examples. It should be noted that the following examples are provided for illustrative purposes only and do not constitute a limitation on the scope of protection claimed for the present invention.

[0060] Unless otherwise specified, the raw materials, reagents, methods, etc. used in the examples are conventional raw materials, reagents, methods in the art.

[0061] Furfural residue was purchased from Hongye Biotechnology Co., Ltd., size 100 mesh, volatile matter 3%;

[0062] Determination of acid value: according to HG / T 2708-95 "Determination of acid value in polyester polyols" method;

[0063] Determination of softening point: According to GB / T 15332-1994 "Ring and ball method for determination of softening point of hot melt adhesives";

[0064] Determination of volatile matter: Take 5 g of sample, put it into a 120℃ forced air oven and dry it for 2 hours, weigh it, and the lost weight divided by the sample amount is the volatile matter.

[0065] Example 1

[0066] A polyester resin for high-hardness, high-temperature-resistant powder coating, comprising the following raw materials by mass:

[0067]

[0068] Concentrated hydrochloric acid, the amount used is 1% of the mass of p-cresol;

[0069] Tetrabutyl titanate, the amount used is 0.3% of the mass of dimethyl adipate;

[0070] Antioxidant 168, the dosage is 6% of the mass of phenol;

[0071] Activated carbon, the dosage is 1% of the mass of furfural residue.

[0072] The method for preparing the above-mentioned polyester resin for high-hardness, high-temperature resistant powder coating comprises the following steps:

[0073] A, the furfural slag of formula ratio is added in the washing kettle earlier, add the water of 1.5 times of furfural slag quality, start stirring and be warming up to 50 ℃ and carry out stirring washing 1h, to remove residual water-soluble salt in the furfural slag, add 10% sodium carbonate solution regulator solution pH value to 7, then through centrifugation, oven dry obtain the furfural slag (volatile matter 2% within) after processing, standby;

[0074] B. Add the treated furfural residue into the reactor, add the formulated amount of p-cresol, phenol and N,N-dimethylformamide, stir well, heat to 145°C, and carry out heat preservation, dissolution and extraction reaction for 2 hours;

[0075] C. When there is no obvious change in the insoluble matter in the reaction system, it means that all kinds of organic matter such as lignin that can be extracted from the furfural residue have been basically extracted and dissolved, add the formulated amount of activated carbon for high-temperature decolorization at 145°C for 5 minutes, cool to 50°C, and then filter press to remove the insoluble matter to obtain a usable filtrate;

[0076] D. The filtrate is then pumped back into the reactor, and a formulated amount of formaldehyde aqueous solution and concentrated hydrochloric acid are added, and the temperature is raised to 90° C., and then the temperature is kept to carry out a hydroxymethylation reaction;

[0077] E. Take samples and detect free p-cresol and phenol by liquid chromatography. When the conversion rates of free p-cresol and phenol are both greater than 98%, it means that the hydroxymethylation reaction is basically completed. Then gradually increase the temperature to 170° C., and gradually remove excess formaldehyde aqueous solution, concentrated hydrochloric acid and N,N-dimethylformamide during the heating process;

[0078] F. Sampling and testing. When the content of volatile matter is less than 1%, add the formulated amount of dimethyl adipate and tetrabutyl titanate, then gradually increase the temperature to 190° C. at a heating rate of 10° C. / h, and keep the temperature to carry out transesterification grafting chain extension reaction;

[0079] G. Take a sample and use gas chromatography to detect the content of free dimethyl adipate in the polymer. When the conversion rate of dimethyl adipate reaches more than 97%, it means that the transesterification grafting chain extension reaction is basically completed; at this time, add the formula amount of 1,3-dihydroxybutane and ethylmalonic acid, and then continue to heat up to 230°C at a heating rate of 8°C / h to carry out chain extension polymerization reaction. When the acid value of the polymer reaches 25-32mgKOH / g, add the formula amount of antioxidant 168, start the vacuum system for vacuum polycondensation, and control the vacuum degree at -0.098Mpa;

[0080] H. Take samples to detect the acid value of the polymer. When the acid value of the polymer reaches 12-18 mgKOH / g, release the vacuum system of the reactor, add the formulated amount of 1,1-cyclohexanediacetic acid to carry out carboxyl end-capping reaction, and when the acid value of the polymer reaches 40-48 mgKOH / g, stop the reaction, then discharge the material at high temperature, and use a steel belt with a cooling system to cool the polyester resin, crush and granulate it to obtain the polyester resin.

[0081] The acid value of the obtained polyester resin is 44 mgKOH / g, and the softening point is 109°C.

[0082] Example 2

[0083] A polyester resin for high-hardness, high-temperature-resistant powder coating, comprising the following raw materials by mass:

[0084]

[0085] Concentrated hydrochloric acid, the amount used is 1.2% of the mass of p-cresol;

[0086] Tetrabutyl titanate, the amount used is 0.4% of the mass of dimethyl adipate;

[0087] Antioxidant 168, the dosage is 8% of the mass of phenol;

[0088] Activated carbon, the dosage is 1.5% of the mass of furfural residue.

[0089] The preparation method is the same as that of Example 1.

[0090] The acid value of the obtained polyester resin is 41 mgKOH / g, and the softening point is 112°C.

[0091] Example 3

[0092] A polyester resin for high-hardness, high-temperature-resistant powder coating, comprising the following raw materials by mass:

[0093]

[0094]

[0095] Concentrated hydrochloric acid, the amount used is 0.8% of the mass of p-cresol;

[0096] Tetrabutyl titanate, the amount used is 0.5% of the mass of dimethyl adipate;

[0097] Antioxidant 168, the dosage is 6% of the mass of phenol;

[0098] Activated carbon, the dosage is 1.3% of the mass of furfural residue.

[0099] The preparation method is the same as that of Example 1.

[0100] The acid value of the obtained polyester resin is 47 mgKOH / g, and the softening point is 106°C.

[0101] Example 4

[0102] A polyester resin for high-hardness, high-temperature-resistant powder coating, comprising the following raw materials by mass:

[0103]

[0104] Concentrated hydrochloric acid, the amount used is 1.3% of the mass of p-cresol;

[0105] Tetrabutyl titanate, the amount used is 0.3% of the mass of dimethyl adipate;

[0106] Antioxidant 168, the dosage is 5% of the mass of phenol;

[0107] Activated carbon, the dosage is 1.2% of the mass of furfural residue.

[0108] The preparation method is the same as that of Example 1.

[0109] The acid value of the obtained polyester resin is 43 mgKOH / g, and the softening point is 107°C.

[0110] Comparative Example 1

[0111] The polyester resin in Example 1 in CN202210027474.X is used as Comparative Example 1. Due to the difference in the acid value of the polyester resin, in the powder coating formula, the amount of the polyester resin in Comparative Example 1 is 550 parts by mass, the triglycidyl trimesic acid curing agent (Aplus101) is 50 parts by mass, and the amounts of other components remain unchanged (as follows).

[0112] Comparative Example 2

[0113] The polyester resin is the same as that in Comparative Example 1, except that the curing conditions are changed to 185°C / 15min.

[0114] Performance Testing

[0115] Triglycidyl trimesic acid curing agent (Aplus101) curing system powder coating formula (mass parts):

[0116]

[0117] The triglycidyl trimesic acid curing agent (Aplus101) is a product of Shanghai Yaohe Biochemical Technology Co., Ltd.; the leveling agent model is GLP599, and the brightener model is BLC701, both of which are from Ningbo Nanhai Chemical Co., Ltd., and other raw materials are common commercially available raw materials.

[0118] Preparation of coating film: Mix all materials according to the above powder coating formula, melt extrude, tablet and crush them by twin screw extruder, then crush and sieve the tablets (160-180 mesh) to make finished powder coating. Then spray the powder coating on the surface treated tinplate substrate by electrostatic spray gun, with a film thickness of 70-80μm, and cure at 160℃ / 15min to obtain coating film.

[0119] The coating index test is based on GB / T 21776-2008 "Standard Guide for Testing of Powder Coatings and Their Coatings"; the pencil hardness test is based on GB / T 6739-2006 "Determination of Film Hardness of Paints and Varnishes by Pencil Method". The pencil hardness parameters are 3B-2B-B-HB-FH-2H-3H-4H, and the hardness level increases from left to right. The high temperature resistance test is to heat the cured sample in a blast constant temperature oven and observe the changes and degree of changes in the appearance of the sample before and after baking in the oven. The smaller the change, the better the high temperature resistance.

[0120] The polyester resins prepared in the above examples and comparative examples were used to prepare coatings according to the coating formulations provided by the present invention. The coating film properties were tested and the results are shown in Table 1 below.

[0121] Table 1

[0122]

[0123] As can be seen from the above table, the powder coating of the triglycidyl trimesic acid curing agent (Aplus101) prepared by the polyester resin product prepared by the product of the present invention has a smooth and flat appearance, a gloss of more than 93%, and a 50cm positive impact resistance. The hardness of the coating film reaches 3H, and there is no obvious change in the coating film after boiling in boiling water for 2h, and the high temperature resistance of 250℃ is relatively excellent, and the appearance of the coating film at 250℃ / 10h is almost unchanged. The polyester resin of comparative example 1 cannot be fully cured at 160℃ / 15min, resulting in poor appearance, impact and other properties, while comparative example 2 can basically achieve full curing after the curing temperature is increased to 185℃, but due to the lack of compatibility with the Aplus101 curing agent in terms of molecular structure flexibility and other aspects, the recoil still has slight cracking, and the high temperature resistance of 250℃ has very slight yellowing, and the coating hardness is also slightly worse than the product of the present invention.

[0124] The product of the invention not only has excellent compatibility with the triglycidyl trimesic acid curing agent (Aplus101), but also realizes the comprehensive utilization of furfural residues, which not only reduces the raw material cost of the polyester resin, but also reduces environmental pollution, realizes the high added value comprehensive utilization of furfural residues, and has obvious economic and environmental significance.

[0125] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents, without departing from the spirit and essence of the claims of the present invention; and these modifications or replacements are still within the scope defined by the claims of the present invention.

Claims

1. A polyester resin for high hardness and high temperature resistant powder coating, It is characterized in that The polyester resin for high-hardness and high-temperature-resistant powder coating is prepared by polymerizing the following raw materials in parts by mass: The raw materials for preparing the polyester resin for high-hardness and high-temperature resistant powder coating also include catalyst 1, catalyst 2, activated carbon and antioxidant; catalyst 1 is concentrated hydrochloric acid with a mass fraction of 36-38%, and the amount used is 0.8-1.5% of the mass of p-cresol; catalyst 2 is tetrabutyl titanate, and the amount used is 0.3-0.5% of the mass of dimethyl adipate.

2. The polyester resin for high hardness and high temperature resistant powder coating according to claim 1, It is characterized in that The antioxidant is antioxidant 168, and the dosage is 5-8% of the mass of phenol; the dosage of activated carbon is 1-1.5% of the mass of furfural residue.

3. The polyester resin for high hardness and high temperature resistant powder coating according to claim 1, It is characterized in that The size of furfural residue is 80-120 mesh, and the volatile matter is 2-5%.

4. The polyester resin for high hardness and high temperature resistant powder coating according to claim 1, It is characterized in that The mass content of the formaldehyde aqueous solution is 37-40%.

5. A method for preparing the polyester resin for high-hardness, high-temperature-resistant powder coating according to any one of claims 1 to 4, It is characterized in that The following steps are involved: A, the furfural slag of formula ratio is first added into the washing kettle, add water of 1.2-1.5 times of furfural slag quality, start stirring and heat up to carry out stirring washing, to remove residual water-soluble salt in the furfural slag, the pH value of regulator solution is to 6.8-7.5, then through centrifugation, oven dry obtain the furfural slag after processing, standby; B. Add the treated furfural residue into a reactor, add the formulated amount of p-cresol, phenol and N,N-dimethylformamide, stir well, and heat to perform dissolution and extraction reaction; C. When there is no significant change in the insoluble matter in the reaction system, add the formulated amount of activated carbon for high-temperature decolorization treatment, cool down, and then perform filter pressing to remove the insoluble matter to obtain a usable filtrate; D. Then the filtrate is pumped back into the reactor, the formulated amount of formaldehyde solution and catalyst 1 are added, and the temperature is raised to carry out hydroxymethylation reaction; E. Sampling and detecting free p-cresol and phenol by liquid chromatography. When the conversion rates of free p-cresol and phenol are both greater than 98%, gradually raising the temperature, and gradually removing excess formaldehyde aqueous solution, catalyst 1 and N,N-dimethylformamide during the heating process; F. Sampling and testing, when the content of volatile matter is less than 1%, adding the formulated amount of dimethyl adipate and catalyst 2, and then heating to carry out transesterification grafting chain extension reaction; G. Sampling and detecting the content of free dimethyl adipate in the polymer by gas chromatography. When the conversion rate of dimethyl adipate reaches 97% or more, adding the formulated amount of 1,3-dihydroxybutane and ethylmalonic acid, and then continuing to raise the temperature to carry out chain extension polymerization reaction. When the acid value of the polymer reaches 25-32 mgKOH / g, adding the formulated amount of antioxidant, and starting the vacuum system for vacuum polycondensation; H. Take samples to detect the acid value of the polymer. When the acid value of the polymer reaches 12-18 mgKOH / g, release the vacuum system of the reactor, add the formulated amount of 1,1-cyclohexanediacetic acid to carry out carboxyl end-capping reaction, and when the acid value of the polymer reaches 40-48 mgKOH / g, stop the reaction, then discharge the material at high temperature, and use a steel belt with a cooling system to cool the polyester resin, crush and granulate it to obtain the polyester resin.

6. The preparation method according to claim 5, It is characterized in that In step A, the temperature is raised to 50-60°C and stirred for washing for 0.5-1h; In step B, the temperature is raised to 140-145° C. and the extraction reaction is carried out for 2-4 hours.

7. The preparation method according to claim 5, It is characterized in that In step C, the high temperature decolorization treatment temperature is 140-145°C for 5-8 minutes; the temperature is lowered to 40-50°C; In step D, the temperature is raised to 85-90°C.

8. The preparation method according to claim 5, It is characterized in that In step E, the temperature is raised to 170-175°C; In step F, the temperature is gradually increased to 190-195° C. at a heating rate of 10-12° C. / h.

9. The preparation method according to claim 5, It is characterized in that In step G, the temperature is further increased to 225-230° C. at a heating rate of 6-8° C. / h; the vacuum degree is -0.096 MPa to -0.098 MPa.

10. Use of the polyester resin for high hardness and high temperature resistant powder coating according to any one of claims 1 to 4 or the polyester resin for high hardness and high temperature resistant powder coating prepared by the preparation method according to any one of claims 5 to 9 in triglycidyl trimesic acid cured powder coating.